A method for preparing porous material-loaded single crystal silicon
By depositing single crystal silicon on the surface of the porous material, the problem of the negative electrode material of lithium-ion battery affecting the circulation performance due to volume expansion is solved, and the electrode material with high capacitance and good cycle stability is achieved, which is suitable for new batteries.
Patent Information
- Application Number
- CN202411017025.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing lithium-ion battery negative electrode material silicon affects the cyclic performance of energy storage devices due to volume expansion problems, and the energy density of commercial graphite is insufficient, making it difficult to meet the demand for high energy density.
Porous materials are prepared by sol-gel method, and single crystal silicon is deposited on its surface. Through high-temperature carbonization and activation, a three-dimensional network framework with micropores, mesopores and macropores are formed to overcome the volume expansion problem of silicon.
It has achieved high capacitance, good cycle stability and low impedance electrode materials, and is suitable for new batteries such as lithium-ion batteries. It has a simple process and low price, and is suitable for industrial production.
Smart Images

Figure CN118545714B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochemistry, and in particular to a method for preparing porous material-loaded single crystal silicon. Background Art
[0002] Lithium-ion batteries have attracted much attention from scientific researchers, and electrode materials are an important factor in determining the capacity, energy density, and cycle performance of energy storage devices. Therefore, it is particularly important to seek an excellent electrode material. The main commercial negative electrode material is graphite (372mAh / g), and its energy density is far from meeting the requirements. Silicon has attracted widespread attention due to its abundant reserves, high theoretical specific capacity (4200mAh / g), and low deintercalation potential. However, its volume expansion problem when used as a negative electrode material seriously affects the cycle performance of energy storage devices. Therefore, it is worth our in-depth study to seek an electrode material that can retain the high capacity characteristics of silicon while effectively curbing its volume effect.
[0003] At present, a lot of research has been carried out on carbon silicon materials, but it is very important to find a simple and efficient preparation method in industrial production. For nanoporous materials prepared by the sol-gel method, the raw materials are abundant, the variety is complete, and the preparation cost is low. On the basis of this simple preparation, silicon is deposited on the surface of the porous network skeleton. The existence of the network skeleton can well curb the volume expansion problem of silicon, which is conducive to the high capacity of silicon itself. In addition, the carbon skeleton has excellent conductivity and low impedance. Its nanoporous structure and large specific surface area also provide more active sites for the deintercalation of lithium ions. Therefore, using this silicon-carbon composite material as an electrode material will show great advantages, simple process, low price, and can be prepared on a large scale. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a porous material loaded with single crystal silicon. The preparation method of the composite material is simple in process, low in price, and can be used for industrial production. At the same time, the composite material has high capacity, large specific surface area, good cyclability, and low impedance, and can be used as an electrode material for new batteries such as lithium-ion batteries.
[0005] The present invention solves the technical problem by adopting the following technical solutions:
[0006] A method for preparing porous material-supported single crystal silicon comprises the following steps:
[0007] S1, sealing and aging the organic synthesized organosol to form a gel, and cooling to room temperature to form a wet gel;
[0008] S2, adjusting the skeleton structure through a drying process to obtain an organic aerogel, and subjecting the organic aerogel to high-temperature carbonization and activation to obtain a porous material having a three-dimensional network of micropores, mesopores and macropores penetrating the skeleton;
[0009] S3, placing the porous material obtained in step S2 as a substrate in a process chamber and performing a vacuum operation;
[0010] S4, after evacuation, introduce a carrier gas of hydrogen and argon mixed gas, and after stabilization, introduce a reaction gas of silane and argon mixed gas, with the silane:argon gas being introduced in a ratio of 1:1-1:10, to deposit on the heated porous material substrate;
[0011] S5. Maintain the deposition temperature for 0.5-5h, stop introducing the reaction gas, retain the hydrogen flow, and naturally cool the entire process chamber to room temperature to obtain a porous material loaded with single crystal silicon.
