Silicon carbide cementing cement for high temperature wells and preparation method thereof
By preparing silicon carbide fine powder and aluminum isopropoxide to react to form high-temperature resistant stabilizers, combined with oil well cement and other materials, silicon carbide cementing cement, the problem of cementite strength decline and insufficient thermal conductivity at high temperature is solved, and the problem of cementite strength decline and thermal conductivity is achieved. Improved stability and thermal conductivity under high temperature conditions.
Patent Information
- Application Number
- CN202411025928.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The strength of existing high-temperature cementing cement declines under high temperature and high pressure conditions, and it is difficult to meet the needs of high temperature and thermal conductivity in deep underground wells.
By preparing silicon carbide fine powder and reacting with aluminum isopropoxide, ethyl orthosilicate, etc. to form high temperature resistant stabilizers, and combined with oil well cement, dispersant, retarder, etc., silicon carbide cementing cementing cementing cement to improve cement resistance of cement High temperature performance and thermal conductivity.
It significantly improves the high-temperature resistance and thermal conductivity of cement, reduces the strength decay rate at high temperature, and maintains good thermal conductivity under high temperature conditions, and is suitable for cementing needs of deep wells and geothermal wells.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cementing cement materials, and in particular relates to silicon carbide cementing cement for high-temperature wells and a preparation method thereof. Background Art
[0002] Cementing is the premise and foundation for the safe, economical and efficient development of oil and gas resources, and is also a key link in the construction of oil and gas wells. Cementing is to inject cement slurry into the annulus between the casing and the formation, which plays a role in isolating complex formations that are prone to collapse and leakage, isolating oil, gas and water layers, establishing oil and gas outflow channels, preventing cross-channeling between production layers, and protecting casing. Therefore, the quality of cementing will directly affect the mining safety, production life and economic benefits of oil and gas wells. In recent years, my country has made major breakthroughs in deep oil and gas exploration and development. Shendi Tako 1 Well has become the first well in my country to exceed 10,000 meters in drilling depth. The development of deep layers has brought new challenges to cementing technology. The first problem is how to solve the difficulties in designing cement slurry systems under high temperature and high pressure (bottom hole circulation temperature>160℃) during high temperature cementing and the problem of cement stone strength decline caused by high temperature at the bottom of the well. On the other hand, green energy such as geothermal energy is also developing rapidly, and geothermal wells are moving deeper and deeper. The lower cementing of deep geothermal wells not only requires cement stone to have good resistance to high temperature decay, but also requires cement stone to have good heat transfer and thermal conductivity to improve energy utilization efficiency. The solution to these technical difficulties must rely on breakthroughs in cementing cement materials.
[0003] Since the calcium-silicon ratio of the mineral composition of G-grade cement determines the instability of the crystal form of the hydration product at high temperature, thus causing structural instability, the existing high-temperature cementing cement usually uses G-grade oil well cement as the basic cement, and then adds fly ash, slag, quartz sand and other admixtures and high-temperature retarders to prepare high-temperature cementing cement to meet the requirements of cementing construction, mainly solving the high-temperature stability problem of cement slurry within 200°C. However, in recent years, with the deepening of oil and gas exploration and development, the bottom temperature of the well has become higher and higher, reaching above 240°C, and some wells even exceed 300°C (such as shale oil in-situ conversion wells). There are also some literatures that have studied the high-temperature resistant cement slurry system within this temperature range, but no relatively mature products and solutions have yet been formed. Summary of the invention
[0004] In view of the defects of the prior art, the present invention provides a silicon carbide cementing cement for high-temperature wells and a preparation method thereof, by preparing a high-temperature resistant stabilizer, which is added to the cement to greatly improve the high-temperature resistance of the cement.
[0005] A silicon carbide cementing cement for high-temperature wells is prepared from the following raw materials in parts by weight: 110-120 parts of oil well cement, 50-55 parts of water, 10-15 parts of high-temperature stabilizer, 2-4 parts of dispersant, 1-4 parts of retarder, and 2-4 parts of fluid loss reducer, wherein the high-temperature stabilizer is prepared by the following method:
[0006] (S1) ball milling and sieving silicon carbide to obtain silicon carbide fine powder;
[0007] (S2) Aluminum isopropoxide and ethyl orthosilicate are mixed and added to ethanol, and the mixture is stirred and mixed evenly. A hydrochloric acid solution is added, and the mixture is stirred and reacted at 40-50° C. for 3-5 hours. Then, the silicon carbide fine powder obtained in step (S1) is added thereto, and the mixture is stirred and mixed evenly. The mixture is heat-insulated for aging, drying, and calcining to obtain the high temperature resistant stabilizer.
