A high-performance lithium iron phosphate positive electrode material and preparation method thereof
By using ultrasonic liquid phase sintering technology in the preparation of lithium iron phosphate cathode materials, the problems of poor sphericity and carbon layer density are solved, and the preparation of high-performance lithium iron phosphate cathode materials is achieved, which has excellent charge and discharge performance and Low production costs.
Patent Information
- Application Number
- CN202411015066.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The traditional preparation method of lithium iron phosphate cathode materials has problems such as poor sphericity of the material, poor density of the carbon layer, and uneven coating, making it difficult to meet higher performance requirements.
Mix the iron source, phosphorus source, lithium source, and carbon source evenly and then perform liquid phase sintering under the action of ultrasonic waves. Ultrasonic waves are used to accelerate the mass transfer rate of the physical phase, improve the activity and density of the material, reduce the formation of irregular crystal forms, and improve the sphericity. , and protect the carbon coating through low-pressure crushing.
The obtained lithium iron phosphate cathode material has good sphericity, dense carbon layer, uniform coating, good charge and discharge performance, easy operation, low equipment requirements, and reduced production costs.
Smart Images

Figure CN118529708B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery materials, and in particular to a high-performance lithium iron phosphate positive electrode material and a preparation method thereof. Background Art
[0002] With the increasing popularity of electric vehicles and unwavering support for clean energy, the electric vehicle market is experiencing rapid expansion. This development has significantly driven the technological advancement and industrialization of lithium-ion batteries. Among these, olivine-structured lithium iron phosphate (LiFePO4), with its significant advantages such as low cost, excellent cycle performance, low toxicity, and safety and stability, has become the preferred cathode material for new energy vehicles and portable electronics.
[0003] However, as technology develops, traditional preparation methods have problems such as poor material sphericity, poor carbon layer density, and uneven coating, which can no longer meet people's demand for further development of battery performance. How to optimize the preparation method at a lower cost to meet higher performance requirements has become a focus of people's attention. Summary of the Invention
[0004] The object of the present invention is to provide a method for preparing a high-performance lithium iron phosphate positive electrode material, which is easy to operate, has low requirements on equipment, and can improve problems such as the sphericity of the material.
[0005] Another object of the present invention is to provide a high-performance lithium iron phosphate positive electrode material, which has good sphericity, a dense carbon layer, a uniform coating, and better charge and discharge performance.
[0006] The embodiment of the present invention is achieved as follows:
[0007] A method for preparing a high-performance lithium iron phosphate positive electrode material, comprising:
[0008] The iron source, phosphorus source, lithium source and carbon source are mixed evenly to form a granular material;
[0009] The granular material is liquid-phase sintered under the action of ultrasound.
[0010] A high-performance lithium iron phosphate positive electrode material is prepared by the above-mentioned preparation method of the high-performance lithium iron phosphate positive electrode material.
[0011] The beneficial effects of the embodiments of the present invention are:
[0012] The embodiment of the present invention provides a high-performance lithium iron phosphate cathode material and a preparation method thereof, which uniformly mixes an iron source, a phosphorus source, a lithium source, and a carbon source to form a granular material, and then performs liquid-phase sintering under the action of ultrasound. A large amount of liquid phase will be generated in the raw materials at a certain sintering temperature, and the proportion of liquid phase in the raw materials is close to 30-50%. At this time, ultrasound is introduced, and sonochemistry will accelerate the mass transfer rate between the phases, increase the probability of generating lattice defects, improve the activity and density of the material, and is less likely to form skeleton crystals. The amount of irregular crystals will be reduced, and the sphericity of the particles will be improved. On this basis, due to the addition of ultrasound, the number of liquid bridge connections between particles is reduced, so only low-pressure crushing is required to complete the crushing, thereby better protecting the carbon coating on the surface of the material. This preparation method is not only easy to operate and has low equipment requirements, but also the lithium iron phosphate cathode material obtained by this preparation method has better charge and discharge performance and high practical value. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without paying any creative work.
