A kind of construction waste recycled concrete, preparation method and application

By pressurizing the recycled coarse aggregate of construction waste in a glass powder mixed solution and adding silica fume and cement mortar, alkali and silicone and secondary hydration reactions, the compression resistance, crack resistance and durability of recycled construction waste are improved by using alkali and silicone and secondary hydration reactions. Performance solves the problem of insufficient performance in the prior art.

CN118545964BActive Publication Date: 2024-12-06HUNAN YUNZHONG REGENERATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411012187.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-12-06
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing recycled concrete of construction waste is insufficient in terms of compressive strength, splitting strength and carbonization depth, and comprehensive performance needs to be improved.

Method used

The regenerated coarse aggregate of construction waste is placed in a glass powder mixed solution for pressurization treatment. After the pretreated aggregate is generated, silica fume and cement mortar are added. Through alkali and silicone reaction and secondary hydration reaction, expandable alkali silicate coagulation is formed. Glue and aluminosilicate gels to enhance the aggregate structure.

Benefits of technology

It significantly improves the permeability, freezing resistance, compressive strength and splitting strength of recycled concrete of construction waste, reduces water absorption, and enhances overall strength and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118545964B_ABST
    Figure CN118545964B_ABST
Patent Text Reader

Abstract

The present invention provides a construction waste recycled concrete, a preparation method and application; the preparation method of the construction waste recycled concrete comprises the following steps: S1, taking construction waste recycled coarse aggregate; S2, placing the construction waste recycled coarse aggregate in a glass powder mixed solution to obtain a feed liquid, and pressurizing the feed liquid; the glass powder mixed solution comprises glass powder, water and sodium hydroxide; S3, after the pressurization treatment, separating the construction waste recycled coarse aggregate in the feed liquid to obtain a pretreated aggregate; then, mixing silica fume into the pretreated aggregate to obtain a premix; S4, mixing cement mortar into the premix to obtain construction waste recycled concrete. The present invention can enhance the performance of construction waste recycled concrete in terms of compressive strength, splitting strength, carbonization depth and the like, and improve the application value of construction waste recycled concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of concrete, and in particular to construction waste recycled concrete, a preparation method and application thereof. Background Art

[0002] The rapid development of urban construction will inevitably generate a large amount of construction waste. Among them, recycled coarse aggregate from construction waste is obtained after sorting, crushing and screening of construction waste. The quality of recycled concrete directly made from recycled coarse aggregate from construction waste is usually not high. Therefore, how to obtain high-performance concrete based on recycled aggregate from construction waste is one of the effective ways to achieve the reduction and resource utilization of construction waste, and it is also the main technical difficulty that needs to be overcome at present.

[0003] The Chinese invention patent application with publication number CN111892375A discloses a construction waste recycled concrete and a preparation method thereof, wherein the construction waste recycled concrete is prepared by using construction waste recycled coarse aggregate, silica fume mixture, cement, river sand, water and water reducing agent. Although the above patent application can obtain concrete for construction; however, due to the influence of construction waste recycled coarse aggregate on concrete, it does not obtain higher quality construction waste recycled concrete. The construction waste recycled concrete in the patent application still needs to be strengthened in terms of compressive strength, splitting strength, carbonization depth, etc., and the comprehensive performance needs to be further improved.

[0004] In view of this, it is necessary to provide a construction waste recycled concrete, a preparation method and an application to solve or at least alleviate the technical defects of how to improve the comprehensive performance of construction waste recycled concrete. Summary of the invention

[0005] The main purpose of the present invention is to provide a construction waste recycled concrete, a preparation method and an application, aiming to solve the above-mentioned technical problem of how to improve the comprehensive performance of construction waste recycled concrete.

