A high crack-resistant cement mortar based on gold tailings and preparation method thereof
By growing carbon nanotubes in gold tailings and using rare earth elements, the problem of crack expansion in cement mortar during loading and hydration has been solved, and the crack resistance and mechanical properties of the mortar have been significantly improved, making it suitable for engineering construction.
Patent Information
- Application Number
- CN202411013993.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Cement mortar is prone to crack expansion during the load and hydration process, which affects the quality of the project. It is difficult to effectively solve this problem with existing technology.
Using high crack-resistant cement mortar based on gold tailings, carbon nanotubes are grown in the gold tailings, and Fe2O3 is reduced at high temperatures to generate nanoscale metal Fe, which induces the in-situ growth of carbon nanotubes and combines rare earth elements to improve The dispersion and generation rate of carbon nanotubes improve the crack resistance of mortar.
It significantly improves the mechanical properties and anti-cracking effect of cement mortar, avoids the agglomeration of carbon nanotubes, enhances the filling effect of mortar, and is suitable for a wide range of engineering construction.
Abstract
Description
Technical Field
[0001] The invention relates to the field of plaster mortar, in particular to a high-cracking-resistant cement mortar based on gold tailings and a preparation method thereof. Background Art
[0002] Cement mortar, as a commonly used building material, has many advantages such as abundant raw materials, low price, strong applicability, high strength, easy molding and good durability. However, due to the defects in the structure of cement mortar itself, there are a large number of capillary channels inside. Under the combined action of external loads and its own hydration process, the cracks generated in the transition zone between aggregates and interfaces can easily expand rapidly, leading to cracking and deformation, affecting the quality of the project. Summary of the invention
[0003] Purpose of the invention: In view of the above technical problems, the present invention proposes a high crack-resistant cement mortar based on gold tailings and a preparation method thereof.
[0004] The technical solutions adopted are as follows:
[0005] A high crack-resistant cement mortar based on gold tailings, comprising the following components in parts by weight:
[0006] 430 parts of cement, 1300 parts of sand, 75 parts of gold tailings powder, 40 parts of nano kaolin, 30 parts of redispersible latex powder, 0.5 parts of hydroxyethyl cellulose ether, 2 parts of polycarboxylate water reducer, and 220 parts of water;
[0007] Carbon nanotubes are in-situ grown on the surface of the gold tailings powder;
[0008] The preparation method of the gold tailings powder is as follows:
[0009] Dissolve water-soluble coal tar and water-soluble rare earth salt in water, grind gold tailings and add them, stir thoroughly to obtain a suspension, heat the suspension to evaporate water to obtain a mixture, and finally heat-treat the mixture;
[0010] The mass fraction of Fe2O3 in the gold tailings is ≥8%.
[0011] Furthermore, the water-soluble rare earth salt is lanthanum nitrate and / or cerium nitrate.
[0012] Furthermore, the mass ratio of the water-soluble coal tar pitch to the gold tailings is 1:1-10.
[0013] Furthermore, the heat treatment is performed under an inert gas atmosphere.
[0014] Furthermore, the heat treatment temperature is 700-1200° C., and the time is 1-5 h.
[0015] Furthermore, the redispersible latex powder is any one or more combinations of vinyl acetate / ethylene copolymer rubber powder, ethylene / vinyl chloride / vinyl laurate terpolymer rubber powder, acrylate / styrene copolymer rubber powder, vinyl acetate homopolymer rubber powder, and styrene and butadiene copolymer rubber powder.
[0016] Furthermore, the water reducer is a polycarboxylate water reducer.
[0017] The present invention also provides a method for preparing a high crack-resistant cement mortar based on gold tailings:
[0018] Cement, sand, gold tailings powder and nano-kaolin are mixed in advance to obtain a dry component, the redispersible latex powder is dispersed in water to obtain a wet component, the dry component is added to the wet component, and finally the cellulose ether and the water reducing agent are added.