[0014] Figure 1 This is the SEM image of the lithium iron phosphate positive electrode material provided in Comparative Example 1 of the present invention;
[0015] Figure 2 This is the SEM image of the lithium iron phosphate positive electrode material provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0016] To make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer are used. Where the manufacturer of the reagents or instruments is not specified, all are conventional products that can be purchased commercially.
[0017] A high-performance lithium iron phosphate positive electrode material and a preparation method thereof according to an embodiment of the present invention are described in detail below.
[0018] A method for preparing a high-performance lithium iron phosphate positive electrode material, comprising:
[0019] S1. The iron source, phosphorus source, lithium source, and carbon source are mixed and uniformly formed into pellets;
[0020] S2. Liquid-phase sintering of the pellets under ultrasonic action.
[0021] The frequency of the ultrasonic wave is 20KHz~1MHz, preferably 50K~70KHz. In practical applications, an ultrasonic wave generator is installed in the heating zone of the kiln to introduce ultrasonic waves into the liquid phase sintering process. In the early stage of sintering heating stage, as the temperature rises, the substances in the phase gradually become molten and gas escapes. The molten liquid phase will flow into the gaps between the unmelted phase particle skeletons and wrap the unmelted phase particles, causing wetting and fusion. With the addition of ultrasound, sonochemistry will accelerate the mass transfer rate between the phases, increase the probability of lattice defects, improve the activity and density of the material, make it less likely to form skeletal crystals, reduce the amount of irregular crystal forms, and improve the sphericity of the particles; in the later stage of sintering heating stage, liquid bridges will exist between the particles, and the sound waves will generate a certain sound pressure acting on the surface of the particles, changing the stress state of the material surface and accelerating the movement of the solid phase particles. High-frequency sound waves will drive the particles to twist, break free from the bonding force brought by the liquid bridge, reduce particle adhesion, and make the material particles more spherical; the normal thermodynamic driving force of the grains comes from the concentration difference and the crystal synthesis rate is slow. The force generated by the sound wave vibration can accelerate the rearrangement of the grains and improve the crystal purity of the material.
[0022] Furthermore, the liquid-phase sintering temperature is 620-680°C, and the sintering time is 10-15 hours. The addition of ultrasound causes localized squeezing and stretching within the liquid phase. The expansion generates a large number of microbubbles, while the squeezing causes the microbubbles to burst. The bursting of the bubbles generates localized ultrahigh temperatures and pressures, which accelerate the transfer of phases. As a result, the external sintering temperature can be lowered to 620-650°C, and the sintering time can be reduced by 5-8 hours compared to current sintering processes, significantly reducing production costs.
[0023] Optionally, the iron source includes at least one of ferric nitrate nonahydrate, ferrous oxalate, ferric oxide, ferric phosphate, and ferrocene; the phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, lithium dihydrogen phosphate, and ferric phosphate; and the lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium nitrate, and lithium dihydrogen phosphate. The molar ratio of phosphorus atoms, iron atoms, and lithium atoms provided by the phosphorus, iron, and lithium sources is 1:0.95-1.1:0.95-1.1. Combining these ratios yields superior product performance.
[0024] Furthermore, the carbon source includes at least one of glucose, sucrose, PEG, and starch; the amount of the carbon source is 1wt% to 4wt% of the total amount of the lithium source, phosphorus source, and iron source. The carbon source can form a carbon coating on the surface of the composite lithium iron phosphate. The carbon coating helps improve the material's conductivity and can limit the growth of the composite lithium iron phosphate during sintering, resulting in small particles and improving charge and discharge performance.
[0025] Alternatively, the iron source, phosphorus source, lithium source, and carbon source are ground using a ball mill to a particle size (D50) of 0.5-3 μm and a D100 of 3-20 μm, and then spray granulated to form granules. During the grinding stage, no chemical reaction occurs between the phases, and all components except the carbon source are insoluble in the solvent system. Thorough grinding of the materials prevents recrystallization of the dissolved phase during spraying, which could lead to continuous growth and adhesion of crystals, resulting in pipe blockage and hindering the preparation process.
