Sulfonated polyetheretherketone resin, water-lubricated bearing composite material and preparation method thereof

By adjusting the sulfonation reaction conditions and end-capping treatment, a sulfonated polyetheretherketone resin with a high sulfonation degree and suitable molecular weight is prepared and combined with carbon fiber particles, which solves the high cost and mechanical problems of the sulfonated polyetheretherketone resin in the existing technology. The problem of insufficient performance is achieved by achieving high performance and low cost of water-lubricated bearing composites.

CN118546353BActive Publication Date: 2024-10-18JIHUA LAB

Patent Information

Application Number
CN202411018649.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-18
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The sulfonated polyether ether ketone resin prepared by the existing condensation polymerization method has high cost and insufficient mechanical properties, making it difficult to commercialize. Moreover, products with high sulfonation degree have poor thermal stability, which affects the compactness and wear resistance of the material.

Method used

Using 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt as the sulfonation unit, by adjusting the reaction conditions and end-capping treatment, a sulfonation degree of 7 to 12% with an average Sulfonated polyetheretherketone resin with a molecular weight of 10,000 to 20,000 is combined with carbon fiber particles and hot-pressed through programmed heating and pressure molding to form a water-lubricated bearing composite material.

Benefits of technology

It reduces the material cost, improves the hydrophilicity, wear resistance and mechanical properties of the composite material, while avoiding the problems of molecular weight reduction and thermal stability, and achieving higher density and tribological properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118546353B_ABST
    Figure CN118546353B_ABST
Patent Text Reader

Abstract

The invention discloses a sulfonated polyetheretherketone resin, a water-lubricated bearing composite material and a preparation method thereof, and relates to the technical field of polymer materials. The sulfonated polyetheretherketone resin uses bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, and potassium carbonate as raw materials, and obtains a sulfonated polyetheretherketone resin with a sulfonation degree of 7 to 12% and an average molecular weight of 10000 to 20000 through a polycondensation reaction. Since 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt is used as a reactant, a sulfonic acid group can be introduced very conveniently, and the molecular weight of the product can be kept unchanged when the sulfonation degree is increased; during preparation, the average molecular weight of the product is between 10000 and 20000 through an end-capping treatment, and the dispersibility and compatibility of the product in the polyetheretherketone resin are good, so it can be used as a hydrophilic auxiliary material of a water-lubricated bearing composite material, so as to achieve a reduction in material cost while improving the hydrophilicity of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a sulfonated polyetheretherketone resin, a water-lubricated bearing composite material and a preparation method thereof. Background Art

[0002] As a water-lubricated bearing material, polyetheretherketone (PEEK) has poor hydrophilicity and is difficult to form a stable water film during low-speed and heavy-load operation, which is prone to severe wear and sharp noise. Therefore, it is of great significance to modify PEEK to improve its tribological properties. In the prior art, the tribological modification of polyetheretherketone (PEEK) is mainly divided into physical blending and chemical modification. Physical blending is to dope some functional fillers into the PEEK matrix to improve the tribological properties of the material by improving the mechanical strength and enhancing the lubrication effect, such as doping with zero-dimensional fillers (Al2O3, SiC, Si3N4, etc.), one-dimensional fillers (carbon fiber, glass fiber, carbon nanotubes, etc.) and two-dimensional fillers (graphene, MoS2, etc.) and other functional fillers. Chemical modification generally reduces the friction and wear of the material by enhancing the surface hydration of the material and promoting the formation of water film under water lubrication conditions. For example, the introduction of negatively charged groups can greatly enhance the surface hydration on the basis of maintaining the mechanical strength of the PEEK matrix, thereby improving the water lubrication performance of the material.