[0019] Beneficial effects of the present invention:
[0020] The present invention provides a high crack-resistant cement mortar based on gold tailings. Carbon nanotubes have ultra-high mechanical strength and are good doping materials for improving the crack resistance of cement mortar. However, the ultra-strong van der Waals force between carbon nanotubes easily causes agglomeration. The present application utilizes Fe2O3 in gold tailings to be reduced to generate nano-scale metal Fe during high-temperature carbonization of coal tar pitch, and induces carbon nanotubes to grow in situ on the surface of gold tailings, so that they can be evenly dispersed in cement mortar with the gold tailings, which plays a positive role in improving the crack resistance of cement mortar and avoids the agglomeration of carbon nanotubes caused by direct addition. The remaining components in the gold tailings can also be used as carriers of nano-scale metal Fe and the grown carbon nanotubes. The addition of rare earth elements can reduce the temperature required for the generation of carbon nanotubes and increase the generation rate of carbon nanotubes, so that they have a better filling effect in cement mortar. The cement mortar prepared by the present invention has good mechanical properties and crack resistance, and can be widely used in various engineering constructions. DETAILED DESCRIPTION
[0021] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0022] Cement: PO42.5 ordinary Portland cement, Conch;
[0023] Sand: Zone 2 machine-made sand produced by Lingshou County Shuokai Mineral Products Co., Ltd., with a fine mesh modulus of 2.8, MB≤1.0;
[0024] Gold tailings: China Gold Group Hunan Xinrui Mining Co., Ltd., the composition is shown in Table 1 below:
[0025] Table 1: Chemical composition (mass fraction) / %
[0026] ;
[0027] Nano-kaolin: Lingshou County Jingteng Mineral Products Processing Plant;
[0028] Redispersible latex powder: VAE type redispersible latex powder, Jinan Shanhai Chemical Technology Co., Ltd.;
[0029] Hydroxyethyl cellulose ether: Shandong Huaren Chemical Technology Co., Ltd.;
[0030] Polycarboxylate water reducer: Qingshuichi brand, Wuhan Runxingyuan Technology Co., Ltd.;
[0031] Water: Homemade deionized water. Example 1
[0032] A high crack-resistant cement mortar based on gold tailings, comprising the following components in parts by weight:
[0033] 430 parts of cement, 1300 parts of sand, 75 parts of gold tailings powder, 40 parts of nano kaolin, 30 parts of redispersible latex powder, 0.5 parts of hydroxyethyl cellulose ether, 2 parts of polycarboxylate water reducer, and 220 parts of water;
[0034] The preparation method of gold tailings powder is as follows:
[0035] Dissolve 10g of water-soluble coal tar and 0.1g of lanthanum nitrate in 100ml of water, then add 20g of gold tailings after grinding through an 80-mesh sieve, stir thoroughly to obtain a suspension, heat the suspension in an oven to evaporate the water to obtain a mixture, and finally heat the mixture to 800℃ in a tubular furnace under argon protection for 5h.
[0036] The preparation method of the above-mentioned high crack-resistant cement mortar based on gold tailings:
[0037] Cement, sand, gold tailings powder and nano-kaolin are mixed in advance to obtain a dry component, the redispersible latex powder is dispersed in water to obtain a wet component, the dry component is added to the wet component, and finally hydroxyethyl cellulose ether and polycarboxylic acid water reducer are added.
