A kind of polar polypropylene composite film and preparation method thereof

By introducing epoxy grafted propylene-ethylene and maleic anhydride-grafted ethylene-vinyl acetate copolymer into polypropylene materials to form ester bonds to improve compatibility, the problem of difficulty in film formation of polypropylene materials was solved and achieved Preparation of efficient and easy-to-process polar polypropylene composite membranes.

CN118546464BActive Publication Date: 2024-10-29佛山(华南)新材料研究院
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411020849.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-29
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

In the existing technology, non-polar polypropylene materials have poor compatibility with polar materials, making it difficult to form films, and existing improved methods have problems such as low production efficiency, complex structures, and high costs.

Method used

Epoxy grafted propylene-ethylene copolymer and maleic anhydride grafted ethylene-vinyl acetate copolymer are used to form ester bonds under the action of catalyst, which reduces the interfacial energy and improves the compatibility of polypropylene with other materials. Twin-screw extruders and thermoplastic processing equipment are used to prepare polar polypropylene composite films.

Benefits of technology

It effectively improves the surface polarity and compatibility of the polypropylene composite membrane, simplifies the production process, reduces the cost, and enables easy processing and batch preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118546464B_ABST
    Figure CN118546464B_ABST
Patent Text Reader

Abstract

The invention discloses a polar polypropylene composite film and a preparation method thereof, and belongs to the technical field of functional plastic films. The invention adds epoxy grafted propylene-ethylene copolymer and maleic anhydride grafted ethylene-vinyl acetate copolymer, and reacts in situ under the catalytic action of a catalyst to form an ester bond so that the two molecular chains are connected to each other, which can effectively improve the compatibility between polypropylene, ethylene-vinyl acetate copolymer and ethylene-acrylic acid type copolymer, promote film formation, and the terpolymer formed after the epoxy grafted propylene-ethylene copolymer and the maleic anhydride grafted ethylene-vinyl acetate copolymer react can fully penetrate into the interior of polypropylene to limit the spherulite growth of polypropylene, strengthen the compatibility of polypropylene and other polar components, can effectively improve the appearance and transparency of the composite film, and can solve the problem of poor compatibility and difficulty in film formation between non-polar polypropylene and polar materials as a whole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional plastic films, in particular to a polar polypropylene composite film and a preparation method thereof. Background Art

[0002] Polypropylene (PP) has good wear resistance, heat resistance, water resistance, aging resistance, chemical solvent resistance and good mechanical properties. It is halogen-free, heavy metal-free, and its waste can be recycled. It is a non-toxic and environmentally friendly material and is suitable for use as a decorative material in the field of home decoration and building materials. Decorative materials require beautiful patterns and textures, which are generally achieved through ink printing. However, PP is a non-polar material, and its inert surface affects its printing performance. Specifically, most of the inks on the market, especially environmentally friendly water-based inks, have poor adhesion to its surface and are difficult to print, which limits the application of PP as a decorative material.

[0003] In order to overcome the above shortcomings, the prior art solves the problem by performing secondary printing on PP, that is, first coating the PP film with a surface treatment agent to change its surface polarity, and then performing water-based printing after curing. This solution has the disadvantages of low production efficiency and VOC pollution generated during the curing process of the surface treatment agent. In order to improve production efficiency and reduce solvent volatilization, it can be solved by multi-layer co-extrusion technology. For example, the Chinese patent number CN201710392581.1 discloses a modified PP decorative film, which is coated with a layer of maleic anhydride grafted PP on the surface of the PP base film by a co-extrusion method to improve its surface polarity. However, the grafting rate of maleic anhydride grafted PP is low (<3 wt%), and the degree of improvement of its surface polarity is limited, and the adhesion to water-based ink is not significantly improved. For example, the Chinese patent number CN201210362145.7 discloses a method of covering polyamide resin on PP to obtain a PP film product with high printing adhesion. However, due to the large difference in surface polarity between PP and polyamide, they cannot be directly co-extruded and composited. An additional adhesive layer needs to be introduced, which makes the product structure complex and the manufacturing cost high. For example, the Chinese patent number CN202410351094.0 discloses a polar PP decorative film and its preparation method, which introduces isocyanate functional groups on the PP molecular chain and then uses isocyanate to initiate the polymerization of caprolactam to obtain a polypropylene-polyamide copolymer, thereby improving the polarity of polypropylene. This method requires at least two steps of graft polymerization reaction, the production process is relatively complicated, and there may be a risk of insufficient monomer reaction.