[0003] Sulfonation is one of the most mature and widely used chemical modification methods for PEEK. Common sulfonation methods include post-sulfonation and polycondensation synthesis. The post-sulfonation method is to directly treat the PEEK material with concentrated sulfuric acid or chlorosulfonic acid to graft sulfonic acid groups on the molecular chain. However, due to the excessively intense reaction conditions, not only is the degree of sulfonation difficult to control, but it is also very easy to cause the molecular chain to break, thereby greatly reducing the mechanical strength of the sulfonated material. The polycondensation synthesis method is to use sulfonated monomers to introduce sulfonic acid groups into the molecular chain, and the degree of sulfonation can be controlled by adjusting the reaction time, temperature and feed ratio. For example, the Chinese invention patent with publication number CN117384463A discloses a carbon fiber reinforced sulfonated PEEK composite material and a preparation method thereof. The composite material is composed of a sulfonated PEEK resin matrix and short carbon fiber particles. The sulfonated PEEK resin powder is prepared by polycondensation synthesis, and its sulfonation degree is 1.5-2.5%, with good mechanical strength and low friction coefficient and water contact angle. However, the carbon fiber reinforced sulfonated PEEK composite material prepared by this preparation method has the following defects: first, although it has good hydrophilicity when the sulfonation degree is 1.5-2.5%, the sulfonated polyetheretherketone with this sulfonation degree can usually only be used as a substrate. However, compared with the commercial PEEK substrate or the sulfonated PEEK material prepared by the post-sulfonation method, its cost is too high, which affects its commercial utilization; secondly, when the sulfonation degree is increased by adjusting the raw material ratio, the molecular weight of the sulfonated polyetheretherketone prepared by the preparation method will be reduced, resulting in insufficient mechanical properties; thirdly, the high-sulfonation product obtained by the preparation method has poor thermal stability. When added to the PEEK substrate as a filler, it will partially decompose during the sintering process, resulting in insufficient density of the material and decreased wear resistance.

[0004] It can be seen that the existing technology still needs to be improved and enhanced. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a sulfonated polyetheretherketone resin, a water-lubricated bearing composite material and a preparation method thereof, aiming to solve the defect that the sulfonated polyetheretherketone prepared by the existing condensation synthesis method can only be used as a substrate, resulting in high cost.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A sulfonated polyetheretherketone resin, wherein the sulfonation degree of the sulfonated polyetheretherketone resin is 7-12% and the average molecular weight is 10000-20000;

[0008] The preparation method of the sulfonated polyetheretherketone resin is:

[0009] Step S1. Add bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, potassium carbonate, xylene and dimethyl sulfoxide into a reactor; heat to 150° C. under nitrogen protection and react for 2 hours;

[0010] Step S2. Continue to raise the temperature to 165°C and react at this temperature for 2 to 3 hours, during which water and xylene are separated;

[0011] Step S3. Add a mixture of 4,4'-difluorobenzophenone and DMSO to the reaction solution and continue stirring for 30 min;

[0012] Step S4. Add N,N-dimethylformamide to dilute the reaction solution, and pour the diluted reaction solution into ice water. After cooling and solidification, a strip of solid is formed, and the strip of solid is repeatedly soaked in water;

[0013] Step S5. The strip-shaped solid is crushed into powder, and the powder is washed with ethanol and water at 80° C. for multiple times to obtain a white powder. After the white powder is dried, a sulfonated polyetheretherketone resin is obtained.

[0014] In the sulfonated polyetheretherketone resin, in the step S1, the molar ratio of bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, and potassium carbonate is 10.0: (8.0-9.0): (1.0-2.0): (22.0-26.0).

[0015] In the sulfonated polyetheretherketone resin, in the step S1, the molar ratio of bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, and potassium carbonate is 10.0:8.5:1.5:24.0.

[0016] In the sulfonated polyetheretherketone resin, in step S3, the amount of 4,4'-difluorobenzophenone added is 0.2% of the amount of 4,4'-difluorobenzophenone added in step S1.

[0017] A water-lubricated bearing composite material, wherein the material comprises, by mass percentage, 70-85% of polyetheretherketone resin, 5-15% of sulfonated polyetheretherketone resin, and 5-20% of carbon fiber particles, wherein the sulfonated polyetheretherketone resin is the sulfonated polyetheretherketone resin as described above.

[0018] In the water-lubricated bearing composite material, the average particle size of the carbon fiber particles is 1000-1500 meshes.

[0019] A method for preparing a water-lubricated bearing composite material, wherein the method is used to prepare the water-lubricated bearing composite material as described above, and the method comprises the steps of: taking polyetheretherketone resin, sulfonated polyetheretherketone resin and carbon fiber according to a ratio, and obtaining a mixed powder by ball milling, oscillation dispersion and drying; and hot pressing the mixed powder under vacuum conditions by programmed heating and programmed pressure to obtain a water-lubricated bearing composite material.

