A hollow multi-level ordered porous electrode and a preparation method and a battery

By designing a combination of hollow carbon powder layer, catalyst particle layer and ionomer layer in the porous electrode, an ordered three-phase interface region is formed, which solves the problem of low utilization rate of traditional porous electrode catalysts and improves the performance and high efficiency of the electrode. Voltage behavior at current density.

CN118538926BActive Publication Date: 2024-10-29CHINA UNIV OF MINING & TECH

Patent Information

Application Number
CN202411012987.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-29
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The traditional porous electrode catalytic layer has less three-phase interface area and low catalyst utilization, which affects the performance of proton exchange fuel cells.

Method used

Design a hollow multi-level ordered porous electrode, including a hollow carbon powder layer, a catalyst particle layer and an ionomer layer. The catalyst nanoparticle array is distributed on the inner and outer surfaces of the hollow carbon powder layer, and the ionomer layer is distributed between the catalyst nanoparticles. space, forming an orderly transmission channel perpendicular to the base layer to improve catalyst utilization.

Benefits of technology

It achieves 100% catalyst utilization, reduces transmission resistance, improves the material transmission performance and voltage performance of porous electrodes, and alleviates the problem of local mass transfer resistance under low precious metal catalyst usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118538926B_ABST
    Figure CN118538926B_ABST
Patent Text Reader

Abstract

The present invention provides a hollow multi-level ordered porous electrode and a preparation method and a battery, and relates to the field of battery technology. The hollow multi-level ordered porous electrode of the present invention includes a hollow carbon powder layer with a hollow structure, and a catalyst particle layer and an ionomer layer are attached to the surface of the hollow carbon powder layer, so that all catalyst nanoparticles participate in the formation of a three-phase interface region, improve the catalyst utilization rate, and reduce the use of porous electrode catalysts. At the same time, due to the ordered active material, electron and proton transmission channels perpendicular to the substrate layer, the transmission resistance of the hollow multi-level ordered porous electrode can be reduced, the material transmission performance of the porous electrode can be improved, and the hollow multi-level ordered porous electrode has a higher voltage at a high current density, which alleviates the local mass transfer resistance problem faced by traditional porous electrodes under low precious metal catalyst usage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a hollow multi-level ordered porous electrode and a preparation method thereof and a battery. Background Art

[0002] Due to its advantages such as high efficiency, low-temperature start-up and rapid response, proton exchange membrane fuel cells are widely used in many fields such as transportation, mobile equipment and residential electricity.

[0003] The core component of a single cell of a proton exchange membrane fuel cell - the porous electrode, is generally composed of components such as a microporous layer, a support layer, and a catalyst layer. Each component is closely related to the performance, cost, and stability of the electrode. For example, the catalyst layer is the site of the oxygen reduction reaction or hydrogen oxidation reaction of the proton exchange membrane fuel cell. The traditional catalyst layer generally adopts coating, spraying or brushing processes to load a uniform mixture containing a catalyst, an ionomer, and a solvent on a gas diffusion layer or a polymer electrolyte membrane to form a porous thin layer. The porous electrode prepared in this way can be divided into a GDE electrode or a CCM electrode.

[0004] However, the catalyst and ionomer materials in the traditional porous electrode formed by the above method are disorderly distributed, which affects the transport process of reactants, products, electrons, protons and other substances inside the traditional porous electrode. The three-phase interface area is small and the catalyst utilization rate is low, which affects the performance of the proton exchange fuel cell. Summary of the invention

[0005] The problem to be solved by the present invention is that the three-phase interface area of ​​the traditional porous electrode catalyst layer is small and the catalyst utilization rate is low.

[0006] In order to solve the above problems, the present invention provides a hollow multi-level ordered porous electrode, comprising a substrate layer and a catalytic unit, wherein the catalytic unit comprises:

[0007] A hollow carbon powder layer, wherein the hollow carbon powder layer is vertically distributed on the surface of the base layer, and the hollow carbon powder layer is a cylindrical structure with a hollow interior and an open end away from the base layer;

[0008] A catalyst particle layer, wherein the catalyst particle layer comprises catalyst nanoparticles distributed in an array, and the catalyst nanoparticles are distributed on the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer;

[0009] The ionomer layer is distributed on the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer and is located between adjacent catalyst nanoparticles.

[0010] Preferably, the wall thickness of the hollow carbon powder layer is 20-200 nm.

[0011] Preferably, the thickness of the catalyst particle layer is 0.5-10 nm.

[0012] Preferably, the diameter of the catalyst nanoparticles is 0.5-10 nm.

[0013] Preferably, the gap between adjacent catalyst nanoparticles is 0.5-10 nm.

[0014] Preferably, the thickness of the ionomer layer is 0.25-5 nm.