[0008] Preferably, the mass ratio of aluminum isopropoxide, tetraethyl orthosilicate, ethanol, hydrochloric acid solution and silicon carbide fine powder is 7-12:15-20:150-200:12-15:2-3.
[0009] Preferably, the concentration of the hydrochloric acid solution is 1-3 mol / L.
[0010] Preferably, the heat preservation and aging time is 5-7h.
[0011] Preferably, the calcination condition is calcination at 400-600° C. for 1-3 h; and the drying condition is drying at 105-110° C. for 1-2 h.
[0012] Preferably, the mesh size of the sieve is 300-500 meshes.
[0013] Preferably, the dispersant is an aldehyde-ketone condensate.
[0014] Preferably, the retarder is a compound of borax and lignin sulfonate.
[0015] Preferably, the fluid loss additive is 2-acrylamido-2-methylpropanesulfonic acid polymer (AMPS polymer for short).
[0016] The method for preparing silicon carbide cementing cement for high-temperature wells comprises the following steps: adding oil well cement into water, stirring and mixing evenly, heating to 40-50° C., adding a high temperature stabilizer, a dispersant, a retarder, and a fluid loss reducer, stirring evenly, and obtaining the silicon carbide cementing cement.
[0017] Advantages of the present invention:
[0018] (1) The present invention mixes silicon carbide and Al / Si oxide uniformly and prepares a high temperature resistant stabilizer through a sol-gel reaction, which has good high temperature resistance and mechanical improvement properties. After being added to cement, the high temperature resistant stabilizer improves the high temperature resistance of cementing cement, so that the hydration process of cement better meets the high temperature cementing requirements, and can effectively solve the problem of high temperature strength decline of cement stone in deep well and ultra-deep well cementing projects;
[0019] (2) The cementing slurry prepared by the present invention not only has good high temperature resistance, but also has strong heat transfer and thermal conductivity, and can meet the demand for cementing thermal conductive cement under working conditions such as geothermal wells and shale oil in-situ conversion;
[0020] (3) The preparation method of the present invention is simple and the raw materials are widely available. The high-efficiency cement slurry prepared has good engineering properties, can withstand high temperatures, and has broad application prospects. DETAILED DESCRIPTION
[0021] The parts referred to in the embodiments of the present invention are all parts by weight;
[0022] The model of the dispersant aldehyde-ketone condensate used in the embodiment of the present invention is SXY-2;
[0023] The retarder used in the embodiment of the present invention is HR-20 retarder or HR-25 retarder purchased from Halliburton, both of which are composites of borax and lignin sulfonate;
[0024] The fluid loss additive used in the embodiment of the present invention is G34S fluid loss additive or G310HS fluid loss additive purchased from Weihui Chemical Co., Ltd., both of which are 2-acrylamido-2-methylpropanesulfonic acid polymers.
[0025] Example 1
[0026] A silicon carbide cementing cement for high-temperature wells is prepared from the following raw materials in parts by weight: 110 parts of oil well cement, 50 parts of water, 10 parts of high-temperature stabilizer, 2 parts of dispersant aldehyde-ketone condensate, 1 part of HR-20 retarder, and 2 parts of G34S fluid loss reducer, wherein the high-temperature stabilizer is prepared by the following method:
[0027] (S1) ball milling silicon carbide and passing it through a 300-mesh sieve to obtain silicon carbide fine powder;
[0028] (S2) 7 parts of aluminum isopropoxide and 15 parts of tetraethyl orthosilicate are mixed and added to 150 parts of ethanol, and the mixture is stirred and mixed evenly. 12 parts of 1 mol / L hydrochloric acid solution are added, and the mixture is stirred and reacted at 40° C. for 3 hours. Then, 2 parts of the silicon carbide fine powder obtained in step (S1) are added thereto, and the mixture is stirred and mixed for 30 minutes. The mixture is heat-insulated and aged for 5 hours, dried at 110° C. for 1 hour, and calcined at 400° C. for 1 hour to obtain the high temperature resistant stabilizer.