[0020] In the preparation method of the water-lubricated bearing composite material, the programmed temperature and programmed pressurization are as follows: the first stage: heating to 300°C at a rate of 10°C / min, during which the pressure is 100 MPa; the second stage: heating to 355-370°C at a rate of 5°C / min, during which the pressure is reduced to 15 MPa; the third stage: keeping warm at 360°C and 15 MPa for 180 min; the fourth stage: cooling to 240-260°C at a rate of 5°C / min, during which the pressure is 15 MPa; the fifth stage: increasing the pressure to 50MPa and keeping warm at 240-260°C for 60 min; the sixth stage: cooling to 50°C at a rate of 10°C / min, during which the pressure is 50MPa.

[0021] Beneficial effects: The first aspect of the present invention provides a sulfonated polyetheretherketone resin, which uses 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt as the sulfonation unit, and can very conveniently introduce sulfonic acid groups. Moreover, when the sulfonation degree is increased to 7-12%, the molecular weight of the product can be kept unchanged. At the same time, during the preparation, the end-capping treatment is performed to make the average molecular weight of the product between 10,000 and 20,000. Since the sulfonated polyetheretherketone with this molecular weight and sulfonation degree has good dispersibility and compatibility in the polyetheretherketone resin, it can be used as a hydrophilic auxiliary material for water-lubricated bearing composite materials, thereby achieving the goal of improving the hydrophilicity of the composite materials while reducing material costs.

[0022] The second aspect of the present invention provides a water-lubricated bearing composite material. The composite material uses a commercially available polyetheretherketone resin as a substrate. By adding a sulfonated polyetheretherketone resin with hydrophilic properties and carbon fiber particles with a reinforcing effect, the sulfonated polyetheretherketone resin has good dispersibility and strong bonding force in the polyetheretherketone resin, so that the density of the composite material can be higher, while improving the wear resistance, tribological properties and mechanical properties of the composite material, while reducing material costs.

[0023] A third aspect of the present invention provides a method for preparing a water-lubricated bearing composite material. By means of programmed heating and programmed pressurization, the composite material can be made denser and have better wear resistance and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1This is a process flow chart for sulfonated polyetheretherketone resin.

[0025] Figure 2 This is a diagram of the temperature and pressure increase program during sintering of the water-lubricated bearing composite material prepared in Example 4. DETAILED DESCRIPTION

[0026] The present invention provides a sulfonated polyetheretherketone resin, a water-lubricated bearing composite material and a preparation method thereof. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] The existing polycondensation synthesis method uses potassium 2,5-dihydroxybenzenesulfonate as the sulfonation unit. When the sulfonation degree is high, the molecular weight is low, resulting in a decrease in the friction coefficient and mechanical strength of the material when the water contact angle is reduced. In particular, when it is used as a hydrophilic auxiliary material and added to a PEEK substrate, although the high sulfonation degree can improve the hydrophilicity of the composite material with PEEK as the substrate, the wear resistance of the composite material is reduced due to the small molecular weight, resulting in the application of the sulfonated polyetheretherketone prepared by the polycondensation synthesis method as a hydrophilic auxiliary material being limited.

[0028] In this regard, the first aspect of the present invention provides a sulfonated polyetheretherketone having a sulfonation degree of 7 to 12% and an average molecular weight of 10,000 to 20,000, which is prepared by the following preparation method (eg Figure 1 shown):

[0029] Step S1. Add bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, potassium carbonate, xylene and dimethyl sulfoxide into a reactor, wherein the molar ratio of bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt and potassium carbonate is 10.0: (8.0-9.0): (1.0-2.0): (22.0-26.0), heat to 150° C. under nitrogen protection, and react for 2 hours;

[0030] Step S2. Continue to raise the temperature to 165°C and react at this temperature for 2 to 3 hours, during which water and xylene are separated;

[0031] Step S3. Add a mixture of 4,4'-difluorobenzophenone and DMSO to the reaction solution and continue stirring for 30 min;

[0032] Step S4. Add N,N-dimethylformamide to dilute the reaction solution, and pour the diluted reaction solution into ice water. After cooling and solidification, a strip of solid is formed, and the strip of solid is repeatedly soaked in water;

[0033] Step S5. crushing the strip-like solid into powder, and washing the powder with ethanol and water at 80° C. for multiple times to remove impurities to obtain a white powder, and drying the white powder to obtain a sulfonated polyetheretherketone resin.