[0038] According to T 0506-2005 "Test Method for Strength of Cement Mortar", the specimens were prepared and tested for strength. The specimens had a size of 40mm×40mm×160mm. After being formed and demolded, the specimens were placed in a standard curing room for curing for 28 days, then taken out and placed in the air for 24 hours. The compressive strength was measured to be 39.6MPa and the flexural strength was 9.8MPa. Example 2
[0039] A high crack-resistant cement mortar based on gold tailings, comprising the following components in parts by weight:
[0040] 430 parts of cement, 1300 parts of sand, 75 parts of gold tailings powder, 40 parts of nano kaolin, 30 parts of redispersible latex powder, 0.5 parts of hydroxyethyl cellulose ether, 2 parts of polycarboxylate water reducer, and 220 parts of water;
[0041] The preparation method of gold tailings powder is as follows:
[0042] Dissolve 10g of water-soluble coal tar and 0.1g of lanthanum nitrate in 100ml of water, then add 10g of gold tailings after grinding through an 80-mesh sieve, stir thoroughly to obtain a suspension, heat the suspension in an oven to evaporate the water to obtain a mixture, and finally heat the mixture to 700℃ in a tubular furnace under argon protection for 5h.
[0043] The preparation method of the above-mentioned high crack-resistant cement mortar based on gold tailings:
[0044] Cement, sand, gold tailings powder and nano-kaolin are mixed in advance to obtain a dry component, the redispersible latex powder is dispersed in water to obtain a wet component, the dry component is added to the wet component, and finally hydroxyethyl cellulose ether and polycarboxylic acid water reducer are added.
[0045] According to T 0506-2005 "Test Method for Strength of Cement Mortar", the specimens were prepared and tested for strength. The specimens had a size of 40mm×40mm×160mm. After being formed and demolded, the specimens were placed in a standard curing room for curing for 28 days. The specimens were then taken out and placed in the air for 24 hours. The compressive strength was measured to be 34.7MPa and the flexural strength was 8.6MPa. Example 3
[0046] A high crack-resistant cement mortar based on gold tailings, comprising the following components in parts by weight:
[0047] 430 parts of cement, 1300 parts of sand, 75 parts of gold tailings powder, 40 parts of nano kaolin, 30 parts of redispersible latex powder, 0.5 parts of hydroxyethyl cellulose ether, 2 parts of polycarboxylate water reducer, and 220 parts of water;
[0048] The preparation method of gold tailings powder is as follows:
[0049] Dissolve 10g of water-soluble coal tar and 0.1g of lanthanum nitrate in 100ml of water, then add 30g of gold tailings after grinding through an 80-mesh sieve, stir thoroughly to obtain a suspension, heat the suspension in an oven to evaporate the water to obtain a mixture, and finally heat the mixture to 1000℃ in a tubular furnace under argon protection for 5h.
[0050] The preparation method of the above-mentioned high crack-resistant cement mortar based on gold tailings:
[0051] Cement, sand, gold tailings powder and nano-kaolin are mixed in advance to obtain a dry component, the redispersible latex powder is dispersed in water to obtain a wet component, the dry component is added to the wet component, and finally hydroxyethyl cellulose ether and polycarboxylic acid water reducer are added.
[0052] According to T 0506-2005 "Test Method for Strength of Cement Mortar", the specimens were prepared and tested for strength. The specimens had a size of 40mm×40mm×160mm. After being formed and demolded, they were placed in a standard curing room for curing for 28 days. The specimens were then taken out and placed in the air for 24 hours. The compressive strength was measured to be 35.5MPa and the flexural strength was 9.1MPa. Example 4
[0053] A high crack-resistant cement mortar based on gold tailings, comprising the following components in parts by weight:
[0054] 430 parts of cement, 1300 parts of sand, 75 parts of gold tailings powder, 40 parts of nano kaolin, 30 parts of redispersible latex powder, 0.5 parts of hydroxyethyl cellulose ether, 2 parts of polycarboxylate water reducer, and 220 parts of water;
[0055] The preparation method of gold tailings powder is the same as that of Example 1. The gold tailings used are from Liaoning Jinfeng Gold Mining Co., Ltd. and the composition is shown in Table 2 below:
[0056] Table 2: Chemical composition (mass fraction) / %
[0057] ;
[0058] The preparation method of the above-mentioned high crack-resistant cement mortar based on gold tailings:
[0059] Cement, sand, gold tailings powder and nano-kaolin are mixed in advance to obtain a dry component, the redispersible latex powder is dispersed in water to obtain a wet component, the dry component is added to the wet component, and finally hydroxyethyl cellulose ether and polycarboxylic acid water reducer are added.