[0015] Preferably, the distribution density of the catalytic units on the base layer is 50-200 per square micron.

[0016] The present invention also provides a method for preparing a hollow multi-level ordered porous electrode, which is used to prepare the hollow multi-level ordered porous electrode as described above, comprising:

[0017] preparing an ordered array carrier on the surface of the substrate layer;

[0018] A carbon powder layer is prepared on the surface of the ordered array carrier, and after calcination and acid or alkali washing, a hollow carbon powder layer is obtained on the base layer;

[0019] Attaching catalyst nanoparticles distributed in an array to the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer to obtain a catalyst particle layer;

[0020] An ionomer layer is attached to the regions between the adjacent catalyst nanoparticles on the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer.

[0021] Preferably, the preparing a carbon powder layer on the surface of the ordered array carrier comprises: preparing a carbon powder layer on the ordered array carrier by at least one of spraying, dripping, spin coating and chemical vapor deposition methods, the slurry used in the spraying, dripping, spin coating and chemical vapor deposition methods consists of a carbon powder material and a solvent, wherein the concentration of the slurry is 1wt%-85wt%, the solvent comprises at least one of water, ethanol and propanol, and the carbon powder material comprises at least one of acetylene black, high pyrolytic graphite, graphene and carbon nanotubes.

[0022] The present invention also provides a battery, comprising the hollow multi-level ordered porous electrode as described above.

[0023] The hollow multi-level ordered porous electrode of the present invention comprises a hollow carbon powder layer with a hollow structure, and a catalyst particle layer and an ionomer layer are attached to the surface of the hollow carbon powder layer. The hollow carbon powder layer constitutes an electronic conductive phase, and the ionomer layer constitutes an ion conductive phase. The active material can be transmitted through a channel perpendicular to the substrate layer (i.e., a hollow channel inside the hollow carbon powder layer). Both the ion conductive phase and the electronic conductive phase are perpendicular to the substrate layer, and all catalyst nanoparticles participate in forming a three-phase interface region. The catalyst utilization rate can reach 100%, thereby improving the catalyst utilization rate of the porous electrode and reducing the amount of catalyst used in the porous electrode.

[0024] At the same time, due to the ordered active material, electron and proton transmission channels perpendicular to the substrate layer, the transmission resistance of the hollow multi-level ordered porous electrode can be reduced, the material transmission performance of the porous electrode can be improved, and the hollow multi-level ordered porous electrode can have a higher voltage under high current density. Therefore, the present invention can also alleviate the local mass transfer resistance problem faced by traditional porous electrodes when using low amounts of precious metal catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic diagram of the structure of a hollow multi-level ordered porous electrode according to an embodiment of the present invention;

[0026] Figure 2 A schematic top view of a hollow multi-level ordered porous electrode catalyst unit according to an embodiment of the present invention;

[0027] Figure 3 Schematic diagram of the preparation process of the hollow multi-level ordered porous electrode according to an embodiment of the present invention;

[0028] Figure 4 The proton conductivity comparison between Example 1 and the comparative example;

[0029] Figure 5 The oxygen mass transfer resistance of Example 1 and the comparative example is compared;

[0030] Figure 6 This is a contact angle test diagram of the ordered electrode in Example 1.

[0031] Description of reference numerals:

[0032] 1. Base layer; 2. Ordered array carrier; 3. Carbon powder layer; 4. Hollow carbon powder layer; 5. Catalyst particle layer; 6. Ionomer layer. DETAILED DESCRIPTION

[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0034] In electrochemical reactions, the interface region between solid catalysts, liquid electrolytes, and gas (or liquid) reactants is called the three-phase interface region. In traditional porous electrodes, since the three-phase interface region is composed of active substances, electronic conductive phases, and ion conductive phases, only 20% of the catalyst nanoparticles in the traditional catalyst layer form an effective three-phase interface region, and the catalyst utilization rate is only 10%-20%. This is mainly because the random distribution of catalyst nanoparticles leads to irregular formation of the three-phase interface region, which makes some catalyst nanoparticles unable to fully participate in the reaction, resulting in low catalyst utilization. Therefore, ordered porous electrodes have gradually attracted the attention of researchers. The ordered porous electrode was proposed by Dutch scientist Middleman in 2002. It has low tortuosity, high porosity and specific surface area, and has attracted widespread attention in the field of fuel cells. In recent years, people have used a variety of methods to construct ordered electrodes, including strong electric field method, chemical vapor deposition method, hydrothermal synthesis method, etc. Among them, the more representative work is 3M's nanostructured thin film (NSTF) electrode. NSTF uses whisker-like PR149 as a carrier and columnar Pt-based metal as a catalyst, presenting a hierarchical ordered structure. However, this type of ordered porous electrode is not doped with ionomers, which affects the proton conductivity and water transport performance of this type of battery.