[0026] In addition, various doping elements can be added during the grinding stage, including one or more of Cu, Ag, Ni, Mg, Al, Ti, Nb, and V. Doping elements can produce a variety of lattice defects, which is beneficial to the formation of particle gradation.
[0027] Furthermore, 1-3 wt % of a dispersant is added during grinding. Dispersants are high-molecular-weight organic compounds that effectively assist in dispersing the materials during the grinding process. Furthermore, during the sintering stage, the dispersant's thermal decomposition temperature is higher than the melting point of other raw materials. Even at temperatures as high as 450°C, it can still disperse the phases, reducing uneven material supply caused by eddy currents during the sintering process. For example, crystals suspended below the molten metal are more easily supplied with solute, while crystals near the bottom of the sagger are deprived of solute, resulting in different growth morphological characteristics.
[0028] In addition, ultrasound at 20KHz~1MHz can also be used to assist in grinding. In actual operation, an ultrasonic generator can be added to the dispersion tube to provide ultrasonic waves, which is conducive to uniform premixing of the various phases.
[0029] Optionally, the preparation method prepares granules by spray granulation. When the atomizing disk rotates at a speed of 8,000 to 13,000 rpm, the atomized particles become smaller, increasing their surface energy and reducing sintering energy consumption. This can reduce the proportion of core particles in the agglomerated particles of the spray material and increase the proportion of surface particles. These particles adhere less during sintering, increasing the proportion of particles with high sphericity and improving the sphericity of the particles.
[0030] Furthermore, other preferred embodiments of the present invention include a pulverization step after liquid-phase sintering, where the sintered material is transferred to a pulverization bin at a pressure of 0.4-0.6 MPa. Because the sintering step reduces inter-particle bridging, low-pressure pulverization is sufficient, preventing the high-pressure gas from damaging the carbon coating and thus affecting material properties.
[0031] The present invention also provides a high-performance lithium iron phosphate cathode material prepared by the above-mentioned method for preparing a high-performance lithium iron phosphate cathode material. The material has good sphericity, a dense carbon layer, a uniform coating, and excellent charge and discharge performance.
[0032] The features and performance of the present invention are further described in detail below with reference to the embodiments.
[0033] Example 1
[0034] This embodiment provides a high-performance lithium iron phosphate positive electrode material, and the preparation method thereof is as follows:
[0035] S1. Add an iron source (ferrous oxalate), a phosphorus source (ammonium dihydrogen phosphate), and a lithium source (lithium carbonate) to a ball mill at a molar ratio of 1:0.95:0.95 for phosphorus, iron, and lithium. Then, add a carbon source (2 wt% of the total weight of the lithium, phosphorus, and iron sources) and grind under 50 kHz ultrasonic wave to obtain a premix.
[0036] S2. The premix is spray-granulated to obtain granules, wherein the atomizing disk rotates at 13,000 rpm.
[0037] S3. Liquid-phase sintering of the pellets was performed under the action of 50 kHz ultrasonic waves at a temperature of 650°C for 12 h.
[0038] S4. Crush the sintered material with a crushing pressure of 0.6 MPa.
[0039] Example 2
[0040] This embodiment provides a high-performance lithium iron phosphate positive electrode material, and the preparation method thereof is as follows:
[0041] S1. Add an iron source (ferric nitrate), a phosphorus source (lithium dihydrogen phosphate), and a lithium source (lithium nitrate) to a ball mill at a molar ratio of 1:1.1:0.95 between phosphorus and iron. Then, add a carbon source (4 wt% of the total weight of the lithium, phosphorus, and iron sources) and grind under 70 kHz ultrasonic wave to obtain a premix.
[0042] S2. The premix is spray-granulated to obtain granules, wherein the atomizing disk rotates at 8000 rpm.
[0043] S3. Liquid-phase sintering of the pellets was performed under the action of 70 kHz ultrasonic waves at a temperature of 680°C for 10 h.
