A method for preparing nested coated silicon-carbon material
Through the preparation method of nested coated silicon carbon materials, the problems of complex process and high cost of nested coated silicon carbon materials are solved, and the high cycle stability and high specific capacity of the negative electrode materials of lithium-ion batteries are achieved, and the capacity improvement is achieved. , overcomes the problem of silicon volume expansion and is suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202411013007.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-26
Smart Images

Figure CN118545726B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemistry, and in particular to a method for preparing a nested coated silicon-carbon material. Background Art
[0002] Silicon is the negative electrode material for lithium-ion batteries with the highest specific capacity (4200 mA∙h / g) discovered by humans so far, and is one of the most promising negative electrode materials. The problems of silicon negative electrode materials include low cycle life, large volume change, and continuous production of SEI film, while silicon-carbon lithium-ion battery negative electrode materials can effectively improve these problems, so silicon-carbon negative electrode materials are undoubtedly the focus of future negative electrode material development. At present, silicon-based materials are mainly doped with artificial graphite in the form of additives, becoming the first choice for improving the energy density of current power batteries. The materials with reversible capacity of commercial composite materials below 450 mA∙h / g are: carbon-coated silicon oxide and carbon-coated nano-silicon-carbon composite materials. They can basically meet the application requirements in terms of cycle performance and rate characteristics. However, silicon negative electrode materials with higher energy density face many technical challenges in the development process. Therefore, designing and developing silicon negative electrode materials with low cost, high safety and high capacity has become a top priority for improving the energy density of lithium-ion batteries.
[0003] At present, it is very important to seek a simple and efficient preparation method for the process preparation of nested coated silicon-carbon materials in industrial production. For nanoporous carbon materials prepared by the sol-gel method, the drying process usually requires extremely high equipment conditions such as supercritical drying or freeze drying. Such a preparation process is not only complicated and costly, but also not conducive to large-scale preparation. Therefore, the simple preparation process of atmospheric pressure drying provides a good support for the realization of industrial applications. On the basis of this preparation, silicon is introduced into the nanoporous carbon material to generate SiOx in situ. The coating layer of the carbon material effectively curbs the volume expansion problem of silicon, which is conducive to the high capacity of silicon itself. Therefore, the use of nested coated silicon-carbon materials as electrode materials will show great advantages, simple process, low price, and can be prepared on a large scale. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a nested coated silicon-carbon material, which can coat silicon in a carbon layer and nest with a carbon skeleton to form a network structure, and generate CC@SiO2 aerogel through a high-temperature reaction. The material can be used as a negative electrode material for lithium-ion batteries.
[0005] The present invention solves the technical problem by adopting the following technical solutions:
[0006] A method for preparing a nested coated silicon-carbon material comprises the following steps:
[0007] S1, mixing and stirring the silicon source and ammonia water, dissolving them in deionized water and ethanol solvent, forming SiO2 sol by hydrolysis and polycondensation, and then pouring them into the shell organic material and stirring them evenly, centrifuging them, and the shell organic material covers the outer layer of the SiO2 particles with an organic shell, that is, obtaining organic @SiO2 nanoparticles with a core-shell structure;
[0008] S2, preparing an organic network skeleton sol from a skeleton organic raw material by a sol-gel method, mixing the organic network skeleton sol with organic @SiO2 nanoparticles, and stirring them together to form a three-dimensional network skeleton sol loaded with organic @SiO2 nanoparticles;
[0009] S3, sealing the sol obtained in step S2 and placing it in a vacuum drying oven for aging at a temperature of 50° C. for 1-5 days, and cooling it to room temperature to form an organic-organic@SiO2 wet gel;
[0010] S4, preparing organic-organic@SiO2 aerogel by solvent replacement and drying;
[0011] S5, carbonizing the organic-organic@SiO2 aerogel at high temperature to obtain CC@SiO2 aerogel, wherein the high temperature carbonization temperature is 800°C-1000°C;
[0012] S6, and then form CC@SiOx nanomaterials through a high temperature of 1300°C-1600°C.
[0013] Moreover, the silicon source includes at least one of methyl orthosilicate, tetraethyl orthosilicate, and alkoxysilane.
[0014] Moreover, the shell organic material includes at least one of glucose, cellulose, polyurethane, polyimide, and phenolic resin.