[0006] To achieve the above object, the present invention provides a method for preparing recycled concrete from construction waste, comprising the steps of:

[0007] S1, taking recycled coarse aggregate from construction waste;

[0008] S2, placing the construction waste recycled coarse aggregate in a glass powder mixed solution to obtain a liquid; and subjecting the liquid to a pressure treatment. The pressure treatment comprises: applying a pressure of 800-2000 kPa to the liquid for a period of 10-30 minutes;

[0009] The mass ratio of the recycled coarse aggregate from construction waste to the mixed solution of glass powder is 1:3-10; the mixed solution of glass powder includes glass powder, water and sodium hydroxide; in the mixed solution of glass powder, the mass ratio of glass powder, water and sodium hydroxide is 1:5-10:0.02-0.1;

[0010] S3, after the pressurization treatment, separating the recycled coarse aggregate from the construction waste in the liquid to obtain pretreated aggregate; then, mixing silica fume into the pretreated aggregate to obtain a premix; the mass ratio of the recycled coarse aggregate from the construction waste to the silica fume is 1:0.01-0.1;

[0011] S4, mixing cement mortar into the premix to obtain construction waste recycled concrete; the mass ratio of the construction waste recycled coarse aggregate to the cement mortar is 1:0.8-1.5.

[0012] Furthermore, the pressure treatment process is carried out in a pressure vessel, and the direction of applying pressure is from top to bottom.

[0013] Furthermore, the density of the glass powder used in the glass powder mixed solution is 2.4-2.7 g / cm 3 The specific surface area of ​​the glass powder used in the glass powder mixed solution is 200-300m 2 / kg.

[0014] Furthermore, the recycled coarse aggregate from construction waste has three particle sizes, the first particle size range of the recycled coarse aggregate from construction waste is 19-31.5 mm, the second particle size range of the recycled coarse aggregate from construction waste is 9.5-19 mm, and the third particle size range of the recycled coarse aggregate from construction waste is 4.75-9.5 mm.

[0015] The mass ratio of the first grade of recycled coarse aggregate from construction waste, the second grade of recycled coarse aggregate from construction waste, and the third grade of recycled coarse aggregate from construction waste is 1:1~5:1~5.

[0016] Furthermore, the construction waste recycled coarse aggregate contains concrete particles and mortar particles, and the concrete particles contain crushed stones and old slurry.

[0017] Furthermore, the density of the silica fume is 2.2-2.4 g / cm 3 The specific surface area of ​​the silica fume is 15000~20000m 2 / kg.

[0018] Furthermore, the method for obtaining the cement mortar includes: mixing cement, river sand, water, and a water reducing agent to obtain the cement mortar; in the cement mortar, the mass ratio of cement, river sand, water, and a water reducing agent is 1:1.5~3.5:0.4~0.7:0.006~0.01.

[0019] Furthermore, the process of mixing the cement mortar into the premix includes: placing a portion of the premix in a mold, and adding a portion of the cement mortar into the mold under vibration; then, adding another portion of the premix into the mold, and adding another portion of the cement mortar into the mold under vibration.

[0020] The present invention also provides a construction waste recycled concrete, which is prepared by any of the above-mentioned preparation methods for the construction waste recycled concrete.

[0021] The present invention also provides a use of any of the above-mentioned construction waste recycled concrete in building construction.

[0022] Compared with the prior art, the present invention has at least the following advantages:

[0023] The present invention can improve the comprehensive performance of recycled concrete from construction waste; the present invention can not only enable the recycled concrete from construction waste to have a higher level of impermeability and frost resistance, but also enhance its performance in terms of compressive strength, splitting strength, carbonization depth, etc. The invention adopts glass powder and silica fume to strengthen the recycled coarse aggregate of construction waste; under the action of external pressure, the glass powder enters the deep pores of the recycled aggregate, and generates an alkali-silicon reaction in an alkaline environment to generate an expansive alkali silicate gel, thereby blocking the pores of the recycled aggregate, reducing its water absorption rate and improving its strength; a layer of silica fume adheres to the surface of the recycled coarse aggregate of construction waste, and the silica fume and the old slurry of the recycled coarse aggregate of construction waste undergo a secondary hydration reaction, and a hydration reaction occurs in an alkaline environment to generate a large amount of aluminum silicate gel, thereby further strengthening the surface structure of the recycled aggregate; the glass powder in the pores of the recycled coarse aggregate of construction waste participates in the secondary hydration reaction of the silica fume and the old slurry, and the glass powder and the silica fume are hydrated in an alkaline environment, thereby increasing the amount of silicate gel and the silicon content of the hydration product in the pores and the interface area, and the silicate gel rich in silicon has a stronger bonding ability, further fills the pores and improves the interface structure and strength of the recycled aggregate and the new slurry, thereby improving the overall strength of the recycled concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0025] Figure 1 This is a microscopic morphology of the recycled concrete from construction waste in Example 1 of the present invention, corresponding to the holes in the recycled concrete from construction waste;