[0044] S4. Crush the sintered material with a crushing pressure of 0.6 MPa.
[0045] Example 3
[0046] This embodiment provides a high-performance lithium iron phosphate positive electrode material, and the preparation method thereof is as follows:
[0047] S1. Add an iron source (ferrocene), a phosphorus source (ammonium dihydrogen phosphate), and a lithium source (lithium hydroxide) to a ball mill at a molar ratio of 1:1:0.95. Then, add a carbon source (3 wt% of the total weight of the lithium, phosphorus, and iron sources) and grind under 60 kHz ultrasonic wave to obtain a premix.
[0048] S2. The premix is spray-granulated to obtain granules, wherein the atomizing disk rotates at 10,000 rpm.
[0049] S3. Liquid-phase sintering of the pellets was performed under the action of 60 kHz ultrasonic waves at a temperature of 6206°C for 15 h.
[0050] S4. Crush the sintered material with a crushing pressure of 0.4 MPa.
[0051] Examples 4 to 11
[0052] Examples 4-11 each provide a high-performance lithium iron phosphate cathode material, prepared by methods substantially identical to those of Example 1, differing in the ultrasonic frequencies used during the grinding and sintering stages, and in the amount of dispersant added during the grinding stage. The preparation conditions for Example 1 and Examples 4-11 are shown in Table 1.
[0053] Table 1. Preparation conditions of Example 1 and Examples 4 to 11
[0054]
[0055] Comparative Example 1
[0056] This comparative example provides a lithium iron phosphate positive electrode material, and its preparation method is basically the same as that of Example 1, except that ultrasound is not used in the sintering stage.
[0057] Comparative Example 2
[0058] This comparative example provides a lithium iron phosphate positive electrode material, and its preparation method is basically the same as that of Example 1, except that the crushing pressure is 0.8 MPa.
[0059] Test example
[0060] The lithium iron phosphate positive electrode materials provided in Examples 1 to 11 and Comparative Examples 1 to 2 were used to test the physical parameters and charge-discharge performance of the finished products. The test results are shown in Table 2.
[0061] Table 2. Lithium iron phosphate cathode material performance test results
[0062]
[0063] As can be seen from Table 2, the product performance obtained in Examples 1 to 3 of the present invention is better when different lithium sources, phosphorus sources, and iron sources are used, and the charge and discharge performance is excellent, which can reach 158.9 mAh / g or more. The method of Example 10 can reach up to 160.9 mAh / g. On this basis, we further studied the influence of reaction conditions. Compared with Example 1, Examples 4 to 5 changed the ultrasonic frequency in the sintering stage. When the ultrasonic frequency was 60kHz, the first discharge gram capacity of the product was the best. When Examples 5 to 7 all used 70kHz ultrasound in the sintering stage, the ultrasonic frequency in the grinding stage was changed. Also, when it was 60kHz, the first discharge gram capacity of the product was the best. Examples 8 to 11 investigated the effect of the amount of dispersant on product performance and found that the dispersant had a significant effect on the grinding viscosity. As the amount of dispersant added increased, the grinding viscosity decreased accordingly, showing that the compacted density of the product increased, but the first discharge gram capacity did not correspond to continuous enhancement. Studies have shown that after the amount of dispersant exceeded 2‰, the first discharge gram capacity decreased instead. In addition, we set up a product that was not ultrasonically treated during the sintering stage as a comparison (Comparative Example 1). We found that without ultrasonic treatment, the compaction density of the product was significantly reduced, and the initial discharge capacity was also significantly reduced, reaching only 155.4 mAh / g. From the microstructure, we can see that the particles of the product without ultrasonic treatment have poor sphericity, uneven size, and poor dispersion ( Figure 1 ), while the product treated with ultrasound (Example 1) has good sphericity, uniform size, and good dispersion ( Figure 2 In Comparative Example 2, we increased the pressure during the crushing stage. It can be seen that at a crushing pressure of 0.8 MPa, the carbon coating on the product surface was damaged to a certain extent, with a significant reduction in carbon content. Although the compaction density was comparable to that of the embodiment, the initial discharge capacity was significantly reduced, reaching only 154.4 mAh / g, indicating that the damage to the carbon coating significantly affected product performance. The present application, however, achieves this reduction in crushing pressure precisely due to the effect of ultrasound, thereby effectively protecting the carbon coating.
