A BaTiO3-based lead-free piezoelectric ceramic material and preparation method thereof

By optimizing the composition and preparation process of BaTiO3-based lead-free piezoelectric ceramic materials, the problem of insufficient performance of barium titanate-based piezoelectric ceramic materials has been solved, and high-voltage electrical performance, stability and environmentally friendly ceramic material preparation have been achieved.

CN118530022BActive Publication Date: 2024-10-01HUNAN MEICHENG NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410996691.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-01
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The existing barium titanate-based piezoelectric ceramic materials have poor piezoelectricity, poor stability, high Curie temperature and low temperature, which limits their wide application.

Method used

BaTiO3-based lead-free piezoelectric ceramic materials are used, including specific proportions of BaCO3, CaCO3, ZrO2, TiO2, BiGaO3, Gd2O3, MnO2, Bi2O3 and other components, and through specific grinding, calcination and pressing processes, dispersants and sintering aids are added Agents and binders to optimize the microstructure and performance of ceramic materials.

Benefits of technology

It improves the piezoelectric performance, stability and Curie temperature of ceramic materials, reduces the sintering temperature, avoids lead pollution, and the process is simple and environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of piezoelectric ceramic materials, and specifically to a BaTiO3-based lead-free piezoelectric ceramic material and a preparation method thereof. The material, calculated by mass percentage, includes the following main raw material components: 33-35wt% BaCO3, 34.8-38.3wt% CaCO3, 10.5-12.7wt% ZrO2, 7.6-9.5wt% TiO2, 1.5-2wt% BiGaO3, 0.5-2wt% Gd2O3, 0.5-1wt% MnO2, 2.7-4.1wt% Bi2O3, and the BaTiO3-based lead-free piezoelectric ceramic material also includes a dispersant, a sintering aid, and a binder. The BaTiO3-based lead-free piezoelectric ceramic material provided by the present invention has high piezoelectricity, stability and high Curie temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of piezoelectric ceramic materials, and in particular to a BaTiO3-based lead-free piezoelectric ceramic material and a preparation method thereof. Background Art

[0002] Piezoelectric ceramics refer to polycrystalline materials formed by high-temperature sintering of oxide mixtures (zirconium oxide, lead oxide, titanium oxide, etc.) and solid-phase reaction, and are generally referred to as ferroelectric ceramics that have piezoelectric effect through DC high-voltage polarization treatment.

[0003] As an important functional material with strong mechanical, thermal, electrical and light sensitivity, piezoelectric ceramics have been widely used in sensors, ultrasonic transducers, micro-displacement devices and other electronic devices. With the advancement and optimization of processing technology, piezoelectric ceramics have high research and application value in aerospace, electronics, information and other high-tech fields due to their advantages of low cost and high voltage electricity conversion.

[0004] When traditional lead-containing piezoelectric ceramics are sintered at high temperatures, PbO volatilizes, which not only pollutes the environment, but also causes the ceramic stoichiometric ratio to be too high, affecting the material properties. Therefore, lead-free piezoelectric ceramics have gradually become a research focus.

[0005] At present, barium titanate-based lead-free piezoelectric ceramic system is one of the main research directions of lead-free piezoelectric ceramics. The existing barium titanate-based piezoelectric ceramics have a low Curie temperature (Tc = 120°C), poor electrical properties, and it is difficult to effectively improve its various properties through doping, all of which limit its wide application. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems of poor piezoelectricity, poor stability, high Curie temperature and low Curie temperature of barium titanate-based piezoelectric ceramic materials in the prior art.

[0007] The technical solutions adopted are as follows:

[0008] The first aspect of the present invention provides a BaTiO3-based lead-free piezoelectric ceramic material, which comprises the following main raw material components calculated by mass percentage:

[0009] 33~35wt%BaCO3, 34.8~38.3wt%CaCO3, 10.5~12.7wt%ZrO2, 7.6~9.5wt%TiO2, 1.5~2wt%BiGaO3, 0.5~2wt%Gd2O3, 0.5~1wt%MnO2, 2.7~4.1wt%Bi2O3, the BaTiO3-based lead-free piezoelectric ceramic material also includes a dispersant, a sintering aid, and a binder.

[0010] Preferably, the dispersant is MQ-568 dispersant produced by Wuhan Meiqilin New Materials Co., Ltd.

[0011] Further preferably, in the BaTiO3-based lead-free piezoelectric ceramic material, the content of the dispersant is 0.8-1.2 wt % of the total amount of the main raw materials.