[0060] According to T 0506-2005 "Test Method for Strength of Cement Mortar", the specimens were prepared and tested for strength. The specimens had a size of 40mm×40mm×160mm. After being formed and demolded, they were placed in a standard curing room for curing for 28 days. The specimens were then taken out and placed in the air for 24 hours. The compressive strength was measured to be 20.4MPa and the flexural strength was 5.6MPa. Example 5
[0061] A high crack-resistant cement mortar based on gold tailings, comprising the following components in parts by weight:
[0062] 430 parts of cement, 1300 parts of sand, 75 parts of gold tailings powder, 40 parts of nano kaolin, 30 parts of redispersible latex powder, 0.5 parts of hydroxyethyl cellulose ether, 2 parts of polycarboxylate water reducer, and 220 parts of water;
[0063] The preparation method of gold tailings powder is the same as that of Example 1. The gold tailings used are from Qianxinan Jinlong Gold Mining Co., Ltd., and the composition is shown in Table 3 below:
[0064] Table 3: Chemical composition (mass fraction) / %
[0065] ;
[0066] The preparation method of the above-mentioned high crack-resistant cement mortar based on gold tailings:
[0067] Cement, sand, gold tailings powder and nano-kaolin are mixed in advance to obtain a dry component, the redispersible latex powder is dispersed in water to obtain a wet component, the dry component is added to the wet component, and finally hydroxyethyl cellulose ether and polycarboxylic acid water reducer are added.
[0068] According to T 0506-2005 "Test Method for Strength of Cement Mortar", the specimens were prepared and tested for strength. The specimens had a size of 40mm×40mm×160mm. After being formed and demolded, they were placed in a standard curing room for curing for 28 days. The specimens were then taken out and placed in the air for 24 hours. The compressive strength was measured to be 23.7MPa and the flexural strength was 6.6MPa.
[0069] Comparative Example 1:
[0070] The method is basically the same as Example 1, except that the gold tailings are ground through an 80-mesh sieve and then added instead of the gold tailings powder.
[0071] According to T 0506-2005 "Test Method for Strength of Cement Mortar", the specimens were prepared and tested for strength. The specimens had a size of 40mm×40mm×160mm. After being formed and demolded, they were placed in a standard curing room for curing for 28 days. The specimens were then taken out and placed in the air for 24 hours. The compressive strength was measured to be 13.8MPa and the flexural strength was 4.2MPa.
[0072] Comparative Example 2:
[0073] The method is basically the same as Example 1, except that no gold tailings powder is added.
[0074] According to T 0506-2005 "Test Method for Strength of Cement Mortar", the specimens were prepared and tested for strength. The specimens had a size of 40mm×40mm×160mm. After being formed and demolded, the specimens were placed in a standard curing room for curing for 28 days. The specimens were then taken out and placed in the air for 24 hours. The compressive strength was measured to be 9.1MPa and the flexural strength was 3.3MPa.
[0075] Comparative Example 3:
[0076] The method is basically the same as Example 1, except that lanthanum nitrate is not added during the preparation of the gold tailings powder.
[0077] According to T 0506-2005 "Test Method for Strength of Cement Mortar", the specimens were prepared and tested for strength. The specimens had a size of 40mm×40mm×160mm. After being formed and demolded, they were placed in a standard curing room for curing for 28 days. The specimens were then taken out and placed in the air for 24 hours. The compressive strength was measured to be 19.7MPa and the flexural strength was 5.3MPa.