[0026] Figure 2 It is a microscopic morphology diagram of the recycled concrete from construction waste in Example 1 of the present invention, corresponding to the micro cracks in the recycled concrete from construction waste;

[0027] Figure 3 This is a microscopic morphology of the recycled concrete from construction waste in Comparative Example 1 of the present invention, corresponding to the holes in the recycled concrete from construction waste;

[0028] Figure 4 It is a microscopic morphology of the recycled concrete from construction waste in Comparative Example 1 of the present invention, corresponding to the micro cracks in the recycled concrete from construction waste;

[0029] Figure 5 It is a microscopic morphology of the recycled concrete from construction waste in Comparative Example 4 of the present invention, corresponding to the holes in the recycled concrete from construction waste;

[0030] Figure 6 It is a microscopic morphology of the recycled concrete from construction waste in Comparative Example 4 of the present invention, corresponding to the micro cracks in the recycled concrete from construction waste;

[0031] Figure 7 The old interface microhardness diagram of the construction waste recycled concrete in Example 1, Comparative Example 1 and Comparative Example 4 of the present invention;

[0032] Figure 8 This is the new interface microhardness diagram of the construction waste recycled concrete in Example 1, Comparative Example 1 and Comparative Example 4 of the present invention.

[0033] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0036] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention are familiar to those skilled in the art and the description of the present invention, and any methods, equipment and materials of the prior art similar or equivalent to the methods, equipment and materials described in the embodiments of the present invention can also be used to implement the present invention.

[0037] The present invention provides a method for preparing recycled concrete from construction waste, comprising the steps of:

[0038] S1, taking recycled coarse aggregate from construction waste, wherein the recycled coarse aggregate from construction waste may have multiple particle sizes.

[0039] In the present invention, the recycled coarse aggregate from construction waste can have three particle sizes, the particle size range of the recycled coarse aggregate from construction waste in the first grade is 19-31.5 mm, the particle size range of the recycled coarse aggregate from construction waste in the second grade is 9.5-19 mm, and the particle size range of the recycled coarse aggregate from construction waste in the third grade is 4.75-9.5 mm. The mass ratio of the recycled coarse aggregate from construction waste in the first grade, the recycled coarse aggregate from construction waste in the second grade, and the recycled coarse aggregate from construction waste in the third grade can be 1:1-5:1-5, and can further be 1:2-4:2-4.

[0040] It should be noted that the construction waste recycled coarse aggregate is obtained after sorting, crushing and screening of construction waste, and the construction waste recycled coarse aggregate usually contains concrete particles and mortar particles, and the concrete particles include crushed stone and old slurry. The construction waste recycled coarse aggregate is usually dried before use; that is, before use, the construction waste recycled coarse aggregate is dried at 100-105°C for 2-3 hours and then cooled to room temperature.

[0041] S2, placing the construction waste recycled coarse aggregate in a glass powder mixed solution to obtain a slurry; pressurizing the slurry; the pressurizing treatment includes: applying a pressure of 800~2000kPa to the slurry, and can further be 900~1100kPa; applying for 10~30min, and can further be 10~20min.

[0042] The process of the pressure treatment is usually carried out in a pressure vessel, and the direction of applying pressure is from top to bottom; that is, the pressure is applied downward from the liquid surface of the feed liquid. The pressure treatment may specifically include: loading the glass powder mixed solution into a pressure barrel with a piston, adding the construction waste recycled coarse aggregate into the glass powder mixed solution, thereby obtaining the feed liquid; then, opening the air valve, pressing the piston downward to make the piston contact with the liquid surface of the feed liquid, closing the air valve, and immediately applying a downward pressure of 800~2000kPa to the piston, and keeping the pressure constant for 10~30min.