[0012] Moreover, in step S1, the organosol includes at least one of resorcinol-formaldehyde, melamine-formaldehyde, phenol-formaldehyde, polyurethane, polyurea, polyimide, polyamide, polybenzoxazine, polyacrylonitrile, polypyrrole, cellulose, and chitosan. All proportions of resorcinol-formaldehyde, melamine-formaldehyde, and phenol-formaldehyde prepared in the prior art are suitable for the present invention, and the gels formed by polyurethane, polyurea, polyimide, polyamide, polybenzoxazine, polyacrylonitrile, and polypyrrole in the preparation are suitable for the present invention. Or the organic matter used to prepare carbon aerogel in the prior art is also acceptable. The present invention has no special limitation on the organosol, and only makes a carbon skeleton material. Sols of different proportions or original components of different proportions do not affect the final material combination and structure, because they are all carbonized at high temperature, and therefore do not affect the structure of the final product.
[0013] Moreover, in step S2, before adjusting the skeleton structure in the drying process, a skeleton improver is added to improve the skeleton, and the skeleton improver solution is used to replace pure water to wash the wet gel three times. The amount of the skeleton improver solution used is relatively flexible, and the wet gel can be immersed.
[0014] Moreover, the skeleton improving agent is sodium dodecyl sulfate or sodium hexadecylbenzene sulfonate.
[0015] Moreover, the concentration of the skeleton improving agent is 0.1-0.5wt%.
[0016] Moreover, in the step S2, the hydrogen in the carrier gas hydrogen and argon mixed gas accounts for 95%-99%, and the mixing ratio of silane and argon mixed gas in the reaction gas is 1:5-10.
[0017] Furthermore, in the step S2, the high temperature carbonization temperature is 600°C-1100°C under a nitrogen atmosphere.
[0018] Furthermore, in the step S2, the activation temperature is 600°C-1100°C under a carbon dioxide atmosphere.
[0019] Furthermore, in step S3, the heating temperature of the substrate is 200°C-800°C, and the density of the substrate is 200-500 mg / cm 3 .
[0020] Moreover, the mass fraction of silicon in the prepared porous material loaded with single-crystalline silicon is 5%-25%.
[0021] The advantages and positive effects of the present invention are:
[0022] 1. The mass fraction of silicon in the material prepared by the present invention is 5%-25%. Porous carbon materials prepared under different ratios will cause different distributions of micropores, mesopores and macropores, resulting in different amounts of silicon deposition. When the silicon-carbon material prepared by the present invention is used as a negative electrode material for battery materials, it has excellent structural stability and electrochemical properties. Silicon is deposited on a porous skeleton, and the stable structure and network pore structure of the network skeleton are used to overcome the volume expansion of the silicon material during the charge and discharge process, thereby achieving high capacitance performance.
[0023] 2. The preparation method involved in the present invention has simple process, low price, and can be mass-produced. The silicon-carbon material prepared by the CVD method exhibits low impedance, good cycle stability and high specific capacity when used as an electrode material for lithium-ion batteries.
[0024] 3. The porous material prepared by the sol-gel method of the present invention has a stable skeleton structure and a through three-dimensional network pore structure. Subsequently, during the deposition process, the macropores are used as channels to allow silane gas to enter the micropores and mesopores of the material. The stable skeleton structure and pore structure of the porous material can effectively overcome its volume expansion when used as a negative electrode material for lithium-ion batteries.
[0025] 4. The present invention uses solutions with different surface tensions to improve the skeleton, including replacing the pure water solvent with aqueous solutions of surfactants such as sodium dodecyl sulfate and sodium hexadecylbenzene sulfonate. The use of low surface tension solvents can effectively reduce the surface tension generated by the aqueous solution, which is beneficial to increase the pores and thus increase the surface area between the organic networks.
[0026] 5. After adding the skeleton improver, the surface tension of the aerogel material can be reduced, the pores can be increased, and a negative charge layer can be formed on the surface of the aerogel, which is beneficial to the capture of silane gas, so that the silicon deposition of the present invention can reach up to 25%. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1This is a comparison of the macroscopic morphologies of the organic aerogels that have not been treated with surfactants and those that have been treated with surfactants in Example 1 of the present invention (the shrinkage of the line without surfactant treatment is 5%-15%, and the shrinkage of the line after surfactant treatment is 0.3%-3.7%).
[0028] Figure 2 It is a schematic diagram of pore making and pore expansion of the porous material in Example 1 of the present invention.
[0029] Figure 3 It is an illustration of the microscopic morphology of the porous material composed of micropores, mesopores and macropores in Example 1 of the present invention.