[0012] Preferably, the sintering aid is Li2CO3 and CeO2 in a mass ratio of 1:0.5~1.

[0013] More preferably, in the BaTiO3-based lead-free piezoelectric ceramic material, the content of the sintering aid is 0.42-0.71 wt % of the total amount of the main raw materials.

[0014] Preferably, the binder is a polyvinyl alcohol aqueous solution, and in the polyvinyl alcohol aqueous solution, the concentration of the polyvinyl alcohol is 8.5-9wt%.

[0015] Preferably, in the BaTiO3-based lead-free piezoelectric ceramic material, the content of the binder is 3.7-4.3wt% of the total amount of the main raw materials.

[0016] The second aspect of the present invention provides a method for preparing the BaTiO3-based lead-free piezoelectric ceramic material according to the first aspect of the present invention, the method comprising:

[0017] (1) Calculating by mass percentage, weighing the required mass of BaCO3, CaCO3, ZrO2, TiO2, BiGaO3, Gd2O3, MnO2, and Bi2O3, and mixing them uniformly to obtain a mixture, and weighing the required mass of a dispersant; placing the mixture and the dispersant in a ball mill, adding deionized water, and performing a first grinding treatment to obtain an intermediate I;

[0018] (2) Weighing the required mass of sintering aid and dispersant, adding them to the intermediate I, and adding deionized water, performing a second grinding treatment to obtain an intermediate II;

[0019] (3) drying the intermediate II, placing it in a crucible, and transferring it to a muffle furnace, and then performing a first calcination treatment under a reducing atmosphere, and naturally cooling it to room temperature in the furnace to obtain an intermediate III;

[0020] (4) After the intermediate III is naturally cooled to room temperature, it is ground to obtain a powder, and then a polyvinyl alcohol aqueous solution is added, mixed evenly, stirred at 70° C. and 80 rpm for 1 hour, and then granulated to obtain an intermediate IV;

[0021] (5) The intermediate IV is placed in a mold and subjected to a pressing treatment. The intermediate IV is then placed in a crucible and transferred to a muffle furnace. The intermediate is then subjected to a second calcination treatment in a reducing atmosphere. The intermediate is naturally cooled to room temperature in the furnace to obtain a BaTiO3-based lead-free piezoelectric ceramic material.

[0022] Preferably, in step (1), the conditions of the first grinding treatment meet the following requirements: room temperature, a ball milling rate of 350-380 rpm, a time of 12-14 h, and a mass ratio of the ball mill to the mixed material of 5:1.

[0023] Further preferably, in step (1) and step (2), the amount of deionized water used is 0.5-1 kg relative to 1 kg of the mixture.

[0024] Preferably, in step (1) and step (2), the dispersant is used in a ratio of 1:1.

[0025] Preferably, in step (2), the conditions of the second grinding treatment meet the following requirements: room temperature, ball milling rate of 350-380 rpm, and time of 8-10 h.

[0026] More preferably, in step (3), the conditions of the first calcination treatment meet the following requirements: a heating rate of 3-5°C / min, a calcination temperature of 800-850°C, and a calcination time of 2-3h.

[0027] Preferably, in step (5), the second calcination treatment is firstly to raise the temperature to 600-700°C at a rate of 3-5°C / min, calcine at this temperature for 1 hour, then to raise the temperature to 995-1150°C at a rate of 5°C / min, and calcine at this temperature for 3.5-4 hours.

[0028] Further preferably, in step (5), the conditions for the pressing treatment meet the following conditions: the pressure is 15-30 MPa and the time is 30-60 min.

[0029] Preferably, in step (3) and step (5), the reducing atmosphere is independently selected from any one of a hydrogen atmosphere, an ammonia atmosphere, a carbon monoxide atmosphere, and a nitrogen-hydrogen mixed gas atmosphere.

[0030] The present invention has the following beneficial effects:

[0031] (1) The piezoelectric ceramic material of the present invention is based on BaCO3, CaCO3, ZrO2, and TiO2. The preparation method of the ceramic material is simple, the sintering temperature is low, and the obtained ceramic material does not contain lead. During the high-temperature sintering process, no volatile and toxic lead oxide will be produced, and during the waste treatment process, no damage will be caused to humans and the ecological environment.