[0015] Moreover, the skeleton organic raw material includes at least one of polyurethane, polyimide, phenolic resin, cellulose, chitosan, and starch. All proportions of polyurethane, polyimide, and phenolic resin (preparation of precursors hydroquinone-formaldehyde, melamine-formaldehyde, and phenol-formaldehyde) prepared in the prior art are suitable for the present invention, and the gels formed by polyurethane, polyimide, and phenolic resin in the preparation are suitable for the present invention. Alternatively, organic matter used in the prior art to prepare carbon aerogels is also acceptable. The present invention does not specifically limit organic sols, and only makes a carbon skeleton material. Sols of different proportions or original components of different proportions do not affect the final material combination and structure, because they are all carbonized at high temperatures, and therefore do not affect the structure of the final product.
[0016] Furthermore, an anionic surfactant is added to the SiO2 sol in step S1, and the final concentration of the anionic surfactant is 0.1-0.5 wt%.
[0017] Moreover, the anionic surfactant is sodium dodecylbenzene sulfonate or α-olefin sulfate.
[0018] Moreover, the mass ratio of the silicon source: shell organic material: skeleton organic raw material is 1-10: 0.2-2: 1-30.
[0019] Moreover, in the step S5, the high temperature carbonization step is to first continuously introduce nitrogen at a rate of 20 ml / min-60 ml / min, raise the temperature to 800° C.-1000° C., and maintain it for 2-5 hours.
[0020] Moreover, in the CC@SiOx nanomaterial, 0≤x<2.
[0021] Moreover, silicon accounts for 5%-60% of the total mass fraction of the prepared silicon-carbon material.
[0022] The advantages and positive effects of the present invention are:
[0023] 1. The preparation process of the present invention can be used for large-scale production. At the same time, the prepared material exhibits advantages such as high specific capacity and cycle stability when used as a negative electrode material to compensate for the energy density. The size of silicon in the obtained silicon-carbon material is 10nm-500nm. When used as an electrode material for lithium-ion batteries or supercapacitors, the maximum capacitance can reach 3265 mA∙h / g.
[0024] 2. The preparation method of the present invention is simple in process and can be mass-produced. The prepared nested coated silicon-carbon material overcomes volume expansion when used as a negative electrode material for lithium-ion batteries, and exhibits good cycle stability and high specific capacity.
[0025] 3. In the present invention, organic-organic @SiO2 aerogel is carbonized at high temperature to obtain CC@SiO2 aerogel, which is more conducive to the formation of SiO x , wherein 0≤x<2, and the closer x is to 1, the higher the capacitance of the material; at the same time, a layer of carbon coating is formed on the surface of the silicon particles of the present invention, and after the carbon coating is formed, it grows together with the carbon skeleton, thereby overcoming the silicon expansion, making the cycle performance of the prepared CC@SiOx nanomaterial more stable.
[0026] 4. The anionic surfactant used in the preparation process of SiO2 particles of the present invention can adsorb the hydrophobic tail on the organic part of the silane particles to promote the independent dispersion of SiO2 particles, while the hydrophilic head extends to the water phase. The organic raw materials will combine with the water phase to form a stable dispersion system, which promotes the independent encapsulation of SiO2 particles and SiO2 particles.
[0027] 5. The anionic surfactants used in the present invention include sodium dodecylbenzene sulfonate, α-olefin sulfate (AOS), etc. These surfactants can dissociate in the solvent to generate negative charges. Since like charges repel each other, the electrostatic repulsion between silane particles increases, thereby preventing the particles from agglomerating and achieving a dispersion effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a TEM image of the coated silicon-carbon of the nested coated silicon-carbon material prepared by the present invention.
[0029] Figure 2 It is a SEM picture of the nested coated silicon-carbon material prepared by the present invention.
[0030] Figure 3 It is the TEM line scan element ratio of the nested coated silicon-carbon material prepared by the present invention.
[0031] Figure 4 It is the cycle life of the nested coated silicon-carbon material prepared by the present invention.