[0029] The method for preparing the silicon carbide cementing cement for high-temperature wells comprises: adding oil well cement into water, stirring and mixing evenly, heating to 40° C., adding a high-temperature stabilizer, a dispersant, a retarder, and a fluid loss reducer, stirring evenly, and obtaining the silicon carbide cementing cement.
[0030] Example 2
[0031] A silicon carbide cementing cement for high-temperature wells is prepared from the following raw materials in parts by weight: 120 parts of oil well cement, 55 parts of water, 15 parts of high-temperature stabilizer, 4 parts of dispersant aldehyde-ketone condensate, 4 parts of HR-25 retarder, and 4 parts of G310HS fluid loss reducer, wherein the high-temperature stabilizer is prepared by the following method:
[0032] (S1) ball milling silicon carbide and passing it through a 500-mesh sieve to obtain silicon carbide fine powder;
[0033] (S2) 12 parts of aluminum isopropoxide and 20 parts of tetraethyl orthosilicate are mixed and added to 200 parts of ethanol, and the mixture is stirred and mixed evenly. 15 parts of 3 mol / L hydrochloric acid solution are added, and the mixture is stirred and reacted at 50° C. for 5 hours. Then, 3 parts of silicon carbide fine powder obtained in step (S1) are added thereto, and the mixture is stirred and mixed for 30 minutes. The mixture is heat-insulated and aged for 7 hours, dried at 105° C. for 2 hours, and calcined at 600° C. for 3 hours to obtain the high temperature resistant stabilizer.
[0034] The method for preparing the silicon carbide cementing cement for high-temperature wells comprises: adding oil well cement into water, stirring and mixing evenly, heating to 50° C., adding a high-temperature stabilizer, a dispersant, a retarder, and a fluid loss reducer, stirring evenly, and obtaining the silicon carbide cementing cement.
[0035] Example 3
[0036] A silicon carbide cementing cement for high-temperature wells is prepared from the following raw materials in parts by weight: 115 parts of oil well cement, 52 parts of water, 12 parts of high-temperature stabilizer, 3 parts of dispersant aldehyde-ketone condensate, 2 parts of HR-20 retarder, and 3 parts of G310HS fluid loss reducer, wherein the high-temperature stabilizer is prepared by the following method:
[0037] (S1) ball milling silicon carbide and passing it through a 400-mesh sieve to obtain silicon carbide fine powder;
[0038] (S2) 10 parts of aluminum isopropoxide and 17 parts of tetraethyl orthosilicate are mixed and added to 170 parts of ethanol, and the mixture is stirred and mixed evenly. 13.5 parts of 2 mol / L hydrochloric acid solution are added, and the mixture is stirred and reacted at 45° C. for 4 hours. Then, 2.5 parts of the silicon carbide fine powder obtained in step (S1) are added thereto, and the mixture is stirred and mixed for 30 minutes. The mixture is heat-insulated and aged for 6 hours, dried at 105° C. for 2 hours, and calcined at 500° C. for 2 hours to obtain the high temperature resistant stabilizer.
[0039] The method for preparing the silicon carbide cementing cement for high-temperature wells comprises: adding oil well cement into water, stirring and mixing evenly, heating to 45° C., adding a high-temperature stabilizer, a dispersant, a retarder, and a fluid loss reducer, stirring evenly, and obtaining the silicon carbide cementing cement.
[0040] Comparative Example 1
[0041] When preparing the high temperature resistant stabilizer, the aluminum isopropoxide in step (S2) is replaced by ethyl orthosilicate, and the high temperature resistant stabilizer is prepared by the following method:
[0042] (S1) ball milling silicon carbide and passing it through a 400-mesh sieve to obtain silicon carbide fine powder;
[0043] (S2) adding 27 parts of tetraethyl orthosilicate to 170 parts of ethanol, stirring and mixing evenly, adding 13.5 parts of 2 mol / L hydrochloric acid solution, stirring and reacting at 45°C for 4 hours, and then adding 2.5 parts of the silicon carbide fine powder obtained in step (S1), stirring and mixing for 30 minutes, keeping warm for 6 hours, drying at 105°C for 2 hours, and calcining at 500°C for 2 hours to obtain the high temperature resistant stabilizer;
[0044] The rest is the same as Example 3.