[0035] See also Figure 1 and Figure 2 As shown, a hollow multi-level ordered porous electrode (hereinafter referred to as a porous electrode or an ordered electrode) according to an embodiment of the present invention comprises a substrate layer 1 and a catalytic unit, wherein the catalytic unit comprises:

[0036] A hollow carbon powder layer 4, wherein the hollow carbon powder layer 4 is vertically distributed on the surface of the base layer 1, and the hollow carbon powder layer 4 is a cylindrical structure with a hollow interior and an open end away from the base layer 1;

[0037] A catalyst particle layer 5, wherein the catalyst particle layer 5 comprises catalyst nanoparticles distributed in an array, and the catalyst nanoparticles are distributed on the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer 4;

[0038] The ionomer layer 6 is distributed on the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer 4 and is located between adjacent catalyst nanoparticles.

[0039] The ordered electrode of this embodiment is mainly composed of a hollow carbon powder layer 4, a catalyst particle layer 5 and an ionomer layer 6. The hollow carbon powder layer 4 is vertically distributed on the surface of the base layer 1. The hollow carbon powder layer 4 is a hollow cylindrical structure with one end attached to the base layer 1 and the other end open. It should be noted that the cylindrical shape here is not limited to a cylinder, and can also be a square cylinder or other shapes such as an elliptical cylinder, a polygonal cylinder and some irregularly shaped cylinders.

[0040] Since the hollow carbon powder layer 4 is a hollow structure with open ends, the catalyst nanoparticles can be distributed in an array on the inner and outer surfaces of the hollow carbon powder layer 4 to form a catalyst particle layer 5. Taking the cylindrical hollow carbon powder layer 4 as an example, Figure 2 As shown in Figure 2, it can be seen that the catalyst nanoparticles are evenly distributed along the circumference of the inner and outer walls of the cylinder. Figure 1 As shown, it can be seen that the catalyst nanoparticles are evenly distributed on the inner and outer walls of the cylinder in a direction parallel to the axial direction. Therefore, the catalyst nanoparticles are distributed in an array on the inner and outer walls of the cylinder, that is, the catalyst nanoparticle array is distributed on the inner and outer surfaces of the hollow carbon powder layer 4, and the catalyst particle layer 5 is attached to the inner and outer surfaces of the hollow carbon powder layer 4.

[0041] The ionomer layer 6 is distributed between the catalyst nanoparticles, that is, the ionomer layer 6 is also attached to the inner and outer surfaces of the hollow carbon powder layer 4. However, since the inner and outer surfaces of the hollow carbon powder layer 4 are also attached with array-distributed catalyst nanoparticles, there are certain gaps between the catalyst nanoparticles. Therefore, the ionomer layer 6 cannot completely cover the inner and outer surfaces of the hollow carbon powder layer 4, but is attached to the areas not covered by the catalyst nanoparticles. If the array distribution of the catalyst nanoparticles on the inner and outer surfaces of the hollow carbon powder layer 4 is described as: one circle distributed along the circumferential direction of the inner and outer walls of the cylindrical structure is one layer, then there are multiple layers distributed along the direction parallel to the axial direction of the cylindrical structure, which is composed of Figure 1 It can be seen that the ionomer layer 6 is distributed in the gap between the two layers; one row is distributed along the inner and outer walls of the cylindrical structure parallel to the axial direction, and multiple rows are distributed along the circumferential direction of the cylindrical structure. Figure 2 It can be seen that the ionomer layer 6 is distributed in the gap between the two columns.

[0042] It can be seen from this that in the ordered electrode of this embodiment, the hollow carbon powder layer 4 is perpendicular to the base layer 1. Since the ionomer layer 6 is distributed on the surface of the hollow carbon powder layer 4, the ionomer layer 6 is also a tubular structure parallel to the hollow carbon powder layer 4. It is just that the surface of the ionomer layer 6 is blocked by the array-distributed catalyst nanoparticles to form a tubular structure with a discontinuous surface, that is, the hollow carbon powder layer 4 and the ionomer layer 6 are both perpendicular to the base layer 1.

[0043] The three-phase interface region is generally composed of active substances, electronic conductive phases, and ion conductive phases. The electronic conductive phase in the ordered electrode of this embodiment is composed of a hollow carbon powder layer 4, and the ion conductive phase is composed of an ionomer layer 6. The active substance is transmitted by a channel perpendicular to the substrate layer 1 (i.e., the hollow channel inside the hollow carbon powder layer 4). Therefore, it can be seen that the ion conductive phase and the electronic conductive phase are both perpendicular to the substrate layer 1, and all catalyst nanoparticles participate in the formation of the three-phase interface region. The catalyst utilization rate can reach 100%, which is much higher than the traditional catalyst layer. Only 20% of the catalyst nanoparticles form an effective three-phase interface region. In addition, the ordered active substances, electrons, and protons that are perpendicular to the substrate layer 1 can reduce the transmission resistance of the hollow multi-level ordered porous electrode. Therefore, the ordered electrode of this embodiment can solve the problems of the small three-phase interface area, low catalyst utilization, and high catalyst loading faced by the traditional porous electrode.