[0032] (2) Gd2O3 and MnO2 are added to the piezoelectric ceramic material of the present invention. Gd2O3, as a good dopant, can improve the comprehensive performance of the piezoelectric ceramic material. MnO2, as a good dopant, can solve the problem of excessive leakage current of the ceramic sample during the polarization process and improve the piezoelectric performance at the same time. The inventors of the present invention have found that in the BaTiO3-based lead-free piezoelectric ceramic material, when the addition amount of the Gd2O3 is 0.5~2wt% and the addition amount of the MnO2 is 0.5~1wt%, calculated by mass percentage, the grain growth of the ceramic material can be promoted, and the obtained ceramic material is more dense and has better piezoelectric performance. In combination with the other technical features of the present invention, the stability and Curie temperature of the obtained material are further improved.

[0033] (3) BiGaO3 is added to the piezoelectric ceramic material of the present invention as an auxiliary additive, which introduces an appropriate amount of Ga while supplementing the Bi source. The inventors of the present invention have found that in BaTiO3-based lead-free piezoelectric ceramic materials, when the addition amount of BiGaO3 is 1.5-2wt% by mass, it can promote the sintering characteristics and grain growth of the ceramic material, and in combination with the other technical features of the present invention, further improve the stability, piezoelectric performance and Curie temperature of the obtained material.

[0034] (4) Specific amounts of Li2CO3 and CeO2 are added to the piezoelectric ceramic material of the present invention. Both of them serve as sintering aids, which are helpful for grain boundary diffusion and migration, can improve the density of the obtained ceramic material, and can significantly reduce the sintering temperature during the calcination process, thereby saving energy.

[0035] (5) A specific type of dispersant is added to the piezoelectric ceramic material of the present invention. The dispersant is MQ-568 dispersant produced by Wuhan Meiqilin New Materials Co., Ltd. The dispersant has a suitable viscosity at room temperature and a solid content of 28-30wt%. In the process of preparing BaTiO3-based lead-free piezoelectric ceramic materials, after adding the dispersant, the effective radius of the particles increases due to adsorption, thereby generating steric hindrance, which can effectively slow down the sedimentation rate of the ceramic slurry, thereby improving the density of the embryo during the molding process. The inventors of the present invention have found that the stability, piezoelectric properties and Curie temperature of the obtained material can be further improved in combination with the other technical features of the present invention.

[0036] (6) During the calcination process, the grains grow anisotropically and at a fast rate, which easily forms lath-shaped grains, resulting in uneven grains and a non-dense structure. In order to reduce the calcination temperature and control grain growth, Bi2O3 with a melting point of 825°C is selected as a sintering aid. When sintered together with the other components in the piezoelectric ceramic material, the melting point will be further reduced. However, when the melting point of Bi2O3 is too low, it is very easy to volatilize during sintering. Excessive doping will reduce the density of the porcelain body, resulting in too much second phase in the material, a decrease in the effective interface state density, a decrease in grain boundary resistance, and deterioration of the performance of the resulting material. The inventors of the present invention have found that when the addition amount of Bi2O3 is 2.7~4.1wt%, combined with the other technical features of the present invention, a piezoelectric ceramic material with better density can be obtained at a lower calcination temperature. DETAILED DESCRIPTION

[0037] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0038] The BaTiO3-based lead-free piezoelectric ceramic material and the preparation method thereof of the present invention are described below with reference to specific embodiments.

[0039] In the following examples, unless otherwise specified, all raw materials used are commercially available.

[0040] In the following examples, MQ-568 dispersant was purchased from Wuhan Meiqilin New Materials Co., Ltd., with a viscosity of 8-8.2 mPa.s (25°C) and a solid content of 28-30 wt%;

[0041] In the polyvinyl alcohol aqueous solution, the concentration of the polyvinyl alcohol is 8.5 wt %.

[0042] In the following examples, the room temperature is 25°C±2°C.

[0043] Example 1

[0044] This example is used to provide a method for preparing a BaTiO3-based lead-free piezoelectric ceramic material, which comprises the following steps:

[0045] (1) Weigh 330g BaCO3, 383g CaCO3, 110g ZrO2, 95g TiO2, 20g BiGaO3, 15g Gd2O3, 10g MnO2, and 37g Bi2O3, mix them evenly to obtain a mixture, and weigh 6g MQ-568 dispersant;

[0046] The mixture and the MQ-568 dispersant are placed in a ball mill, 1 kg of deionized water is added, and a first grinding treatment is performed to obtain an intermediate I; the conditions of the first grinding treatment meet the following conditions: room temperature, a ball milling rate of 350-380 rpm, a time of 12 h, and a mass ratio of the ball mill to the mixture of 5:1.