[0043] In the present invention, the mass ratio of the construction waste recycled coarse aggregate to the glass powder mixed solution is 1:3~10, and can further be 1:3~6; the glass powder mixed solution includes glass powder, water, and sodium hydroxide; in the glass powder mixed solution, the mass ratio of glass powder, water, and sodium hydroxide is 1:5~10:0.02~0.1, and can further be 1:6~8:0.02~0.05.

[0044] The density of the glass powder used in the glass powder mixed solution can be 2.4-2.7 g / cm 3 The specific surface area of ​​the glass powder used in the glass powder mixed solution can be 200-300m 2 / kg; the glass powder in the glass powder mixed solution may include waste glass powder, which is powder ground from recycled waste glass. The sodium hydroxide used in the glass powder mixed solution is industrial flake caustic soda with a purity of more than 99%.

[0045] S3, after the pressurized treatment, separating the recycled coarse aggregate from construction waste in the slurry to obtain pretreated aggregate; then, mixing silica ash into the pretreated aggregate to obtain a premix; the mass ratio of the recycled coarse aggregate from construction waste to the silica ash is 1:0.01~0.1, and can further be 1:0.02~0.05.

[0046] Specifically, it can be understood as follows: separating the construction waste recycled aggregate from the glass powder mixed solution, then putting it into a stirring pot, stirring for 20 to 30 seconds, and mixing the silica fume during the stirring process.

[0047] The silica ash is the smoke generated during the high-temperature smelting process of industrial silicon and ferrosilicon. The density of the silica ash can be 2.2-2.4 g / cm 3 The specific surface area of ​​the silica fume can be 15000~20000m 2 / kg.

[0048] S4, mixing cement mortar into the premix to obtain construction waste recycled concrete; the mass ratio of the construction waste recycled coarse aggregate to the cement mortar is 1:0.8-1.5, and can further be 1:1-1.2; the construction waste recycled concrete solidifies during the placement process.

[0049] Those skilled in the art should know that the cement mortar is a mixture of cement, river sand, water and water reducer. In the present invention, the method for obtaining the cement mortar may include: mixing cement, river sand, water and water reducer to obtain the cement mortar; the mixing time may be 120~150s. In the cement mortar, the mass ratio of cement, river sand, water and water reducer may be 1:1.5~3.5:0.4~0.7:0.006~0.01, and may further be 1:2~3:0.45~0.65:0.006~0.01; in the present invention, the cement is one of ordinary Portland cement, Portland cement and composite Portland cement, and the 28-day strength is greater than 42.5MPa; the river sand is medium sand, and the fineness modulus is 2.3~3.1; the water reducer is a polycarboxylic acid water reducer.

[0050] In the present invention, the process of mixing the cement mortar into the premix may include: placing part of the premix in a mold, and adding part of the cement mortar to the mold under vibration; part of the premix may be 40-70% of the charge amount of the premix; and part of the cement mortar may be added in an amount of 30-60% of the charge amount of the cement mortar. Then, another part of the premix is ​​added to the mold, and another part of the cement mortar is added to the mold under vibration. In addition, after adding another part of the cement mortar, vibration may be continued for 10-20 seconds.

[0051] As an explanation of the nouns, the loading amount of the premix is: the total amount of the premix to be added to the mold; the loading amount of the cement mortar is: the total amount of the cement mortar to be added to the mold; the other part of the premix is: the remaining premix to be added to the mold in the loading amount of the premix; the other part of the cement mortar is: the remaining cement mortar to be added to the mold in the loading amount of the cement mortar.