[0044] The hollow multi-level ordered porous electrode of this embodiment is designed with a hollow carbon powder layer 4 having a hollow structure, and a catalyst particle layer 5 and an ionomer layer 6 are attached to the surface of the hollow carbon powder layer 4, so that the catalyst can fully participate in the three-phase interface area, thereby improving the utilization rate of the porous electrode catalyst, thereby reducing the amount of porous electrode catalyst used, and greatly improving the single-cell performance of the hollow multi-level ordered porous electrode compared with the traditional porous electrode at a lower catalyst usage. At the same time, due to the ordered active material, electron and proton transmission channels perpendicular to the substrate layer 1, the transmission resistance is reduced, the material transmission performance of the porous electrode is improved, and the hollow multi-level ordered porous electrode has a higher voltage at a high current density, thereby alleviating the local mass transfer resistance problem faced by traditional porous electrodes at low precious metal catalyst usage.

[0045] In some embodiments, the substrate layer 1 is a gas diffusion layer.

[0046] In fuel cells, the gas diffusion layer plays an important role in supporting the catalyst layer, collecting current, conducting gas and discharging the reaction product water. The material of the gas diffusion layer can be selected from carbon fiber paper with a microporous layer, carbon fiber woven cloth, non-woven cloth and carbon black paper.

[0047] In some of the embodiments, the wall thickness of the cylindrical structure of the hollow carbon powder layer 4 is 20-200 nm.

[0048] Setting the wall thickness of the hollow carbon powder layer 4 within the above-mentioned appropriate range can effectively improve the performance and reaction effect of the ordered electrode. For example, the diffusion path length of the gas molecules in the gas diffusion layer can be controlled by appropriate wall thickness, which is beneficial to improving the reaction efficiency; sufficient surface area can be provided for the reaction to occur, and sufficient active sites can be provided, which is beneficial to the catalytic reaction; the structural stability of the hollow carbon powder layer 4 can be maintained to avoid deformation or rupture during the reaction; and the transfer of substances on the electrode surface can be promoted, which is beneficial to improving the efficiency of the electrochemical reaction.

[0049] In some embodiments, the catalyst particle layer 5 has a thickness of 0.5-10 nm.

[0050] The catalyst particle layer 5 with a thickness of 0.5-10 nm can ensure the provision of sufficient active surface for catalytic reaction, control the reaction rate, and achieve regulation of the reaction speed. At the same time, it can also promote the transfer of substances on the electrode surface, which is beneficial to improving the reaction efficiency.

[0051] In some embodiments, the catalyst nanoparticles have a diameter of 0.5-10 nm.

[0052] The diameter of the catalyst nanoparticles is designed to be 0.5-10nm. The smaller diameter catalyst nanoparticles can provide more surface area and specific surface area, increase the active sites for the reaction, and improve the reaction rate.

[0053] In some embodiments, the gap between adjacent catalyst nanoparticles is 0.5-10 nm.

[0054] The above-mentioned appropriate particle gaps can promote the transfer of substances between catalyst nanoparticles and improve the reaction efficiency, while avoiding excessive gaps that cause the catalyst nanoparticles to become loose and affect the catalytic effect.

[0055] In some embodiments, the thickness of the ionomer layer 6 is 0.25-5 nm.

[0056] By adjusting the thickness of the ionomer layer 6 , the transmission rate of electrons or ions on the electrode surface can be adjusted, thereby adjusting the charge transmission.

[0057] In some embodiments, the distribution density of the catalytic units on the base layer 1 is 50-200 per square micron.

[0058] In this embodiment, a catalytic unit is formed by the hollow carbon powder layer 4, the catalyst particle layer 5, and the ionomer layer 6. Figure 1 As shown in the dashed box in the middle, the catalytic units are vertically distributed on the surface of the substrate layer 1. The catalytic units are alternately distributed on the ordered electrodes, and the distribution on the gas diffusion layer substrate is 50-200 catalytic units per 1 square micron. This distribution density can ensure that more active sites are provided, improve catalytic activity and reaction rate, and will not affect the overall mechanical strength and stability of the material.