[0047] (2) Weigh 4.73 g of Li2CO3, 2.37 g of CeO2, and 6 g of MQ-568 dispersant, add them to the intermediate I, and then add 0.5 kg of deionized water, and perform a second grinding treatment to obtain an intermediate II; the conditions of the second grinding treatment meet the following requirements: room temperature, a ball milling rate of 350-380 rpm, and a time of 8 h.

[0048] (3) Drying the intermediate II, placing it in a crucible, and transferring it to a muffle furnace for a first calcination treatment in a nitrogen-hydrogen mixed gas atmosphere, and naturally cooling it to room temperature to obtain an intermediate III; the conditions of the first calcination treatment are as follows: a heating rate of 5°C / min, a calcination temperature of 800°C, and a calcination time of 2h.

[0049] (4) After the intermediate III is naturally cooled to room temperature, it is ground to obtain a powder, 37 g of polyvinyl alcohol aqueous solution is added, mixed evenly, stirred at 70° C. and 80 rpm for 1 h, and then granulated to obtain intermediate IV.

[0050] (5) The intermediate IV is placed in a mold with a diameter of 10 mm and a thickness of 1 mm, pressed at 20 MPa for 30 min, then placed in a crucible and transferred to a muffle furnace for a second calcination treatment in a nitrogen-hydrogen mixed gas atmosphere, and naturally cooled to room temperature in the furnace to obtain a BaTiO3-based lead-free piezoelectric ceramic material; the second calcination treatment is firstly to increase the temperature to 600°C at a rate of 3°C / min, calcine at this temperature for 1 h, and then to increase the temperature to 995°C at a rate of 5°C / min, and calcine at this temperature for 4 h.

[0051] Example 2

[0052] This example is used to provide a method for preparing a BaTiO3-based lead-free piezoelectric ceramic material, which comprises the following steps:

[0053] (1) Weigh 350g BaCO3, 367g CaCO3, 110g ZrO2, 86.5g TiO2, 17g BiGaO3, 20g Gd2O3, 8.5g MnO2, and 41g Bi2O3, mix them evenly to obtain a mixture, and weigh 4g MQ-568 dispersant;

[0054] The mixture and the MQ-568 dispersant are placed in a ball mill, 1 kg of deionized water is added, and a first grinding treatment is performed to obtain an intermediate I; the conditions of the first grinding treatment meet the following conditions: room temperature, a ball milling rate of 350-380 rpm, a time of 14 h, and a mass ratio of the ball mill to the mixture of 5:1.

[0055] (2) Weigh 2.75 g Li2CO3, 2.75 g CeO2, and 4 g MQ-568 dispersant, add them to the intermediate I, and then add 0.5 kg deionized water to perform a second grinding treatment to obtain an intermediate II; the conditions of the second grinding treatment meet the following requirements: room temperature, a ball milling rate of 350-380 rpm, and a time of 10 h.

[0056] (3) Drying the intermediate II, placing it in a crucible, and transferring it to a muffle furnace for a first calcination treatment in a nitrogen-hydrogen mixed gas atmosphere, and naturally cooling it to room temperature to obtain an intermediate III; the conditions of the first calcination treatment are as follows: a heating rate of 4°C / min, a calcination temperature of 850°C, and a calcination time of 2.5h.

[0057] (4) After the intermediate III is naturally cooled to room temperature, it is ground to obtain a powder, 39 g of polyvinyl alcohol aqueous solution is added, mixed evenly, stirred at 70° C. and 80 rpm for 1 h, and then granulated to obtain intermediate IV.

[0058] (5) The intermediate IV is placed in a mold with a diameter of 10 mm and a thickness of 1 mm, pressed at 30 MPa for 30 min, then placed in a crucible and transferred to a muffle furnace for a second calcination treatment in a nitrogen-hydrogen mixed gas atmosphere, and naturally cooled to room temperature in the furnace to obtain a BaTiO3-based lead-free piezoelectric ceramic material; the second calcination treatment is firstly to increase the temperature to 700°C at a rate of 5°C / min, calcine at this temperature for 1 h, and then to increase the temperature to 1050°C at a rate of 5°C / min, and calcine at this temperature for 3.5 h.