[0034] In this embodiment, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt is used as the sulfonation unit, and by adjusting the ratio of bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, and potassium carbonate, a sulfonated polyetheretherketone with a sulfonation degree of 7 to 12% can be obtained, and its molecular weight does not decrease with the increase of the sulfonation degree, and has better mechanical properties; however, since the sulfonated polyetheretherketone resin contains a sulfonic acid group with a large steric hindrance, when the molecular weight is When the molecular weight of the sulfonated polyetheretherketone is too large or the chain is too long, the fluidity of the sulfonated polyetheretherketone is easily deteriorated, making it difficult to disperse evenly in the polyetheretherketone matrix. Therefore, in the preparation method of the sulfonated polyetheretherketone, 4,4'-difluorobenzophenone is also used for end-capping treatment to make the molecular weight of the product between 10,000 and 20,000, so as to improve its dispersibility in the polyetheretherketone resin, thereby improving the density of the composite material, achieving better wear resistance, tribological properties and mechanical properties while reducing the cost of the composite material.

[0035] As a preferred embodiment, in the step S1, the molar ratio of bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, and potassium carbonate is 10.0:8.5:1.5:24.0. The reactants in this ratio can prepare a sulfonated polyetheretherketone resin with a sulfonation degree of 10%, which has good hydrophilicity, good fluidity at high temperature, and can be well dispersed in the polyetheretherketone matrix, thereby greatly reducing the friction coefficient of the composite material.

[0036] In order to perform the end-capping treatment better, the amount of 4,4'-difluorobenzophenone added needs to be controlled. In a preferred embodiment, in step S3, the amount of 4,4'-difluorobenzophenone added is 0.2% of the amount of 4,4'-difluorobenzophenone added in step S1. The added amount of 4,4'-difluorobenzophenone can better end-cap the polymer, so that the product molecular weight is between 10,000 and 20,000, and the molecular weight distribution range is narrow.

[0037] The second aspect of the present invention provides a water-lubricated bearing composite material, which comprises, by mass percentage, 70-85% of polyetheretherketone resin, 5-15% of sulfonated polyetheretherketone resin, and 5-20% of carbon fiber particles. The sulfonated polyetheretherketone resin is prepared by the method described above, has a sulfonation degree of 7-12%, and an average molecular weight of 10,000-20,000. When a small amount of the sulfonated polyetheretherketone resin is added, the hydrophilicity of the composite material can be well adjusted, and the friction coefficient of the composite material can be greatly reduced.

[0038] In the composite material, polyetheretherketone resin with good mechanical strength is used as the base material, and sulfonated polyetheretherketone resin with medium-strong polar groups and carbon fiber particles that can improve wear resistance are added at the same time, so that the obtained composite material has a lower wear rate and friction coefficient; and because the sulfonated polyetheretherketone resin and polyetheretherketone resin have similar structures and molecular weights can form a graded distribution, the two can be very well combined, which can not only ensure that the mechanical strength of the composite material is not affected, but also enable the sulfonic acid group in the sulfonated polyetheretherketone resin to better exert its hydrophilicity, so that the water lubrication effect of the composite material is better and the friction coefficient is lower. In addition, compared with the prior art using sulfonated polyetheretherketone as the base material, the composite material uses commercial polyetheretherketone as the base material and adds sulfonated polyetheretherketone resin as a hydrophilic auxiliary material, so that the cost can be greatly reduced.

[0039] Specifically, the polyetheretherketone resin can be polyetheretherketone resin of various brands, but preferably polyetheretherketone resin with a brand of 330UPF. This brand of polyetheretherketone resin has good self-lubricating properties, high temperature resistance and good mechanical properties, and can be well combined with sulfonated polyetheretherketone with a molecular weight of 10,000 to 20,000.

[0040] In the water-lubricated bearing composite material, the particle size range of the carbon fiber particles is 1000-1500 meshes. The carbon fiber particles in this particle size range have good dispersibility in the matrix and are not easy to entangle, which can better improve the wear resistance of the composite material and reduce the wear rate.

[0041] The second aspect of the present invention also provides a method for preparing a water-lubricated bearing composite material, which includes the steps of: taking polyetheretherketone resin, sulfonated polyetheretherketone resin and carbon fiber particles according to a ratio, and obtaining a mixed powder by ball milling, oscillation dispersion and drying; and hot pressing the mixed powder under vacuum conditions by programmed heating and programmed pressure to obtain a water-lubricated bearing composite material.