[0059] The embodiment of the present invention further provides a method for preparing a hollow multi-level ordered porous electrode, which is used to prepare the hollow multi-level ordered porous electrode as described above, comprising:

[0060] Prepare an ordered array carrier 2 on the surface of the base layer 1;

[0061] A carbon powder layer 3 is prepared on the surface of the ordered array carrier 2, and after calcination and acid or alkali washing, a hollow carbon powder layer 4 is obtained on the base layer 1;

[0062] Catalyst nanoparticles distributed in an array are attached to the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer 4 to obtain a catalyst particle layer 5;

[0063] An ionomer layer 6 is attached to the regions between adjacent catalyst nanoparticles on the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer 4 .

[0064] In this embodiment, an ordered array carrier 2 is first prepared on a base layer 1. For example, a zinc oxide (ZnO) nanorod array is prepared on the surface of a gas diffusion layer by a hydrothermal method or an electrostatic spraying method. A carbon powder layer 3 is then prepared on the surface of the nanorods. The nanorods are then removed by calcination and alkali washing (or acid washing) to form a hollow carbon powder layer 4. A catalyst particle layer 5 is then attached to the inner and outer walls of the hollow carbon powder layer 4. For example, a physical vapor deposition method is used to attach catalyst nanoparticles to the inner and outer surfaces of the hollow carbon powder layer 4. Finally, an ionomer layer 6 is attached to the surface of the hollow carbon powder layer 4 to obtain the hollow multi-level ordered porous electrode.

[0065] For example, the preparation of a zinc oxide nanoarray is used as an example to illustrate the preparation of an ordered array carrier 2 on a gas diffusion layer (base layer 1). The preparation steps of the zinc oxide nanoarray are as follows:

[0066] Dissolve zinc acetate and sodium hydroxide in ethanol, mix them evenly with ultrasonic treatment, and then put them into a syringe for use; put the syringe into a pusher, connect the syringe needle to a voltage-stabilized power supply, and place the gas diffusion layer on a receiver with a heating device installed inside the receiver for electrostatic spraying. Under the action of the electric field, a large zinc acetate solution is sprayed along the needle, and zinc acetate decomposes on the surface of the gas diffusion layer to form zinc oxide seeds.

[0067] Zinc nitrate hexahydrate and hexamethylenetetramine are placed in a beaker, deionized water is added, and the treated gas diffusion layer is placed in the beaker after ultrasonic treatment, and the beaker is placed in an oven. After the oven is cooled to room temperature, the gas diffusion layer is taken out to obtain a gas diffusion layer containing a zinc oxide array.

[0068] Exemplarily, the steps of preparing the carbon powder layer 3 on the surface of the ordered array carrier 2 are as follows:

[0069] XC-72 carbon powder and polyacrylic acid are dispersed in a deionized water solution and stirred evenly. Then polytetrafluoroethylene solution is added, stirred evenly and placed in a syringe as a spinning solution. An electrospinning device is connected, and the gas diffusion layer containing the zinc oxide array obtained above is placed on the roller surface for electrospinning. The carbon powder spinning solution is ejected from the needle to form nanofibers, which are distributed along the zinc oxide array, thereby forming a carbon powder layer 3 distributed along the zinc oxide.

[0070] Exemplarily, the steps of attaching the catalyst particle layer 5 to the inner wall and the outer wall of the hollow carbon powder layer 4 by physical vapor deposition are as follows:

[0071] The gas diffusion layer forming the hollow carbon powder layer is placed in a physical vapor deposition instrument, the gas is argon, the target material is platinum metal, and sputtering is performed for 30 seconds at a pressure of 0.15 Pa. Since the sputtering pressure is relatively low, the platinum metal particles formed by the argon ion bombardment of the target material are relatively small and few, so a nanoparticle layer can be formed on the inner and outer walls of the hollow carbon powder layer 4.

[0072] Exemplarily, the steps of attaching the ionomer layer 6 on the surface of the hollow carbon powder layer 4 are as follows:

[0073] The ionomer is dispersed in a solvent, and the dispersed solution is sprayed on the sample after the catalyst particle layer is attached. The ionomer material is preferably a perfluorosulfonic acid resin, and the solvent can be ethanol, water or isopropanol, etc. Since the end of the branch chain of the ionomer material is a sulfonate functional group, there is an electrostatic adsorption effect between the NH2 functional group of the XC-72 carbon powder, so the ionomer tends to be distributed between the catalyst nanoparticles, thereby forming an ionomer layer 6.

[0074] In some embodiments, the method used to construct the ZnO nanorod array on the surface of the gas diffusion layer is a simple hydrothermal method, and the steps are as follows:

[0075] Prepare ZnO colloidal solution, the reagents used are 0.01-0.03M zinc acetate solution and sodium hydroxide solution (the solvent is ethanol). Immerse the gas diffusion layer in the ZnO colloidal solution and treat it at 120°C for 20-40min to obtain a ZnO seed layer. Repeat the above process to control the number of ZnO seeds. Next, immerse the gas diffusion layer with ZnO seeds in a series of mixed aqueous solutions of zinc nitrate hexahydrate and hexamethylenetetramine, with concentrations of 0.005M, 0.01M and 0.02M (zinc nitrate and hexamethylenetetramine). Treat at 80-100°C for 3-6h.