[0030] Figure 4 This is the microscopic morphology of silicon single crystal deposited in the carbon skeleton in Example 1 of the present invention.
[0031] Figure 5 This is a cyclic voltammogram of the porous material loaded with single crystal silicon as the negative electrode material of a lithium ion battery in Example 1 of the present invention.
[0032] Figure 6 This is the impedance diagram of the silicon-carbon negative electrode in Example 1 of the present invention.
[0033] Figure 7 This is a charge and discharge curve diagram of the silicon-carbon negative electrode in Example 1 of the present invention.
[0034] Figure 8 It is a flow chart of the method for preparing single crystal silicon loaded with porous material in the present invention. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0036] A method for preparing porous material-supported single crystal silicon comprises the following steps:
[0037] S1, sealing and aging the organic synthesized organosol to form a gel, and cooling to room temperature to form a wet gel;
[0038] S2, adjusting the skeleton structure through a drying process to obtain an organic aerogel, and subjecting the organic aerogel to high-temperature carbonization and activation to obtain a porous material having a three-dimensional network of micropores, mesopores and macropores penetrating the skeleton;
[0039] S3, placing the porous material obtained in step S2 as a substrate in a process chamber and performing a vacuum operation;
[0040] S4, after evacuation, introduce a carrier gas of hydrogen and argon mixed gas, and after stabilization, introduce a reaction gas of silane and argon mixed gas, with the silane:argon gas being introduced in a ratio of 1:1-1:10, to deposit on the heated porous material substrate;
[0041] S5. Maintain the deposition temperature for 0.5-5h, stop introducing the reaction gas, retain the hydrogen flow, and naturally cool the entire process chamber to room temperature to obtain a porous material loaded with single crystal silicon.
[0042] The preparation idea is:
[0043] The process uses the sol-gel method to synthesize a porous material with a mutually cross-linked three-dimensional network structure, and then places the porous material in an atmosphere of reducing gas - silane for high-temperature deposition to obtain a single crystal silicon-loaded porous material.
[0044] In the first stage, a porous material with a network skeleton is prepared based on the sol-gel method. The organic sol synthesized by organic synthesis is sealed and aged to form a gel, and then cooled to room temperature to form a wet gel. After the drying process, an organic aerogel is obtained. Subsequently, the organic aerogel is carbonized at high temperature in a nitrogen atmosphere and activated in a carbon dioxide atmosphere to obtain a porous material with a network skeleton.
[0045] In the second stage, silicon is deposited on the porous material with a three-dimensional network structure. After vacuuming at a certain temperature, hydrogen and silane gases are introduced into the porous material. Silane diffuses from the pore surface and enters the pores, and a certain amount of silicon is deposited in the pores. Subsequently, it is cooled to room temperature to obtain a porous material loaded with single crystal silicon.
[0046] Example 1
[0047] The present invention adopts the CVD method to deposit silicon on a porous skeleton, and utilizes the pore structure of the three-dimensional network skeleton for deposition. The silicon-carbon material prepared in this way can overcome the volume expansion of the silicon material during the charge and discharge process and achieve high capacitance performance.
[0048] A method for preparing porous material-supported single crystal silicon comprises the following steps:
[0049] S1, 22g of resorcinol and 15ml of formaldehyde sol are added to 100ml of aqueous solution to form RF sol, which is sealed and placed in a vacuum drying oven at high temperature for 3 days for aging to form RF gel, and then cooled to room temperature to form RF wet gel;
[0050] S2, replacing pure water with 100 ml of sodium dodecyl sulfate solution (concentration 0.5 wt%) of RF wet gel, and drying at normal pressure to obtain RF dry gel, carbonizing the RF dry gel at 800 ° C for 3 hours in a nitrogen atmosphere, and activating the RF dry gel at 800 ° C for 2 hours in a carbon dioxide atmosphere to obtain carbon aerogel;
[0051] S3, using porous carbon aerogel ground into powder as the substrate (powder density 405mg / cm 3, the powder is conducive to the entry of gas, ensuring that the single crystal silicon is evenly distributed on the surface of the carbon skeleton, which is conducive to increasing the silicon ratio), and placing it in the process chamber;
[0052] S4, after evacuation, introduce a mixture of hydrogen and argon (as carrier gas, hydrogen accounts for 95%-99%) for 1 hour. After stabilization, introduce a mixture of silane and argon (as reaction gas, the mixing ratio is 1:6). The two mixed gases are introduced into the process chamber and heated to 700 ℃ carbon aerogel substrate for deposition;
[0053] S5. Maintain the deposition temperature for 4 hours with a gas flow rate of 400 ml / min, then stop introducing the reaction gas and retain the hydrogen flow to ensure sufficient reduction. The entire process chamber is naturally cooled to room temperature to obtain the silicon-carbon material.