[0042] In the preparation method of the water-lubricated bearing composite material, the polyetheretherketone resin, sulfonated polyetheretherketone resin and carbon fiber particles can be fully and evenly mixed through ball milling and oscillation dispersion, and hot pressing sintering under vacuum conditions by programmed temperature increase or programmed pressure can make the components more densely combined, thereby making the wear resistance and tribological properties of the composite material better.

[0043] In a preferred embodiment, multiple steps are used to perform programmed temperature and programmed pressure, so that the components can have a more dense and uniform structure when they are fused together. Specifically, the programmed temperature and programmed pressure are:

[0044] The first stage: the temperature is raised to 300°C at a rate of 10°C / min, during which the pressure is 100 MPa. In this stage, since the material has not yet melted, the material is compacted by applying pressure.

[0045] The second stage: reduce the heating rate, raise the temperature to 355-370℃ at a rate of 5℃ / min, and reduce the pressure to 15 MPa during the heating period. By reducing the heating rate and pressure, the material is gradually melted. During the melting process, the fluidity of the material increases, so the pressure is reduced to avoid material overflow.

[0046] The third stage: keep the temperature at 355-370℃ and 15 MPa for 180 min to fully melt the materials and form a whole;

[0047] The fourth stage: cooling to 240-260℃ at a rate of 5℃ / min, during which the pressure is 15 MPa, and the material is slowly crystallized by slowly cooling;

[0048] The fifth stage: the pressure is increased to 50 MPa and kept at 240-260°C for 60 min to allow the crystals to precipitate completely, and the precipitated crystals are made dense by applying pressure;

[0049] The sixth stage: cool down to 50℃ at a rate of 10℃ / min, during which the pressure is 50 MPa. The material is cooled by rapid cooling, while maintaining a high pressure to keep the crystal dense.

[0050] In this embodiment, a dense water-lubricated bearing composite material with good mechanical properties and wear resistance can be obtained through a specific temperature increase program and pressure increase program.

[0051] It should be noted that in the third stage, the holding temperature is between 355 and 370°C, which can make the material sintered and plasticized. However, when the temperature is lower than 355°C, the material will be incompletely plasticized, and when the temperature is higher than 370°C, the sulfonated polyetheretherketone resin will be destroyed, resulting in a decrease in the performance of the composite material. Preferably, the holding temperature of the third stage is 360°C.

[0052] In addition, the effect of the insulation temperature in the fifth stage is better when it is 240-260℃, but when it is lower than 240℃, the crystal will precipitate too quickly and the crystallization effect is not good. When the temperature is higher than 260℃, the crystal will precipitate slowly, the time consumption will increase, the pressure will be insufficient, and the density of the material will be insufficient. The optimal insulation temperature for the fifth stage is 250℃.

[0053] To further illustrate a water-lubricated bearing composite material and a preparation method thereof provided by the present invention, the following examples are provided. Example 1

[0054] A sulfonated polyetheretherketone resin has a sulfonation degree of 10% and an average molecular weight of 16,000. The preparation method comprises the following steps: adding bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt and potassium carbonate in a molar ratio of 10.0:8.5:1.5:24.0 into a reactor, using dimethyl sulfoxide and xylene as solvents, heating to 150°C under nitrogen protection, reacting for 2 hours; continuing to heat to 165°C, reacting at the temperature for 2.5 hours, separating water and xylene during the reaction process; adding a mixed solution of 4,4'-difluorobenzophenone (the amount of which is 0.2% of the 4,4'-difluorobenzophenone in the original reactant) and DMSO, and continuing to stir for 30 minutes; min; N,N-dimethylformamide was added to dilute the reaction solution, and the diluted reaction solution was poured into ice water. After cooling and solidification, a strip-like solid was formed, and the strip-like solid was repeatedly soaked in water; the strip-like solid was crushed into powder, and the powder was washed with ethanol and water at 80° C. for 10 times each to obtain a white powder. After the white powder was dried, a sulfonated polyetheretherketone resin was obtained. Example 2

[0055] A sulfonated polyetheretherketone resin having a sulfonation degree of 7% and an average molecular weight of 20,000. The preparation method thereof is substantially the same as that of Example 1, except that the molar ratio of bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, and potassium carbonate is 10.0:9.0:1.0:26.0; and the reaction time at 165° C. is 3 hours. Example 3