[0064] In summary, the embodiment of the present invention provides a high-performance lithium iron phosphate cathode material and a preparation method thereof, which mixes an iron source, a phosphorus source, a lithium source, and a carbon source evenly to form a granular material, and then performs liquid-phase sintering under the action of ultrasound. A large amount of liquid phase will be generated in the raw materials at a certain sintering temperature, and the proportion of liquid phase in the raw materials is close to 30-50%. At this time, ultrasound is introduced, and sonochemistry will accelerate the mass transfer rate between the phases, increase the probability of lattice defects, improve the activity and density of the material, and is not easy to form skeleton crystals. The amount of irregular crystals will be reduced, and the sphericity of the particles will be improved. On this basis, due to the addition of ultrasound, the bridging between the particles is reduced, so only low-pressure crushing is required to complete the crushing, thereby better protecting the carbon coating on the surface of the material. This preparation method is not only easy to operate and has low equipment requirements, but also the lithium iron phosphate cathode material obtained by this preparation method has better charge and discharge performance and high practical value.
[0065] The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention are intended to be within the scope of protection of the present invention.
Claims
1. A method for preparing a high-performance lithium iron phosphate positive electrode material, characterized in that: include: The iron source, phosphorus source, lithium source and carbon source are mixed evenly to form a granular material; The granular material is subjected to liquid phase sintering under the action of ultrasound; the frequency of the ultrasound is 20KHZ~1MHZ; After the liquid phase sintering is completed, the pellets are crushed under a pressure of 0.4-0.6 MPa.
2. The preparation method according to claim 1, characterized in that: The temperature of the liquid phase sintering is 620-680° C., and the time is 10-15 hours.
3. The preparation method according to claim 1, characterized in that: The iron source includes at least one of ferric nitrate nonahydrate, ferrous oxalate, ferric oxide, ferric phosphate, and ferrocene; the phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, lithium dihydrogen phosphate, and ferric phosphate; the lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium nitrate, and lithium dihydrogen phosphate.
4. The preparation method according to claim 1, characterized in that: The molar ratio of phosphorus atoms, iron atoms and lithium atoms provided by the phosphorus source, the iron source and the lithium source is 1:0.95-1.1:0.95-1.
1.
5. The preparation method according to claim 1, characterized in that: The carbon source includes at least one of glucose, sucrose, PEG, and starch; the amount of the carbon source is 1wt% to 4wt% of the total amount of the lithium source, the phosphorus source, and the iron source.
6. The preparation method according to claim 1, characterized in that: The iron source, the phosphorus source, the lithium source and the carbon source are ground by a ball mill to a particle size D50 of 0.5-3 μm and D100 of 3-20 μm, and then granular materials are prepared by spray granulation.
7. The preparation method according to claim 6, characterized in that: Add 1wt‰~3wt‰ of dispersant during grinding.
8. The preparation method according to claim 7, characterized in that: During grinding, 20KHZ~1MHZ ultrasound is used to assist.
9. A high-performance lithium iron phosphate positive electrode material, characterized in that: The high-performance lithium iron phosphate positive electrode material is prepared by the preparation method of any one of claims 1 to 8.
Citation Information
Patent Citations
Method for recovering and preparing lithium iron phosphate from waste lithium iron phosphate battery
CN102751548A
Preparation method for water system lithium ion battery material
CN104241648A
Pressure-controlling deaggregating synthetic method for lithium iron phosphate positive electrode material
CN105322167A
Preparation method of carbon / carbon nanotube coated lithium iron phosphate composite material by in situ synthesis
CN106876705A
Ultrasonic assistance direct-current sintering furnace and sintering method