[0045] Comparative Example 2
[0046] When preparing the high temperature resistant stabilizer, in step (S2), ethyl orthosilicate is replaced by aluminum isopropoxide, and the high temperature resistant stabilizer is prepared by the following method:
[0047] (S1) ball milling silicon carbide and passing it through a 400-mesh sieve to obtain silicon carbide fine powder;
[0048] (S2) adding 27 parts of aluminum isopropoxide to 170 parts of ethanol, stirring and mixing evenly, adding 13.5 parts of 2 mol / L hydrochloric acid solution, stirring and reacting at 45°C for 4 hours, and then adding 2.5 parts of silicon carbide fine powder obtained in step (S1), stirring and mixing for 30 minutes, keeping warm for 6 hours, drying at 105°C for 2 hours, and calcining at 500°C for 2 hours to obtain the high temperature resistant stabilizer;
[0049] The rest is the same as Example 3.
[0050] Comparative Example 3
[0051] When preparing the high temperature resistant stabilizer, silicon carbide is not added, and the high temperature resistant stabilizer is prepared by the following method:
[0052] 10 parts of aluminum isopropoxide and 17 parts of tetraethyl orthosilicate were mixed and added to 170 parts of ethanol, and the mixture was stirred and mixed evenly, and 13.5 parts of 2 mol / L hydrochloric acid solution were added, and the mixture was stirred and reacted at 45° C. for 4 hours, and the mixture was kept warm for 6 hours, dried at 105° C. for 2 hours, and calcined at 500° C. for 2 hours to obtain the high temperature resistant stabilizer;
[0053] The rest is the same as Example 3.
[0054] Comparative Example 4
[0055] No high temperature resistant stabilizer is added, and the rest is the same as in Example 3.
[0056] Performance Testing
[0057] 1. High temperature strength decay detection
[0058] The high temperature strength decay of the cementing cement obtained in Examples 1-3 and Comparative Examples 1-4 was tested (the method refers to SY / T6466-2016). The compressive strength test instrument is a YJ-2001 pressure testing machine, and the cement stone curing instrument is a DFC-0720 pressurized curing kettle. Since the current maximum operating temperature of the pressurized curing kettle is 375°C, and the temperature of domestic and foreign oil fields and geothermal wells does not exceed this value, the experimental temperature is set to 250°C and 350°C, and the test results are shown in Table 1;
[0059] Table 1 Compressive strength test results of different systems
[0060]
[0061] As can be seen from Table 1, the cementing cements prepared in Examples 1-3 of the present invention have two outstanding features: first, the strength development is high at room temperature, and the compressive strength is higher than that of other comparative examples; second, after high-temperature curing, the strength decay is low, with the highest being only 6.73%, while the highest strength decay rate at 7d in the comparative example is high, and with the increase of temperature, the decay rate increases significantly, with the maximum reaching 44.48%. Further analysis shows that the addition of silicon carbide can alleviate the decay of strength at different temperatures to a certain extent, but it can only produce a small improvement through close stacking, and it is still decaying to a large extent overall. The overall decay rate of the cement prepared by the present invention under different high-temperature curing is relatively low, which is mainly because the present invention uses a sol-gel reaction to evenly mix silicon carbide and Al / Si oxide to prepare a high-temperature stabilizer with good high-temperature resistance and mechanical improvement properties.
[0062] 2. The permeability of cement paste was further tested using HK-4 automatic permeability tester. The test method was based on GB / T 19139-2012. The results are shown in Table 2.
[0063] Table 2 Permeability test results of different systems
[0064]
[0065] The test results further confirm that the coarsening of the microstructure is the main reason for the decline in strength, and the result is the increase in permeability. The permeability of the embodiment of the present invention system does not change much after curing under high temperature conditions, while the permeability of the comparative examples increases significantly, especially comparative examples 3 and 4, which increase by more than 5 times. The cement stone structure becomes loose to a certain extent, which is seriously unfavorable for the corrosion and damage protection of the casing.