[0056] A sulfonated polyetheretherketone resin having a sulfonation degree of 12% and an average molecular weight of 10,000. The preparation method thereof is substantially the same as that of Example 1, except that the molar ratio of bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, and potassium carbonate is 10.0:8.0:2.0:22.0; and the reaction time at 165° C. is 2 hours. Example 4

[0057] A water-lubricated bearing composite material comprises, by mass percentage, 80% of polyetheretherketone resin, 10% of sulfonated polyetheretherketone resin, and 10% of carbon fiber particles. The sulfonated polyetheretherketone resin is the sulfonated polyetheretherketone resin prepared in Example 1.

[0058] The preparation method of the water-lubricated bearing composite material comprises: taking polyetheretherketone resin, sulfonated polyetheretherketone resin and carbon fiber in a mass percentage ratio, and obtaining a mixed powder by ball milling, oscillating dispersion and drying; hot pressing the mixed powder by programmed heating and programmed pressure under vacuum conditions, and the specific steps of programmed heating and programmed pressure (such as Figure 2 The first stage is as follows: the temperature is increased to 300°C at a rate of 10°C / min, during which the pressure is 100 MPa; the second stage is increased to 360°C at a rate of 5°C / min, during which the pressure is reduced to 15 MPa; the third stage is kept at 360°C and 15 MPa for 180 min; the fourth stage is cooled to 250°C at a rate of 5°C / min, during which the pressure is 15 MPa; the fifth stage is to increase the pressure to 50 MPa and keep it at 250°C for 60 min; the sixth stage is to cool to 50°C at a rate of 10°C / min, during which the pressure is 50 MPa; and then naturally cooled to room temperature to obtain a water-lubricated bearing composite material. Example 5

[0059] A water-lubricated bearing composite material, which comprises, by mass percentage, 85% of polyetheretherketone resin, 10% of sulfonated polyetheretherketone resin prepared in Example 1, and 5% of carbon fiber particles. The preparation method of the water-lubricated bearing composite material is also the same as that of Example 4. Example 6

[0060] A water-lubricated bearing composite material, wherein the material comprises, by mass percentage, 70% polyetheretherketone resin, 15% sulfonated polyetheretherketone resin prepared in Example 1, and 15% carbon fiber particles. The preparation method of the water-lubricated bearing composite material is also the same as that of Example 4. Example 7

[0061] A water-lubricated bearing composite material, wherein the material comprises, by mass percentage, 75% polyetheretherketone resin, 5% sulfonated polyetheretherketone resin prepared in Example 1, and 20% carbon fiber particles. The preparation method of the water-lubricated bearing composite material is also the same as that of Example 4. Example 8

[0062] A water-lubricated bearing composite material, whose component composition and preparation method are the same as those of Example 4, except that the sulfonated polyetheretherketone resin is the sulfonated polyetheretherketone resin prepared in Example 2. Example 9

[0063] A water-lubricated bearing composite material, whose component composition and preparation method are the same as those of Example 4, except that the sulfonated polyetheretherketone resin is the sulfonated polyetheretherketone resin prepared in Example 3.

[0064] Comparative Example 1

[0065] A water-lubricated bearing composite material is composed of 60% polyetheretherketone resin, 30% sulfonated polyetheretherketone resin and 10% carbon fiber particles. The preparation method of the water-lubricated bearing composite material is the same as that of Example 4, and the sulfonated polyetheretherketone resin is the sulfonated polyetheretherketone resin prepared in Example 1.

[0066] Comparative Example 2

[0067] A water-lubricated bearing composite material, whose composition and preparation method are the same as those of Example 4, except that: the sulfonated polyetheretherketone resin is prepared by the method of Example 1 in the specification of publication number CN117384463A, and has a sulfonation degree of 2.2% and an average molecular weight of 10,000.

[0068] Comparative Example 3

[0069] A water-lubricated bearing composite material, whose component composition and preparation method are the same as those of Example 4, except that the sulfonated polyetheretherketone resin is prepared by a post-sulfonation method, and its sulfonation degree is 20%.

[0070] Comparative Example 4

[0071] A water-lubricated bearing composite material consists of 90% polyetheretherketone resin and 10% carbon fiber particles, and its preparation method is the same as that of Example 4.