[0059] Example 3

[0060] This example is used to provide a method for preparing a BaTiO3-based lead-free piezoelectric ceramic material, which comprises the following steps:

[0061] (1) Weigh 347g BaCO3, 383g CaCO3, 127g ZrO2, 76g TiO2, 15g BiGaO3, 20g Gd2O3, 5g MnO2, and 27g Bi2O3, mix them evenly to obtain a mixture, and weigh 5g MQ-568 dispersant;

[0062] The mixture and the MQ-568 dispersant are placed in a ball mill, 1 kg of deionized water is added, and a first grinding treatment is performed to obtain an intermediate I; the conditions of the first grinding treatment meet the following conditions: room temperature, a ball milling rate of 350-380 rpm, a time of 12 h, and a mass ratio of the ball mill to the mixture of 5:1.

[0063] (2) Weigh 2.1 g Li2CO3, 2.3 g CeO2, and 5 g MQ-568 dispersant, add them to the intermediate I, and then add 0.5 kg deionized water to perform a second grinding treatment to obtain an intermediate II; the conditions of the second grinding treatment meet the following requirements: room temperature, a ball milling rate of 350-380 rpm, and a time of 8 h.

[0064] (3) Drying the intermediate II, placing it in a crucible, and transferring it to a muffle furnace for a first calcination treatment in a nitrogen-hydrogen mixed gas atmosphere, and naturally cooling it to room temperature to obtain an intermediate III; the conditions of the first calcination treatment are as follows: a heating rate of 3°C / min, a calcination temperature of 850°C, and a calcination time of 3h.

[0065] (4) After the intermediate III is naturally cooled to room temperature, it is ground to obtain a powder, 43 g of polyvinyl alcohol aqueous solution is added, mixed evenly, stirred at 70° C. and 80 rpm for 1 h, and then granulated to obtain intermediate IV.

[0066] (5) The intermediate IV is placed in a mold with a diameter of 10 mm and a thickness of 1 mm, pressed at 15 MPa for 60 min, then placed in a crucible and transferred to a muffle furnace for a second calcination treatment in a nitrogen-hydrogen mixed gas atmosphere, and naturally cooled to room temperature in the furnace to obtain a BaTiO3-based lead-free piezoelectric ceramic material; the second calcination treatment is firstly to increase the temperature to 600°C at a rate of 4°C / min, calcine at this temperature for 1 h, and then to increase the temperature to 1150°C at a rate of 5°C / min, and calcine at this temperature for 4 h.

[0067] Comparative Example 1:

[0068] The method of Example 1 is followed, except that the composition of the mixture is 350g BaCO3, 367g CaCO3, 110g ZrO2, and 86.5g TiO2, and the remaining steps and parameters are the same as those of Example 1.

[0069] Comparative Example 2:

[0070] The method of Example 1 is followed, except that the dispersant is sodium hexametaphosphate, and the remaining steps and parameters are the same as those of Example 1.

[0071] Comparative Example 3:

[0072] The method of Example 1 is followed, except that the sintering aid is Li2CO3 and CeO2 in a mass ratio of 1:2, and the remaining steps and parameters are the same as those of Example 1.

[0073] Comparative Example 4:

[0074] The method of Example 1 was followed, except that Gd2O3 and MnO2 were not added, and the remaining steps and parameters were the same as those of Example 1.

[0075] Comparative Example 5:

[0076] The method of Example 1 is followed, except that BiGaO3 is not added, and the remaining steps and parameters are the same as those of Example 1.

[0077] Test example:

[0078] The piezoelectric ceramic materials prepared in the above embodiments and comparative examples were cleaned, and silver paste was printed on the upper and lower surfaces thereof by screen printing technology. The printed silver products were then placed in a heating furnace, heated to 800° C., kept warm for 50-60 min, and cooled to room temperature to prepare piezoelectric ceramic silver sheets. The piezoelectric ceramic silver sheets were polarized by a direct current electric field, with a polarization temperature of 110-130° C., a polarization time of 30-40 min, and a polarization field strength of 3-6 kV / mm to prepare BaTiO3-based lead-free piezoelectric ceramic sensors.

[0079] Table 1:

[0080] ;

[0081] From the above results, it can be seen that the sensor made of the BaTiO3-based lead-free piezoelectric ceramic material obtained by the present invention has higher sensitivity (higher piezoelectric coefficient), higher Curie temperature and better piezoelectric performance. Further, it is explained that the BaTiO3-based lead-free piezoelectric ceramic material of the present invention has higher piezoelectricity, stability and high Curie temperature.