[0052] In the implementation process of the present invention, the process of mixing the cement mortar into the premix may specifically include: loading the premix into the mold twice; loading 40-70% of the premix for the first time, and then placing it on a concrete vibration table for vibration, vibrating for 20-30 seconds, and slowly adding 30-60% of the cement mortar while vibrating, until the cement mortar is about to cover the premix, and at this time, some edges and corners of the recycled aggregate on the top layer are still exposed from the liquid surface of the cement mortar; then, loading the premix a little beyond the edge of the test mold for the second time, and then continue to vibrate, and after vibrating for 20-30 seconds, also vibrating and adding the remaining cement mortar, until the cement mortar covers the edge of the test mold, and then continue to vibrate for 10-20 seconds to scrape the surface of the test piece.

[0053] The present invention also provides a construction waste recycled concrete, which is prepared by any of the above-mentioned preparation methods for the construction waste recycled concrete.

[0054] The construction waste recycled concrete prepared by the present invention has a dense structure, uniform distribution of coarse aggregate, and can generate a large mechanical bite force when subjected to force, thereby improving the overall strength of the construction waste recycled concrete; it can not only make the construction waste recycled concrete have a higher impermeability grade and frost resistance grade, but also can enhance the performance of the construction waste recycled concrete in terms of compressive strength, splitting strength, carbonization depth, etc. The construction waste recycled concrete of the present invention has a large proportion of construction waste recycled coarse aggregate, and the construction waste recycled coarse aggregate is filled and adsorbed with a large amount of glass powder and silica fume, which can continuously undergo hydration reaction, can reduce the loss of concrete moisture, thereby reducing the shrinkage of the construction waste recycled concrete and the formation of shrinkage cracks, and improving the durability of the construction waste recycled concrete; the proportion of construction waste recycled coarse aggregate is relatively high, and part of the cement can also be saved.

[0055] The present invention also provides an application of any of the above-described construction waste recycled concrete in construction, especially in prefabricated buildings. The construction waste recycled concrete of the present invention is very suitable for prefabricated concrete components and can promote the application of construction waste recycled concrete in prefabricated buildings. The construction waste recycled concrete prepared by the present invention can solve the problems of poor working performance, low strength and poor durability of conventional construction waste recycled concrete. The present invention has good economic benefits, and because the raw materials are mainly large-scale urban solid wastes such as construction waste, waste glass and silica fume, the application of the present invention can greatly alleviate the pressure of solid waste on the urban environment, and its social benefits are far greater than the economic benefits.

[0056] The following are specific examples of the present invention:

[0057] Example 1

[0058] A method for preparing recycled concrete from construction waste, comprising the following steps:

[0059] 1. Take the recycled coarse aggregate from construction waste and dry it at 105°C for 3 hours; the recycled coarse aggregate from construction waste is obtained after sorting, crushing and screening of construction waste, and contains concrete particles and mortar particles. The concrete particles are composed of crushed stone and old slurry.

[0060] In this embodiment, the particle size of the recycled coarse aggregate from construction waste is divided into three levels, namely the first level, the second level and the third level; the particle size of the first level recycled coarse aggregate from construction waste is 19~31.5mm, the particle size of the second level recycled coarse aggregate from construction waste is 9.5~19mm, and the particle size of the third level recycled coarse aggregate from construction waste is 4.75~9.5mm.

[0061] Among the construction waste recycled coarse aggregates used in this embodiment, the mass ratio of the first-grade construction waste recycled coarse aggregates, the second-grade construction waste recycled coarse aggregates, and the third-grade construction waste recycled coarse aggregates is 1:3:3.

[0062] 2. Load the glass powder mixed solution into a pressure barrel with a piston, and add the construction waste recycled coarse aggregate that has been dried and cooled to room temperature into the glass powder mixed solution, which is recorded as the slurry; then, open the air valve of the pressure barrel, press the piston downward to make the piston contact with the liquid surface of the slurry, close the air valve, and immediately apply a downward pressure of 1000 kPa to the piston, and keep the pressure constant for 15 minutes; then, separate the construction waste recycled aggregate from the slurry to obtain the pretreated aggregate.

[0063] In this embodiment, the glass powder mixed solution is prepared by mixing waste glass powder, water and sodium hydroxide, and the density of the waste glass powder is 2.5 g / cm 3 , with a specific surface area of ​​260m 2 / kg; the sodium hydroxide is industrial flake caustic soda with a purity of 99.5%; in the glass powder mixed solution, the mass ratio of waste glass powder, water and sodium hydroxide is 1:7:0.03; the mass ratio of construction waste recycled coarse aggregate and glass powder mixed solution is 1:4.