[0072] Comparative Example 5

[0073] A water-lubricated bearing composite material, whose component ratio and preparation method are the same as those of Example 4, except that the preparation method of the sulfonated polyetheretherketone resin is basically the same as that of Example 1, but lacks step S3, and the average molecular weight of the sulfonated polyetheretherketone resin is 25,000 (due to non-end-capping, the average molecular weight obtained is 25,000, but the molecular weight distribution is relatively wide).

[0074] Comparative Example 6

[0075] Sailong SXL.

[0076] Comparative Example 7

[0077] Polyetheretherketone resin with a grade of 330UPF.

[0078] It should be noted that in the above embodiments and comparative examples, the grade of the polyetheretherketone resin is 330UPF; the average particle size of the carbon fiber particles is within 1000-1500 mesh.

[0079] Performance Testing

[0080] The water contact angle of the sulfonated polyetheretherketone resin prepared in Examples 1-3 was measured. The results are shown in Table 1.

[0081] Table 1 Performance test results 1

[0082]

[0083] It can be seen from Table 1 that the sulfonated polyetheretherketone resins prepared in Examples 1-3 all have smaller water contact angles, indicating that they have good hydrophilicity and good water lubrication.

[0084] The performance tests of Examples 4-9 and Comparative Examples 1-7 were performed. The tribological performance test was performed using a UMT rotary friction tester; the hardness was tested using a Shore hardness tester according to GB / T 24112008 / ISO 7619-1:2010 standard; the compressive strength was tested using a universal testing machine according to GB / T 1041-2008 / ISO 604:2002 standard. The specific test results are shown in Table 2.

[0085] Table 2. Performance test results 2

[0086]

[0087] As can be seen from Table 2, the friction coefficient and wear rate of Examples 4-9 are lower than those of Comparative Examples 6 and 7, indicating that adding sulfonated polyetheretherketone resin and carbon fiber particles to polyetheretherketone resin can significantly improve its tribological properties and wear resistance; the hardness of Examples 4-9 is improved to varying degrees compared with Comparative Example 7 or is close to that of Example 7, indicating that the added sulfonated polyetheretherketone resin hardly reduces the hardness of the composite material, while the carbon fiber particles have a very positive effect on the hardness of the composite material; the compressive strength of Examples 4-9 is improved compared with Comparative Example 7 or is close to that of Example 7, indicating that the added sulfonated polyetheretherketone hardly reduces the compressive strength of the composite material, while the carbon fiber particles are beneficial to the improvement of the compressive strength.

[0088] In comparative example 1, when a large amount of sulfonated polyetheretherketone resin is added, its friction coefficient is higher than that of example 4, indicating that the amount of sulfonated polyetheretherketone added should not be too much. This is because the steric hindrance of sulfonated polyetheretherketone is large. When the amount added is too much, the sintering process is easy to affect the entanglement of molecular chains, resulting in performance degradation.

[0089] Although the amount of sulfonated polyetheretherketone resin added in Comparative Example 2 is the same as that in Example 4, the improvement on the material friction coefficient is limited due to the low degree of sulfonation of the sulfonated polyetheretherketone resin.

[0090] In Comparative Example 3, when the degree of sulfonation of the sulfonated polyetheretherketone resin is high, its friction coefficient and wear rate are both high. This is because the molecular chain of the sulfonated polyetheretherketone resin has been destroyed during the sulfonation process, and its compatibility with the polyetheretherketone resin is insufficient, resulting in poor tribological properties and wear resistance, and at the same time causing the hardness and compressive strength of the composite material to decrease.

[0091] Comparative Example 4 has a poor friction coefficient because no sulfonated polyetheretherketone is added.

[0092] The friction coefficient and wear rate of Comparative Example 5 are close to those of Example 4, but its hardness and compressive strength are reduced, indicating that the molecular weight and distribution of the sulfonated polyetheretherketone resin will affect the mechanical properties of the composite material.

[0093] Comparative Example 6 is a commercial water-lubricated bearing material, and its friction coefficient, wear rate and hardness are all lower than those of Examples 4-9, indicating that the tribological properties, wear resistance and hardness of the water-lubricated bearing material prepared by the present invention have exceeded those of existing commercial water-lubricated bearing materials.