[0076] In some of the embodiments, the steps of preparing an ordered array carrier on the surface of a gas diffusion layer by electrostatic spraying are as follows: zinc acetate and sodium hydroxide are dissolved in ethanol, loaded into a syringe after ultrasonic treatment, the syringe needle is connected to a voltage-stabilized power supply, and the gas diffusion layer is placed on a receiver equipped with a heating device for electrostatic spraying.

[0077] In some of the embodiments, preparing the carbon powder layer 3 on the surface of the ordered array carrier 2 includes: preparing the carbon powder layer 3 on the ordered array carrier 2 by at least one of spraying, dripping, spin coating and chemical vapor deposition methods, the slurry used in the spraying, dripping, spin coating and chemical vapor deposition methods mainly consists of a carbon powder material and a solvent, wherein the concentration of the slurry is 1wt%-85wt%, the solvent includes at least one of water, ethanol and propanol, and the carbon powder material includes at least one of carbon black such as acetylene black, high pyrolytic graphite, graphene and carbon nanotubes.

[0078] In some of the embodiments, the hollow carbon powder layer 4 is prepared by calcination, specifically: a base layer 1 product having a carbon powder layer 3 attached to the surface of an ordered array carrier 2 is placed in an inert gas atmosphere, and fired at 700-1200°C for 2-12 hours to form a carbon powder layer 3, and then the product is placed in an alkaline solution so that the zinc oxide inside reacts with sodium hydroxide to remove the zinc oxide, thereby forming a hollow carbon powder layer 4.

[0079] In the preparation process of the hollow carbon powder layer 4, the present embodiment first forms a carbon powder layer 3 on the surface of the zinc oxide array by means of spraying or the like, and then uses a high temperature treatment method to, on the one hand, further carbonize the carbon powder layer 3 to enhance the degree of cross-linking of the carbon powder material in the carbon powder layer 3, and on the other hand, remove the zinc oxide array by alkali washing to form a hollow carbon powder layer 4.

[0080] In some of the embodiments, a catalyst particle layer 5 attached to the sample surface of the hollow carbon powder layer 4 can be obtained by a physical vapor deposition method, with a magnetron sputtering pressure of 0.01-5.0 Pa, a magnetron sputtering time of 0.15-120 min, and an atomic deposition layer number of 2-200 layers. A catalyst metal particle layer can also be obtained by adsorbing a metal precursor salt and reducing it.

[0081] In some of the embodiments, the ionomer layer 6 is attached to the surface of the sample formed by the catalyst particle layer 5 by one of the methods of spraying, dripping and spin coating. The slurry used in these methods is composed of an ionomer material and a solvent, wherein the slurry concentration is 0.05wt%-60wt%, the ionomer material is preferably perfluorosulfonic acid resin, and the solvent can be ethanol, water or isopropanol, etc.

[0082] In this embodiment, a hollow carbon powder layer 4 with a hollow structure is first prepared. Since it is a hollow carbon powder layer 4, the catalyst particle layer 5 formed by the magnetron sputtering method can be distributed inside and outside the hollow carbon powder layer 4, increasing the catalyst distribution area. With the addition of the ionomer layer 6, this porous electrode forms more three-phase interface areas than other porous electrodes, which can improve the catalyst utilization rate and reduce the amount of catalyst used. At the same time, inside this porous electrode, the transmission channels of gas, liquid, electrons, and protons are all perpendicular to the gas diffusion layer, which can reduce the tortuosity of the porous electrode material transmission channel and increase the performance of the porous electrode.

[0083] The present invention also provides a battery, comprising the hollow multi-level ordered porous electrode as described above. The battery may be a fuel cell, an electrolytic cell, or the like.

[0084] The present invention is further described below by means of specific examples.

[0085] Example 1

[0086] (1) Preparation of zinc oxide nanoarrays:

[0087] Weigh 11.04g zinc acetate and 0.8g sodium hydroxide, dissolve in 2g ethanol, ultrasonicate for 30min, and put into a 5mL syringe for use; put the syringe into the pusher, connect the syringe needle to the voltage regulator, and place the gas diffusion layer on the receiver with a heating device inside the receiver; set the syringe flow rate to 50μL / min, the voltage regulator to 10kV, and the heating temperature to 120℃ for electrostatic spraying. As a result, under the action of the electric field, the zinc acetate solution sprayed along the needle is more uniform, and on the gas diffusion layer (such as Figure 3 In (a), zinc acetate decomposes to form zinc oxide seeds.