[0054] The specific surface area of carbon aerogel without single crystal silicon is 503 m 2 / g, the average pore diameter is 3.6nm, and the pore volume is 1.877cc / g.
[0055] The silicon-carbon composite material prepared by this method has a silicon mass fraction of 20% and a specific surface area of 59 m 2 / g, the average pore size is 1.4nm, and the pore volume is 0.047cc / g. When it is used as the negative electrode material of the battery material, it has excellent structural stability and electrochemical performance.
[0056] like Figure 5-Figure 7 As shown, Figure 5 This is a cyclic voltammogram of the porous material loaded with single crystal silicon as the negative electrode material of a lithium ion battery in Example 1 of the present invention. The graph uses an electrochemical workstation to record the relationship between current and potential changes, which is used to analyze the kinetic information and mechanism of the electrochemical reaction.
[0057] Figure 6 This is the impedance diagram of the silicon-carbon cathode in Example 1 of the present invention. The diagram is a Nyquist diagram. The horizontal axis Z´ represents the real part of the impedance, and the vertical axis -Z″ represents the negative number of the imaginary part of the impedance. Each point in the diagram corresponds to a different frequency.
[0058] Figure 7 It is a charge and discharge curve diagram of the silicon-carbon negative electrode in Example 1 of the present invention. The graph uses an electrochemical workstation to record the change of voltage over time during the charge and discharge process, and calculates the charge and discharge capacity by integrating the change of current over time.
[0059] Example 2
[0060] A method for preparing porous material-supported single crystal silicon comprises the following steps:
[0061] S1. 20-30 g of polyimide (PI) sol (solid content 31%) was allowed to stand at room temperature for 24 hours to obtain PI gel;
[0062] S2, the PI wet gel was replaced with 300 ml of sodium hexadecylbenzenesulfonate solution (0.1 wt%) for pure water, followed by CO2 supercritical drying to obtain PI aerogel, the PI aerogel was carbonized at 1050°C for 3 hours in a nitrogen atmosphere, and activated at 600°C for 2 hours in a carbon dioxide atmosphere to obtain carbon aerogel;
[0063] S3, grind the porous carbon aerogel into powder (density 272mg / cm 3 ) as a substrate and placing it in a process chamber;
[0064] S4, after evacuation, introduce a mixture of hydrogen and argon (as carrier gas, the ratio is the same as in Example 1), after stabilization, introduce a mixture of silane and argon (as reaction gas), wherein the mixing ratio is 1:5; the two mixed gases are introduced into the process chamber, and heated to 500 ℃ carbon aerogel substrate for deposition;
[0065] S5. Maintain the deposition temperature for 3 hours with a gas flow rate of 400 ml / min, then stop introducing the reaction gas and retain the hydrogen flow to ensure sufficient reduction. The entire process chamber is naturally cooled to room temperature to obtain the silicon-carbon material.
[0066] The specific surface area of carbon aerogel without single crystal silicon is 578 m 2 / g, the average pore size is 4.37nm, and the pore volume is 4.021cc / g. The mass fraction of silicon in the material prepared by this method is 13%, and the specific surface area is as high as 45m 2 / g, the average pore size is 2.14nm, and the pore volume is 0.117cc / g. When it is used as the negative electrode material of the battery material, it has excellent structural stability and electrochemical performance.