[0064] 3. Stir the pretreated aggregate for 30 seconds, and add silica fume to the pretreated aggregate during the stirring process to obtain a premix; the mass ratio of construction waste recycled coarse aggregate to silica fume is 1:0.03; the density of silica fume is 2.25g / cm 3 , the specific surface area is 1.68×10 4 m 2 / kg.

[0065] 4. Prepare cement mortar; the preparation process of cement mortar is: put cement, river sand, water and water reducing agent into a mixing pot and stir for 120s.

[0066] In this embodiment, the cement is P·O42.5 cement; the river sand is medium sand with a fineness modulus of 2.4; the water reducer is PCA-Ⅰ polycarboxylate water reducer produced by Jiangsu Subote New Materials Co., Ltd.; in the cement mortar, the mass ratio of cement, river sand, water and water reducer is 1:2.5:0.5:0.008.

[0067] 5. Load the premix and cement mortar into a test mold to obtain construction waste recycled concrete; the mass ratio of construction waste recycled coarse aggregate to cement mortar is 1:1.1.

[0068] In this embodiment, the premix is ​​loaded into the test mold twice; 2 / 3 of the premix test mold is loaded for the first time, and then it is placed on a concrete vibration table for vibration. After 25 seconds of vibration, the stirred cement mortar is slowly added while vibrating until the cement mortar is almost covered by the premix (accounting for about 1 / 2 of the cement mortar loaded), and at this time, some edges and corners of the recycled aggregate on the top layer are still exposed from the cement mortar liquid surface; thereafter, the premix is ​​loaded a little beyond the edge of the test mold for the second time, and then vibration is continued. After 25 seconds of vibration, cement mortar is added while vibrating until the cement mortar is covered by the edge of the test mold, and then vibration is continued for 15 seconds to scrape the surface of the test piece.

[0069] Example 2

[0070] Compared with Example 1, this embodiment only adjusts the process of loading the premix and cement mortar into the test mold in step 5, and other conditions are the same as those in Example 1.

[0071] In this embodiment, the process of loading the premix and cement mortar into the test mold is as follows: loading the premix into the test mold twice; loading 1 / 2 of the premix test mold for the first time, and then placing it on a concrete vibration table for vibration. After vibrating for 20 seconds, slowly adding the stirred cement mortar while vibrating until the cement mortar is almost covered by the premix (accounting for about 2 / 5 of the cement mortar loading amount), at this time, some edges and corners of the recycled aggregate on the top layer are still exposed from the cement mortar liquid surface; then, loading the premix a little beyond the edge of the test mold for the second time, and then continue to vibrate. After vibrating for 20 seconds, cement mortar is added while vibrating until the cement mortar is over the edge of the test mold, and then continue to vibrate for 10 seconds to scrape the surface of the test piece.

[0072] Comparative Example 1

[0073] In this comparative example, the recycled concrete from construction waste is composed of cement, water reducing agent, recycled coarse aggregate from construction waste, river sand, water and silica fume; wherein the mass ratio of cement, water reducing agent, recycled coarse aggregate from construction waste, river sand and water is 1:0.008:3.7:2.5:0.5, and the mass ratio of recycled coarse aggregate from construction waste and silica fume is 1:0.03; the sources of the materials used in this comparative example are the same as those in Example 1.

[0074] In this comparative example, the recycled coarse aggregate from construction waste is first put into a mixing pot, followed by cement, silica fume and river sand, and then water and a water reducing agent. The mixture is fully stirred for 300 seconds, and finally molded and vibrated on a vibration table for 30 seconds. The mold is then scraped flat to obtain recycled concrete from construction waste.

[0075] Comparative Example 2

[0076] Compared with Example 1, this comparative example omits step 2, and the construction waste recycled coarse aggregate in step 1 is directly used as the pretreated aggregate in step 3. Other conditions are the same as those in Example 1.