[0088] Weigh 1.2g zinc nitrate hexahydrate and 0.56g hexamethylenetetramine in a beaker, add 200mL deionized water, and ultrasonicate for 30min. Then place the gas diffusion layer in the beaker and place the beaker in a 90℃ oven for 4h. After the oven cools to room temperature, take out the gas diffusion layer, which is the gas diffusion layer containing the zinc oxide array. Figure 3 As shown in (b).

[0089] (2) Preparation of carbon powder layer:

[0090] Disperse 75mg XC-72 carbon powder and 20mg polyacrylic acid in 1mL deionized water solution and stir for 2h. XC-72 is a hydrophilic carbon black with excellent properties such as high specific surface area, high conductivity, and high chemical stability. Polyacrylic acid, as a dispersant, helps to evenly disperse carbon black in the aqueous ion solution to avoid carbon powder aggregation and precipitation. Then add 0.5L 5% PTFE (polytetrafluoroethylene) solution, stir for 2h, and place it in a 2mL syringe as a spinning solution. Connect the electrospinning device and place the gas diffusion layer on the roller surface. Set the syringe flow rate to 20μL / min and the stabilized power supply to 12kV for electrospinning. In this process, the carbon powder spinning solution is ejected from the needle to form nanofibers and distributed along the zinc oxide array, thereby forming a carbon powder layer distributed along the zinc oxide, as shown in Figure 3. Figure 3 As shown in (c).

[0091] (3) Preparation of hollow carbon powder layer:

[0092] The gas diffusion layer after step (2) is placed in a furnace at 800°C and reacted for 2 hours in a nitrogen atmosphere. During the reaction, polyacrylic acid simultaneously forms carbon fibers, thereby connecting the XC-72 carbon powder layer 3 to form a carbon powder layer 3. At the same time, the NH2 functional groups on the surface of the XC-72 carbon powder increase, thereby forming a nitrided XC-72. The above sample is then placed in an alkaline solution, and zinc oxide reacts with sodium hydroxide to form a hollow carbon powder layer 4, as shown in FIG. Figure 3 As shown in (d).

[0093] (4) Preparation of catalyst particle layer:

[0094] The gas diffusion layer after step (3) is placed in a physical vapor deposition instrument, using argon gas, a pressure of 0.15 Pa, a sputtering time of 30 seconds, and a target material of platinum metal with a purity of 99.99%. In this way, a nanoparticle layer is formed inside and outside the carbon powder layer 3, such as Figure 3 As shown in (e), due to the relatively low sputtering pressure, the platinum metal particles formed by the argon ion bombardment of the target material are relatively small and few, so that the particles can be intermittently distributed on the surface of the carbon powder layer 3.

[0095] (5) Preparation of ionomer layer:

[0096] The ionomer is dispersed in an ethanol solution to obtain an ionomer solution having a mass fraction of 1%. The ionomer solution is further sprayed on the sample obtained in step (4). The ionomer is distributed in the gaps between the samples mainly because the end of the branched chain of the ionomer material is a sulfonate functional group, which has an electrostatic adsorption effect with the NH2 functional group of the XC-72 carbon powder. Therefore, the ionomer tends to be distributed between the catalyst nanoparticles, that is, on the surface of the carbon powder layer 3, thereby forming an ionomer layer 6, as shown in FIG. Figure 3 As shown in (f).

[0097] Example 2

[0098] The difference from Example 1 is that in step (3), the calcination temperature is 1200° C. and the calcination time is 2 h; in step (4), the sputtering pressure is 4.5 Pa and the sputtering time is 10 s; and in step (5), the mass fraction of the ionomer solution is 30%.

[0099] Example 3

[0100] The difference from Example 1 is that in step (3), the calcination temperature is 700° C. and the calcination time is 10 h; in step (4), the sputtering pressure is 0.05 Pa and the sputtering time is 2 h; and in step (5), the mass fraction of the ionomer solution is 60%.

[0101] Comparative Example

[0102] Weigh 1.5 mg of 60% Pt / C and place it in a 10 mL glass bottle; use a pipette to measure 3 mL of deionized water and 3 mL of anhydrous ethanol, respectively, and transfer them to the above glass bottle; then use a pipette to measure 7.5 µL of 5% Nafion solution and transfer it to the above glass bottle; place the above glass bottle in an ultrasonic cleaner and ultrasonicate for 60 minutes before use. Use a spray gun to spray the above slurry to 3*3 cm 2 After the slurry is sprayed on the surface of the gas diffusion layer, it is dried to obtain a traditional electrode.