[0067] Example 3
[0068] A method for preparing porous material-supported single crystal silicon comprises the following steps:
[0069] S1, allowing polyurea (PUA) sol (solid content of 37%) to stand to form polyurea wet gel;
[0070] S2, subjecting the polyurea wet gel to CO2 supercritical drying to obtain polyurea aerogel, carbonizing the polyurea aerogel at 900° C. for 2 hours in a nitrogen atmosphere, and activating the polyurea aerogel at 1100° C. for 2 hours in a carbon dioxide atmosphere to obtain carbon aerogel;
[0071] S3, grind the porous carbon aerogel into powder (density 409mg / cm 3 ) as a substrate and placing it in a process chamber;
[0072] S4, after evacuation, introduce a hydrogen and argon mixed gas (as a carrier gas, the ratio is the same as in Example 1), and after stabilization, introduce a silane and argon mixed gas (as a reaction gas), wherein the mixing ratio is 1:5; the two mixed gases are introduced into the process chamber to deposit on the carbon aerogel substrate heated to 600°C;
[0073] S5. Maintain the deposition temperature for 3 hours, stop introducing the reaction gas, and retain the hydrogen flow to ensure sufficient reduction. The entire process chamber is naturally cooled to room temperature to obtain the silicon-carbon material.
[0074] The specific surface area of carbon aerogel without single crystal silicon is 219 m 2 / g, the average pore size is 2.02nm, and the pore volume is 1.545cc / g. The mass fraction of silicon in the material prepared by this method is 5%, and the specific surface area is as high as 98m 2 / g, the average pore size is 1.13nm, and the pore volume is 1.396cc / g. The silicon-carbon negative electrode material that has not been improved by the skeleton modifier is not conducive to the adsorption of silane gas on the surface of the carbon skeleton.
[0075] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.
Claims
1. A method for preparing a porous material-supported single crystal silicon, characterized in that: The steps include: S1, sealing and aging the organic synthesized organosol to form a gel, and cooling to room temperature to form a wet gel; S2, adjusting the skeleton structure through a drying process to obtain an organic aerogel, and subjecting the organic aerogel to high-temperature carbonization and activation to obtain a porous material having a three-dimensional network of micropores, mesopores and macropores penetrating the skeleton; S3, placing the porous material obtained in step S2 as a substrate in a process chamber and performing a vacuum operation; S4, after evacuation, introduce a carrier gas of hydrogen and argon mixed gas, and after stabilization, introduce a reaction gas of silane and argon mixed gas, with the silane:argon gas being introduced in a ratio of 1:1-1:10, to deposit on the heated porous material substrate; S5, maintaining the deposition temperature for 0.5-5h, stopping the introduction of the reaction gas, retaining the hydrogen flow, and naturally cooling the entire process chamber to room temperature to obtain a porous material loaded with single crystal silicon; In step S2, before adjusting the skeleton structure in the drying process, a skeleton improving agent is added to improve the skeleton, and the skeleton improving agent solution is used to replace pure water to wash the wet gel three times; The skeleton improving agent is sodium dodecyl sulfate or sodium hexadecylbenzene sulfonate; The concentration of the skeleton improving agent is 0.1-0.5wt%.
2. The method for preparing a porous material-supported single crystal silicon according to claim 1, characterized in that: In the step S1, the organosol includes at least one of resorcinol-formaldehyde, melamine-formaldehyde, phenol-formaldehyde, polyurethane, polyurea, polyimide, polyamide, polybenzoxazine, polyacrylonitrile, polypyrrole, cellulose, and chitosan.
3. The method for preparing a porous material-supported single crystal silicon according to claim 1, characterized in that: In the step S2, the hydrogen in the carrier gas hydrogen and argon mixed gas accounts for 95%-99%, and the mixing ratio of silane and argon mixed gas in the reaction gas is 1:5-10.
4. The method for preparing a porous material-supported single crystal silicon according to claim 1, characterized in that: In the step S2, the high temperature carbonization temperature is 600°C-1100°C under a nitrogen atmosphere.
5. The method for preparing a porous material-supported single crystal silicon according to claim 1, characterized in that: In the step S2, the activation temperature is 600°C-1100°C under a carbon dioxide atmosphere.
6. The method for preparing a porous material-supported single crystal silicon according to claim 1, characterized in that: In step S3, the heating temperature of the substrate is 200°C-800°C, and the density of the substrate is 200-500 mg / cm 3 .
7. The method for preparing a porous material-supported single crystal silicon according to claim 1, characterized in that: The mass fraction of silicon in the prepared porous material loaded with single-crystal silicon is 5%-25%.
Citation Information
Patent Citations
Preparation method of carbon aerogel
CN111422853A
Carbon material, negative electrode material and preparation method thereof, and battery