[0077] Comparative Example 3

[0078] Compared with Example 1, in this comparative example, silica fume is not mixed into the pretreated aggregate, and the pretreated aggregate is directly used as a premix; other conditions are the same as those in Example 1.

[0079] Comparative Example 4

[0080] Compared with Example 1, in this comparative example, silica fume is replaced by fly ash, and the mass ratio of recycled coarse aggregate from construction waste to fly ash is 1:0.03. Other conditions are the same as those in Example 1.

[0081] Comparative Example 5

[0082] In this comparative example, steps 1 and 2 in Example 1 are used to obtain pretreated aggregates; then, the pretreated aggregates are put into a mixing pot, and then cement, silica fume and river sand are added, and then water and a water reducing agent are added, and the mixture is fully stirred for 300 seconds. Finally, the mixture is molded and vibrated on a vibration table for 30 seconds, and the test mold is scraped flat to obtain construction waste recycled concrete.

[0083] In this comparative example, the mass ratio of cement, water reducing agent, recycled coarse aggregate from construction waste, river sand and water is 1:0.008:3.7:2.5:0.5, and the mass ratio of recycled coarse aggregate from construction waste to silica fume is 1:0.03; the sources of raw materials used in this comparative example are the same as those in Example 1.

[0084] Analysis example 1

[0085] The construction waste recycled concrete in Examples 1-2 and Comparative Examples 1-5 was tested for 28-day compressive strength, 28-day splitting strength, 28-day impermeability grade, 28-day carbonization depth and 28-day frost resistance grade. The specific test steps were in accordance with the relevant provisions of the Standard Test Methods for Mechanical Properties of Ordinary Concrete (GB / T50081-2002) and the Standard Test Methods for Long-term Performance and Durability of Ordinary Concrete (GB / T50082-2009). The specific test results are shown in Table 1.

[0086] Table 1 Comparison of properties of recycled concrete from construction waste

[0087]

[0088] It can be seen from Table 1 that the construction waste recycled concrete prepared by the present invention has significantly improved compressive strength, splitting strength, impermeability, carbonation resistance and frost resistance compared with conventional recycled concrete (Comparative Example 1).

[0089] Compared with Comparative Example 2, Example 1 has significantly improved compressive strength, and the performance in other aspects is greatly improved, indicating that placing the recycled aggregate from construction waste in a mixed solution of glass powder and immersing it under pressure can significantly improve the comprehensive performance of the recycled concrete from construction waste.

[0090] Compared with Comparative Examples 3 and 5, Example 1 has certain improvements in various aspects of performance, indicating that after pressure treatment in the glass powder mixed solution, silica fume is first mixed into the pretreated aggregate and then formed in a mold, which can further improve the performance of the recycled concrete.

[0091] Compared with comparative example 4, the above-mentioned properties of Example 1 are all improved to a certain extent, indicating that silica fume is irreplaceable in the overall technical solution of the present invention.

[0092] Analysis example 2

[0093] Taking the construction waste recycled concrete of Example 1, Comparative Example 1 and Comparative Example 4 as an example, on the 28th day after the preparation, the microstructure of the aggregate in the construction waste recycled concrete was tested by a scanning electron microscope, and the chemical components of the hydration product (construction waste recycled concrete) were analyzed by an energy spectrum analyzer. At the same time, the old interface strength between the aggregate and the old slurry in the construction waste recycled concrete, as well as the new interface between the old slurry and the new slurry were analyzed by a microhardness tester. The specific test results are as follows: Figure 1-Figure 8 And as shown in Table 2.

[0094] Table 2 Analysis of chemical components of recycled concrete from construction waste

[0095]

[0096] From the microscopic analysis results, it can be seen that: the pores of the recycled concrete of Example 1 are filled with a large amount of glass powder and hydration reactants, and the original cracks are basically "healed"; the pores of the recycled concrete of Comparative Example 1 are basically free of fillers, and no hydration products are generated in the cracks; the recycled concrete of Comparative Example 4 has certain fillers in the pores, and there are also certain hydration products in the cracks, but compared with Example 1, the pore fillers are relatively small, and the cracks are basically not "healed". In addition, compared with Comparative Examples 1 and 4, the Ca / Si of the hydration product of Example 1 is low and the (Al+Fe) / Ca is high, indicating that more silicate gel is generated in the recycled concrete of Example 1, and the interface is well improved.