[0078] Performance testing:
[0079] According to the "Test Method for Cement Mortar Crack Resistance" (JC / T 951-2005), the crack resistance of the high crack-resistant cement mortar prepared in Examples 1-5 of the present invention and Comparative Examples 1-3 was measured. The test adopted Kraai's method for calculating the cracking index, and the crack width was divided into 5 levels, each with a corresponding representative value, see the crack width weight table shown in Table 4. The crack width was measured using a reading microscope, and the crack length Li was measured in sections according to the crack width. With the listed crack width weight Ai, the total crack weight value W was calculated according to the following formula:
[0080] W = ΣAi·Li:
[0081] Table 4:
[0082] ;
[0083] The test results are shown in Table 5 below:
[0084] Table 5:
[0085] ;
[0086] It can be seen from Table 5 above that the cement mortar prepared by the present invention has good crack resistance;
[0087] By comparing the data of Example 1 with those of Examples 4 and 5, it can be seen that the crack resistance of the cement mortar prepared by the present invention is positively correlated with the content of iron oxide in the gold tailings;
[0088] By comparing the data of Example 1 with those of Comparative Examples 1 and 2, it can be seen that directly grinding the gold tailings through an 80-mesh screen and adding them to the cement mortar has a certain improvement in the crack resistance, but the effect is not obvious. It may be that the grinding of the gold tailings has a certain promoting effect on the cement hydration, which increases the density of the mortar and improves the crack resistance.
[0089] By comparing the data of Example 1 with that of Comparative Example 3, it can be seen that the addition of lanthanum nitrate during the preparation of gold tailings powder has a positive effect on the crack resistance of cement mortar. The reason may be that the introduction of rare earth elements can improve the formation conditions of carbon nanotubes, allowing more carbon nanotubes to be formed, thereby significantly improving the crack resistance of cement mortar.
[0090] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high crack-resistant cement mortar based on gold tailings, characterized in that: The composition is calculated by weight: 430 parts of cement, 1300 parts of sand, 75 parts of gold tailings powder, 40 parts of nano kaolin, 30 parts of redispersible latex powder, 0.5 parts of hydroxyethyl cellulose ether, 2 parts of polycarboxylate water reducer, and 220 parts of water; Carbon nanotubes are in-situ grown on the surface of the gold tailings powder; The preparation method of the gold tailings powder is as follows: Dissolve water-soluble coal tar and water-soluble rare earth salt in water, grind gold tailings and add them, stir thoroughly to obtain a suspension, heat the suspension to evaporate water to obtain a mixture, and finally heat-treat the mixture; The mass fraction of Fe2O3 in the gold tailings is ≥8%.
2. The high crack-resistant cement mortar based on gold tailings as claimed in claim 1, characterized in that: The water-soluble rare earth salt is lanthanum nitrate and / or cerium nitrate.
3. The high crack-resistant cement mortar based on gold tailings as claimed in claim 1, characterized in that: The mass ratio of the water-soluble coal tar pitch to the gold tailings is 1:1-10.
4. The high crack-resistant cement mortar based on gold tailings as claimed in claim 1, characterized in that: The heat treatment is performed under an inert gas atmosphere.
5. The high crack-resistant cement mortar based on gold tailings as claimed in claim 1, characterized in that: The heat treatment temperature is 700-1200°C and the time is 1-5h.
6. The high crack-resistant cement mortar based on gold tailings as claimed in claim 1, characterized in that: The redispersible latex powder is any one or more combinations of vinyl acetate / ethylene copolymer rubber powder, ethylene / vinyl chloride / vinyl laurate terpolymer rubber powder, acrylate / styrene copolymer rubber powder, vinyl acetate homopolymer rubber powder, and styrene and butadiene copolymer rubber powder.
7. A method for preparing a high crack-resistant cement mortar based on gold tailings as claimed in any one of claims 1 to 6, characterized in that: Cement, sand, gold tailings powder and nano-kaolin are mixed in advance to obtain a dry component, the redispersible latex powder is dispersed in water to obtain a wet component, the dry component is added to the wet component, and finally hydroxyethyl cellulose ether and polycarboxylic acid water reducer are added.