[0032] Figure 5 This is the rate curve of the nested coated silicon-carbon material prepared by the present invention as an electrode material. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto. Example 1
[0034] A method for preparing a nested coated silicon-carbon material comprises the following steps:
[0035] S1. Add 10 ml of methyl orthosilicate to 0.7 g of urea, mix and stir in 30 ml of deionized water and 100 ml of ethanol solvent, form SiO2 sol through hydrolysis and polycondensation, add 2.3 ml of a-olefin sulfate (AOS) (0.5 wt%), and then pour into 7.9 ml of glucose (GLU) solution (5 wt%), stir evenly and centrifuge, use glucose (GLU) to coat a 10 nm organic shell on the surface of SiO2 nanoparticles, and then centrifuge at a centrifugal rate of 7000-10000 r / min for 10-20 min to form GLU@SiO2 nanoparticles with a core-shell structure;
[0036] S2, then phenol and formaldehyde were used to prepare an organic network skeleton sol (39 ml, phenol and formaldehyde ratio 1:2) by sol-gel method, GLU@SiO2 nanoparticles were added to the sol, and the sol and GLU@SiO2 nanoparticles grew together to form a three-dimensional network skeleton;
[0037] S3, the obtained sol is sealed and placed in a vacuum drying oven for aging at 60°C for 3 days to form RF-GLU@SiO2 gel, and then cooled to room temperature to form RF-GLU@SiO2 wet gel;
[0038] S4, RF-GLU@SiO2 aerogel was obtained by ethanol solvent replacement and normal pressure drying;
[0039] S5, carbonizing the RF-GLU@SiO2 aerogel at 1000°C to obtain CC@SiO2 aerogel;
[0040] S6. In the presence of sufficient carbon atoms, the CC@SiOx nanomaterial is formed through a high temperature of 1500°C. In this embodiment, X=1.1.
[0041] The silicon-doped nanoporous carbon material prepared by this method is used as a negative electrode material for lithium-ion batteries, with a capacity of up to 3265 mA∙h / g. Example 2
[0042] A method for preparing a nested coated silicon-carbon material comprises the following steps:
[0043] S1. Add 16 ml of methyl orthosilicate to 0.5 g of urea, mix and stir in 25 ml of deionized water and 85 ml of ethanol solvent, form SiO2 sol through hydrolysis and polycondensation, use 3 g of cellulose to coat a 10 nm organic shell on the surface of SiO2 nanoparticles, and then centrifuge at a centrifugal speed of 7000-10000 r / min for 10-20 min to form cellulose-coated SiO2 nanoparticles with a core-shell structure;
[0044] S2, then phenol and formaldehyde were used to prepare an organic network skeleton by a sol-gel method (41 ml, phenol and formaldehyde ratio 1:2), and after mixing, they were grown together with cellulose-coated SiO2 nanoparticles to form a three-dimensional network skeleton;
[0045] S3, the obtained sol is sealed and placed in a vacuum drying oven for aging at 45°C for 4 days to form RF-cellulose@SiO2 gel, and then cooled to room temperature to form RF-cellulose@SiO2 wet gel;
[0046] S4, RF-cellulose@SiO2 aerogel was obtained after ethanol solvent replacement and normal pressure drying;
[0047] S5, carbonizing the RF-cellulose@SiO2 aerogel at 1000°C to obtain CC@SiO2 aerogel;
[0048] S6. In the presence of sufficient carbon atoms, the CC@SiOx nanomaterial is formed by subjecting the mixture to a high temperature of 1500°C. In this embodiment, X=1.7.
[0049] The silicon-doped nanoporous carbon material prepared by this method is used as a negative electrode material for lithium-ion batteries, with a capacity of up to 1073 mA∙h / g. Example 3
[0050] A method for preparing a nested coated silicon-carbon material comprises the following steps:
[0051] S1. 3 g SiO2 aerogel powder was dissolved in 85 ml aqueous solution under the catalytic effect of 0.2 g urea, and stirred evenly to obtain SiO2 sol. 1.4 g glucose (GLU) was used to coat a 10 nm organic shell on the surface of SiO2 nanoparticles to form GLU@SiO2 nanoparticles with a core-shell structure.