[0097] From the microhardness test results, it can be seen that the old interface and new interface strength of the construction waste recycled concrete in Example 1 are both higher than those in Comparative Example 1 and Comparative Example 4, indicating that Example 1 has a significant effect on improving the interface strength of the construction waste recycled concrete.

[0098] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing recycled concrete from construction waste, It is characterized in that Includes steps: S1, taking recycled coarse aggregate from construction waste; the recycled coarse aggregate from construction waste contains concrete particles and mortar particles, and the concrete particles contain crushed stone and old slurry; S2, placing the construction waste recycled coarse aggregate in a glass powder mixed solution to obtain a liquid feed; and pressurizing the liquid feed; The pressure treatment comprises: applying a pressure of 800-2000 kPa to the liquid for a period of 10-30 minutes; The mass ratio of the recycled coarse aggregate from construction waste to the mixed solution of glass powder is 1:3-10; the mixed solution of glass powder includes glass powder, water and sodium hydroxide; in the mixed solution of glass powder, the mass ratio of glass powder, water and sodium hydroxide is 1:5-10:0.02-0.1; S3, after the pressurization treatment, separating the recycled coarse aggregate from the construction waste in the liquid to obtain pretreated aggregate; then, mixing silica fume into the pretreated aggregate to obtain a premix; the mass ratio of the recycled coarse aggregate from the construction waste to the silica fume is 1:0.01-0.1; S4, mixing cement mortar into the premix to obtain construction waste recycled concrete; the mass ratio of the construction waste recycled coarse aggregate to the cement mortar is 1:0.8-1.5; The method for obtaining the cement mortar includes: mixing cement, river sand, water and a water reducing agent to obtain the cement mortar; in the cement mortar, the mass ratio of cement, river sand, water and a water reducing agent is 1:1.5~3.5:0.4~0.7:0.006~0.

01.

2. The method for preparing recycled concrete from construction waste according to claim 1, It is characterized in that The pressure treatment process is carried out in a pressure container, and the direction of applying pressure is from top to bottom.

3. The method for preparing recycled concrete from construction waste according to claim 1, It is characterized in that The density of the glass powder used in the glass powder mixed solution is 2.4-2.7 g / cm 3 The specific surface area of ​​the glass powder used in the glass powder mixed solution is 200-300m 2 / kg.

4. The method for preparing recycled concrete from construction waste according to claim 1, It is characterized in that The recycled coarse aggregate from construction waste has three particle sizes. The first particle size range of the recycled coarse aggregate from construction waste is 19-31.5 mm, the second particle size range of the recycled coarse aggregate from construction waste is 9.5-19 mm, and the third particle size range of the recycled coarse aggregate from construction waste is 4.75-9.5 mm. The mass ratio of the first grade of recycled coarse aggregate from construction waste, the second grade of recycled coarse aggregate from construction waste, and the third grade of recycled coarse aggregate from construction waste is 1:1~5:1~5.

5. The method for preparing recycled concrete from construction waste according to claim 1, It is characterized in that The density of the silica fume is 2.2-2.4 g / cm 3 The specific surface area of ​​the silica fume is 15000~20000m 2 / kg.

6. The method for preparing recycled concrete from construction waste according to claim 1, It is characterized in that The process of mixing the cement mortar into the premix comprises: placing a portion of the premix in a mold, and adding a portion of the cement mortar into the mold under vibration; then, adding another portion of the premix into the mold, and adding another portion of the cement mortar into the mold under vibration.

7. A kind of recycled concrete from construction waste, It is characterized in that The construction waste recycled concrete is prepared by the method for preparing construction waste recycled concrete according to any one of claims 1 to 6.

8. Use of the construction waste recycled concrete as claimed in claim 7 in building construction.