[0103] Effect Example

[0104] The electrode performance tests were performed on the electrodes obtained in Example 1 and the comparative example, and the results are as follows: Figure 4 As shown, it can be seen that the proton conductivity of the ordered electrode prepared in Example 1 is 0.171 S / cm, and the proton conductivity of the traditional electrode prepared in the comparative example is 0.110 S / cm. The conductivity of the ordered electrode in Example 1 is increased by 55% compared with that of the traditional electrode.

[0105] The improvement of the oxygen mass transfer performance of the electrode is mainly reflected in the decrease of mass transfer resistance. The mass transfer resistance test was performed on the electrodes prepared in Example 1 and the comparative example, and the results are as follows: Figure 5 As shown, it can be seen that the total oxygen mass transfer resistance of the ordered electrode catalyst layer of Example 1 is 1.03 s·cm -1 , where the mass transfer resistance in the pores of the catalyst layer (the oxygen mass transfer resistance in the gas phase of the catalyst layer in the figure) is 0.61s·cm -1 The mass transfer resistance in the three-phase interface region is 0.42 s·cm -1 Compared with the traditional electrode catalyst layer, the three resistances are reduced by 73%, 78% and 58% respectively.

[0106] In addition, the hydrophobicity of the ordered electrode prepared in Example 1 was tested, and the results were as follows: Figure 6 As shown, the contact angle of the ordered electrode is 136°, indicating that the electrode has a water-repelling function.

[0107] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A hollow multi-level ordered porous electrode, characterized in that: It comprises a base layer (1) and a catalytic unit, wherein the catalytic unit comprises: A hollow carbon powder layer (4), the hollow carbon powder layer (4) being vertically distributed on the surface of the base layer (1), the hollow carbon powder layer (4) being a cylindrical structure with a hollow interior and an open end away from the base layer (1); A catalyst particle layer (5), the catalyst particle layer (5) comprising catalyst nanoparticles distributed in an array, the catalyst nanoparticles being distributed on the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer (4); An ionomer layer (6), the ionomer layer (6) being distributed on the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer (4) and being located between adjacent catalyst nanoparticles.

2. The hollow multi-level ordered porous electrode according to claim 1, characterized in that: The wall thickness of the cylindrical structure of the hollow carbon powder layer (4) is 20-200 nm.

3. The hollow multi-level ordered porous electrode according to claim 1, characterized in that: The thickness of the catalyst particle layer (5) is 0.5-10 nm.

4. The hollow multi-level ordered porous electrode according to claim 1, characterized in that: The diameter of the catalyst nanoparticles is 0.5-10 nm.

5. The hollow multi-level ordered porous electrode according to claim 1, characterized in that: The gap between adjacent catalyst nanoparticles is 0.5-10 nm.

6. The hollow multi-level ordered porous electrode according to claim 1, characterized in that: The thickness of the ionomer layer (6) is 0.25-5 nm.

7. The hollow multi-level ordered porous electrode according to claim 1, characterized in that: The distribution density of the catalytic units on the base layer (1) is 50-200 per square micron.

8. A method for preparing a hollow multi-level ordered porous electrode, characterized in that: For preparing the hollow multi-level ordered porous electrode according to any one of claims 1 to 7, comprising: Preparing an ordered array carrier (2) on the surface of a substrate layer (1); A carbon powder layer (3) is prepared on the surface of the ordered array carrier (2), and after calcination and acid or alkali washing, a hollow carbon powder layer (4) is obtained on the base layer (1); Attaching catalyst nanoparticles distributed in an array to the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer (4) to obtain a catalyst particle layer (5); An ionomer layer (6) is attached to the region between adjacent catalyst nanoparticles on the inner and outer surfaces of the cylindrical structure of the hollow carbon powder layer (4).

9. The method for preparing a hollow multi-level ordered porous electrode according to claim 8, characterized in that: The method of preparing a carbon powder layer (3) on the surface of the ordered array carrier (2) comprises: preparing the carbon powder layer (3) on the ordered array carrier (2) by at least one of spraying, dripping, spin coating and chemical vapor deposition methods, wherein the slurry used in the spraying, dripping, spin coating and chemical vapor deposition methods is composed of a carbon powder material and a solvent, wherein the concentration of the slurry is 1wt%-85wt%, the solvent comprises at least one of water, ethanol and propanol, and the carbon powder material comprises at least one of acetylene black, high pyrolytic graphite, graphene and carbon nanotubes.

10. A battery, characterized in that: It comprises the hollow multi-level ordered porous electrode as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Nanowire structures comprising carbon

    CN101563801A

  • Hollow carbon tube array embedded with nano metal, preparation method and application thereof

    CN110449150A

  • Carbon-based composite material, preparation method therefor, and application thereof

    TW202222427A

Cited By

  • Porous electrode and preparation method thereof

    CN119673945A