[0082] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A BaTiO3-based lead-free piezoelectric ceramic material, characterized in that: Calculated by mass percentage, it includes the following main raw material components: 33-35wt%BaCO3, 34.8-38.3wt%CaCO3, 10.5-12.7wt%ZrO2, 7.6-9.5wt%TiO2, 1.5-2wt%BiGaO3, 0.5-2wt%Gd2O3, 0.5-1wt%MnO2, 2.7-4.1wt%Bi2O3, the BaTiO3-based lead-free piezoelectric ceramic material further comprising a dispersant, a sintering aid, and a binder; Wherein, the sintering aid is Li2CO3 and CeO2 in a mass ratio of 1:0.5~1; In the BaTiO3-based lead-free piezoelectric ceramic material, the content of the sintering aid is 0.42-0.71wt% of the total amount of the main raw materials; Wherein, the dispersant is MQ-568 dispersant; In the BaTiO3-based lead-free piezoelectric ceramic material, the content of the dispersant is 0.8-1.2 wt % of the total amount of the main raw materials.

2. The BaTiO3-based lead-free piezoelectric ceramic material according to claim 1, wherein: The binder is a polyvinyl alcohol aqueous solution, and in the polyvinyl alcohol aqueous solution, the concentration of the polyvinyl alcohol is 8.5-9wt%.

3. The BaTiO3-based lead-free piezoelectric ceramic material according to claim 1 or 2, wherein: In the BaTiO3-based lead-free piezoelectric ceramic material, the content of the binder is 3.7-4.3wt% of the total amount of the main raw materials.

4. A method for preparing the BaTiO3-based lead-free piezoelectric ceramic material according to any one of claims 1 to 3, characterized in that: The method includes: (1) Calculating by mass percentage, weighing the required mass of BaCO3, CaCO3, ZrO2, TiO2, BiGaO3, Gd2O3, MnO2, and Bi2O3, and mixing them uniformly to obtain a mixture, and weighing the required mass of a dispersant; placing the mixture and the dispersant in a ball mill, adding deionized water, and performing a first grinding treatment to obtain an intermediate I; (2) Weighing the required mass of sintering aid and dispersant, adding them to the intermediate I, and adding deionized water, performing a second grinding treatment to obtain an intermediate II; (3) drying the intermediate II, placing it in a crucible, and transferring it to a muffle furnace, and then performing a first calcination treatment under a reducing atmosphere, and naturally cooling it to room temperature in the furnace to obtain an intermediate III; (4) After the intermediate III is naturally cooled to room temperature, it is ground to obtain a powder, and then a polyvinyl alcohol aqueous solution is added, mixed evenly, stirred at 70° C. and 80 rpm for 1 hour, and then granulated to obtain an intermediate IV; (5) The intermediate IV is placed in a mold and subjected to a pressing treatment. The intermediate IV is then placed in a crucible and transferred to a muffle furnace. The intermediate is then subjected to a second calcination treatment in a reducing atmosphere. The intermediate is naturally cooled to room temperature in the furnace to obtain a BaTiO3-based lead-free piezoelectric ceramic material.

5. The method according to claim 4, wherein: In step (1), the conditions of the first grinding treatment meet the following requirements: room temperature, a ball milling rate of 350-380 rpm, a time of 12-14 h, and a mass ratio of the ball mill to the mixed material of 5:

1.

6. The method according to claim 4, wherein: In step (1) and step (2), the amount of deionized water used is 0.5-1 kg relative to 1 kg of the mixture.

7. The method according to claim 4, wherein: In step (1) and step (2), the dispersant is used in a ratio of 1:

1.

8. The method according to claim 4, wherein: In step (2), the conditions of the second grinding treatment meet the following requirements: room temperature, ball milling rate of 350-380 rpm, and time of 8-10 h.

9. The method according to claim 4, wherein: In step (3), the conditions of the first calcination treatment are as follows: the heating rate is 3-5°C / min, the calcination temperature is 800-850°C, and the calcination time is 2-3h.

10. The method according to claim 4, wherein: In step (5), the second calcination treatment is to first increase the temperature to 600-700°C at a rate of 3-5°C / min, calcine at this temperature for 1 hour, and then increase the temperature to 995-1150°C at a rate of 5°C / min, and calcine at this temperature for 3.5-4 hours.

11. The method according to claim 4, wherein: In step (5), the conditions for the pressing treatment are as follows: the pressure is 15-30 MPa and the time is 30-60 min.

12. The method according to claim 4, wherein: In step (3) and step (5), the reducing atmosphere is independently selected from any one of a hydrogen atmosphere, an ammonia atmosphere, a carbon monoxide atmosphere, and a nitrogen-hydrogen mixed gas atmosphere.