[0094] It can be seen that the addition amount, sulfonation degree and molecular weight of sulfonated polyetheretherketone resin will affect the performance of the composite material. By adding sulfonated polyetheretherketone resin with a sulfonation degree of 7-12% and an average molecular weight of 10000-20000, the mechanical properties, tribological properties and wear resistance of the material can be improved while reducing the cost of the composite material.

[0095] It is understandable that those skilled in the art can make equivalent substitutions or changes based on the technical solution and inventive concept of the present invention, and all these changes or substitutions should fall within the protection scope of the claims attached to the present invention.

Claims

1. A sulfonated polyetheretherketone resin, characterized in that The sulfonated polyetheretherketone resin has a sulfonation degree of 7 to 12% and an average molecular weight of 10,000 to 20,000; The preparation method of the sulfonated polyetheretherketone resin is: Step S1. Add bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, potassium carbonate, xylene and dimethyl sulfoxide into a reactor, wherein the molar ratio of bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt and potassium carbonate is 10.0: (8.0-9.0): (1.0-2.0): (22.0-26.0); heat to 150° C. under nitrogen protection and react for 2 hours; Step S2. Continue to raise the temperature to 165°C and react at this temperature for 2 to 3 hours, during which water and xylene are separated; Step S3. Add a mixed solution of 4,4'-difluorobenzophenone and DMSO to the reaction solution, wherein the amount of 4,4'-difluorobenzophenone added is 0.2% of the amount of 4,4'-difluorobenzophenone added in step S1, and continue stirring for 30 min; Step S4. Add N,N-dimethylformamide to dilute the reaction solution, and pour the diluted reaction solution into ice water. After cooling and solidification, a strip of solid is formed, and the strip of solid is repeatedly soaked in water; Step S5. The strip-shaped solid is crushed into powder, and the powder is washed with ethanol and water at 80° C. for multiple times to obtain a white powder. After the white powder is dried, a sulfonated polyetheretherketone resin is obtained.

2. The sulfonated polyetheretherketone resin according to claim 1, characterized in that In the step S1, the molar ratio of bisphenol A, 4,4'-difluorobenzophenone, 4,4'-difluorobenzophenone-3,3'-disulfonic acid disodium salt, and potassium carbonate is 10.0:8.5:1.5:24.

0.

3. A water-lubricated bearing composite material, characterized in that: In terms of mass percentage, the material comprises: 70-85% polyetheretherketone resin, 5-15% sulfonated polyetheretherketone resin, and 5-20% carbon fiber particles. The sulfonated polyetheretherketone resin is the sulfonated polyetheretherketone resin as claimed in any one of claims 1 or 2.

4. The water-lubricated bearing composite material according to claim 3, characterized in that: The average particle size of the carbon fiber particles is 1000-1500 meshes.

5. A method for preparing a water-lubricated bearing composite material, characterized in that: Used to prepare the water-lubricated bearing composite material as claimed in claim 3 or 4, the method comprises the steps of: taking polyetheretherketone resin, sulfonated polyetheretherketone resin and carbon fiber according to a ratio, obtaining a mixed powder by ball milling, oscillation dispersion and drying; and hot pressing the mixed powder under vacuum conditions by programmed heating and programmed pressure to obtain a water-lubricated bearing composite material.

6. The method for preparing a water-lubricated bearing composite material according to claim 5, characterized in that: The programmed temperature and programmed pressurization are as follows: the first stage: heating to 300°C at a rate of 10°C / min, during which the pressure is 100 MPa; the second stage: heating to 355-370°C at a rate of 5°C / min, during which the pressure is reduced to 15 MPa; the third stage: keeping the temperature at 360°C and 15 MPa for 180 min; the fourth stage: cooling to 240-260°C at a rate of 5°C / min, during which the pressure is 15 MPa; The fifth stage: increase the pressure to 50 MPa and keep it at 240-260℃ for 60 min; the sixth stage: cool down to 50℃ at a rate of 10℃ / min, during which the pressure is 50 MPa.

Citation Information

Patent Citations

  • Carbon fiber reinforced sulfonated PEEK composite material and preparation method thereof

    CN117384463A

  • Preparation method of continuous carbon fiber reinforced poly(ether ether ketone) composite material and product

    CN108047470A

  • Polymers and process for their manufacture

    CN109843974A

Cited By

  • Sulfonated polyetheretherketone and preparation method thereof

    CN119264414A