[0066] 3. Thermal conductivity test
[0067] The thermal conductivity of the high temperature cementing slurries prepared in Examples 1-3 and Comparative Examples 1-4 was tested (the method was based on GB / T22588-2008). Before the test, they were cured at room temperature and 350°C for 7 days respectively. The test instrument was a NETZSCH LFA467 thermal conductivity tester. The results are shown in Table 3.
[0068] Table 3 Thermal conductivity test results of different systems
[0069]
[0070] The test results show that the present invention can improve the thermal conductivity of cement stone, which can be increased by 48.77% under normal temperature curing conditions compared with the blank sample (Comparative Example 4), which is mainly due to the addition of high temperature resistant stabilizers. After high temperature curing at 350°C, the thermal conductivity of cements of different types has decreased to a certain extent, but the overall reduction rate of the embodiments of the present invention is relatively small, generally less than 5%. The reduction rates of the comparative examples are all higher than 20%, and the reduction degree of the blank samples has exceeded 30%, which has a lot to do with the degradation of cement and loose structure under high temperature. The technical solution of the present invention has alleviated the above process very well, so that the cement stone still maintains good thermal conductivity at high temperatures.
Claims
1. A silicon carbide cementing cement for high temperature wells, characterized in that: The invention is prepared from the following raw materials in parts by weight: 110-120 parts of oil well cement, 50-55 parts of water, 10-15 parts of high temperature resistant stabilizer, 2-4 parts of dispersant, 1-4 parts of retarder, and 2-4 parts of fluid loss reducer, wherein the high temperature resistant stabilizer is prepared by the following method: (S1) ball milling and sieving silicon carbide to obtain silicon carbide fine powder; (S2) mixing aluminum isopropoxide and tetraethyl orthosilicate and adding them to ethanol, stirring and mixing them evenly, adding hydrochloric acid solution, stirring and reacting at 40-50° C. for 3-5 hours, and then adding the silicon carbide fine powder obtained in step (S1), stirring and mixing them evenly, keeping warm for aging, drying, and calcining to obtain the high temperature resistant stabilizer; The mass ratio of the aluminum isopropoxide, tetraethyl orthosilicate, ethanol, hydrochloric acid solution and silicon carbide fine powder is 7-12:15-20:150-200:12-15:2-3.
2. The silicon carbide cementing cement for high temperature wells according to claim 1, characterized in that: The concentration of the hydrochloric acid solution is 1-3 mol / L.
3. The silicon carbide cementing cement for high temperature wells according to claim 2, characterized in that: The heat preservation and aging time is 5-7h.
4. The silicon carbide cementing cement for high temperature wells according to claim 3, characterized in that: The calcination conditions are calcination at 400-600° C. for 1-3 h; the drying conditions are drying at 105-110° C. for 1-2 h.
5. The silicon carbide cementing cement for high temperature wells according to claim 1, characterized in that: The mesh number of the sieve is 300-500 meshes.
6. The silicon carbide cementing cement for high temperature wells according to claim 1, characterized in that: The dispersant is an aldehyde-ketone condensate.
7. The silicon carbide cementing cement for high temperature wells according to claim 1, characterized in that: The retarder is a compound of borax and lignin sulfonate.
8. The silicon carbide cementing cement for high temperature wells according to claim 1, characterized in that: The fluid loss reducer is 2-acrylamido-2-methylpropanesulfonic acid polymer.
9. The method for preparing silicon carbide cementing cement for high temperature wells according to claim 1, characterized in that: Specifically, the oil well cement is added into water, stirred and mixed evenly, heated to 40-50° C., a high temperature stabilizer, a dispersant, a retarder and a fluid loss reducer are added, stirred evenly, and the silicon carbide cementing cement is obtained.
Citation Information
Patent Citations
Cementing slurry system suitable for large range of temperature
CN102127404A
Thermal insulation coating for building exterior walls and preparation method of thermal insulation coating
CN110484119A
Impermeable self-compacting concrete and preparation method thereof
CN113526927A
Ultrahigh-temperature well cementation cement paste as well as preparation method and application thereof
CN114620977A
High-strength lightweight refractory material and preparation method thereof
CN115231927A