[0052] S2, then the dianhydride and diamine were used to prepare an organic network skeleton by a sol-gel method (38 ml, dianhydride and diamine ratio 1:1), and after mixing, they were grown together with GLU@SiO2 nanoparticles to form a three-dimensional network skeleton;
[0053] S3, the obtained sol is sealed and placed in a vacuum drying oven for aging at 30°C for 2 days to form a polyimide-GLU@SiO2 gel, which is then cooled to room temperature to form a polyimide-GLU@SiO2 wet gel;
[0054] S4, polyimide-GLU@SiO2 aerogel was obtained by acetone solvent replacement and normal pressure drying;
[0055] S5, subjecting the polyimide-GLU@SiO2 aerogel to high temperature carbonization at 1000°C to carbonize the organic components to obtain CC@SiO2 aerogel;
[0056] S6. In the presence of sufficient carbon atoms, the CC@SiOx nanomaterial is formed by subjecting the mixture to a high temperature of 1500°C. In this embodiment, X=0.7.
[0057] The silicon-doped nanoporous carbon material prepared by this method is used as a negative electrode material for lithium-ion batteries, with a capacity of up to 817 mA∙h / g. Example 4
[0058] A method for preparing a nested coated silicon-carbon material comprises the following steps:
[0059] S1. Dissolve 3g SiO2 aerogel powder in 100ml aqueous solution under the catalytic action of 0.2g urea, stir evenly to prepare SiO2 sol, add 1.6ml sodium dodecylbenzene sulfonate (0.5wt%), and use 35ml phenolic resin (RF) to coat a 10nm organic shell on the surface of SiO2 nanoparticles to form RF@SiO2 nanoparticles with a core-shell structure;
[0060] S2, then the chitosan aqueous solution (solid content 23%) is used to prepare an organic network skeleton through a sol-gel method, and grown together with RF@SiO2 nanoparticles to form a three-dimensional network skeleton;
[0061] S3, the obtained sol is sealed and placed in a vacuum drying oven for aging at 30°C for 3 days to form a chitosan-RF@SiO2 gel, which is then cooled to room temperature to form a chitosan-RF@SiO2 wet gel;
[0062] S4, chitosan-RF@SiO2 aerogel was obtained by acetone solvent replacement and normal pressure drying;
[0063] S5, subjecting the chitosan-RF@SiO2 aerogel to high temperature carbonization at 1000°C to carbonize the organic components to obtain CC@SiO2 aerogel;
[0064] S6. In the presence of sufficient carbon atoms, the CC@SiOx nanomaterial is formed by subjecting the mixture to a high temperature of 1500°C. In this embodiment, X=0.9.
[0065] The silicon-doped nanoporous carbon material prepared by this method is used as a negative electrode material for lithium-ion batteries, with a capacity of up to 2383 mA∙h / g.
[0066] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.
Claims
1. A method for preparing a nested coated silicon-carbon material, comprising the following steps: S1. Add 10 ml of methyl orthosilicate to 0.7 g of urea, mix and stir in 30 ml of deionized water and 100 ml of ethanol solvent, form SiO2 sol through hydrolysis and polycondensation, add 2.3 ml of α-olefin sulfate, and then pour into 7.9 ml of glucose solution. After uniform stirring and centrifugation, use glucose to coat a 10 nm organic shell on the surface of SiO2 nanoparticles, and then centrifuge at a centrifugal speed of 7000-10000 r / min for 10-20 min to form GLU@SiO2 nanoparticles with a core-shell structure. S2, then phenol and formaldehyde are used to prepare an organic network skeleton sol by a sol-gel method, the ratio of phenol to formaldehyde is 1:2, GLU@SiO2 nanoparticles are added to the sol, and the sol and GLU@SiO2 nanoparticles grow together to form a three-dimensional network skeleton; S3, the obtained sol is sealed and placed in a vacuum drying oven for aging at 60°C for 3 days to form RF-GLU@SiO2 gel, and then cooled to room temperature to form RF-GLU@SiO2 wet gel; S4, RF-GLU@SiO2 aerogel was obtained by ethanol solvent replacement and normal pressure drying; S5, carbonizing the RF-GLU@SiO2 aerogel at 1000°C to obtain CC@SiO2 aerogel; S6. In the presence of sufficient carbon atoms, the CC@SiOx nanomaterial is formed at a high temperature of 1500°C, where X=1.1; The silicon-doped nanoporous carbon material prepared by this method is used as a negative electrode material for lithium-ion batteries, and its capacity is 3265 mA∙h / g.
Citation Information
Patent Citations
Preparation method of silicon carbon negative plate, silicon carbon negative plate and lithium ion battery
CN107579227A
Silicon-oxygen-carbon negative electrode material taking cellulose / silicon dioxide aerogel as precursor and preparation method thereof
CN113410450A