[0004] Therefore, how to prepare polar polypropylene membrane using a simple and easy method is still an issue that needs further study. Summary of the invention

[0005] Based on this, in order to solve the problem that the existing non-polar material polypropylene and polar materials have poor compatibility and are difficult to form films, the present invention provides a polar polypropylene composite film and a preparation method thereof. The specific technical scheme is as follows:

[0006] A polar polypropylene composite film comprises the following raw materials in parts by weight: 50 to 85 parts of polypropylene, 5 to 15 parts of ethylene-vinyl acetate copolymer, 10 to 25 parts of ethylene-acrylic acid type copolymer, 0.5 to 5 parts of epoxy grafted propylene-ethylene copolymer, 0.5 to 5 parts of maleic anhydride grafted ethylene-vinyl acetate copolymer, 0.05 to 0.2 parts of catalyst and 0.1 to 1 parts of auxiliary agent.

[0007] Furthermore, in the ethylene-vinyl acetate copolymer, the mass percentage of vinyl acetate in the ethylene-vinyl acetate copolymer is 15% to 45%.

[0008] Furthermore, the ethylene-acrylic acid type copolymer is at least one of an ethylene-acrylic acid copolymer and an ethylene-methacrylic acid copolymer.

[0009] Furthermore, the epoxy-grafted propylene-ethylene copolymer refers to a propylene-ethylene copolymer grafted with an epoxy functional group, and in the propylene-ethylene copolymer, the mass percentage content of ethylene in the propylene-ethylene copolymer is 4% to 25%.

[0010] Furthermore, the mass percentage of the epoxy functional group in the epoxy-grafted propylene-ethylene copolymer is 0.3% to 2%.

[0011] Furthermore, the maleic anhydride grafted ethylene-vinyl acetate copolymer refers to an ethylene-vinyl acetate copolymer grafted with a maleic anhydride functional group, and in the ethylene-vinyl acetate copolymer, the mass percentage content of vinyl acetate in the ethylene-vinyl acetate copolymer is 15% to 45%.

[0012] Furthermore, the catalyst is a tertiary amine catalyst.

[0013] Furthermore, the tertiary amine catalyst is at least one of N,N-dimethylbenzylamine, dimethylaminophenol, 2, 4, 6-tris(dimethylaminomethyl)phenol, imidazole, 2-methylimidazole and 2-ethyl-4-methylimidazole.

[0014] In addition, the present application also provides a method for preparing a polar polypropylene composite film, the preparation method comprising the following steps:

[0015] The polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer and additives are uniformly mixed, and added to the main unit of a twin-stage twin-screw extruder for first melt kneading to obtain a mixture A;

[0016] The epoxy grafted propylene-ethylene copolymer, the maleic anhydride grafted ethylene-vinyl acetate copolymer and the catalyst are uniformly mixed, and added to the auxiliary unit of the twin-stage twin-screw extruder for a second melt kneading to obtain a mixture B;

[0017] The mixture B is added to the mixture A through a side feeding port, and after being mixed evenly, the mixture is cooled and pelletized through a pelletizing system to obtain a polar polypropylene composite;

[0018] The polar polypropylene compound is added to a thermoplastic processing device, melt-casted into a film, and then cooled, corona-treated, slit, and rolled to obtain a polar polypropylene composite film.

[0019] Furthermore, the temperature of the second melt kneading is 150° C. to 250° C., and the time is 10 s to 80 s.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention introduces epoxy grafted propylene-ethylene copolymer and maleic anhydride grafted ethylene-vinyl acetate copolymer, and the two react in situ under the catalytic action of a catalyst to form an ester bond so that two molecular chains are connected to each other. The obtained propylene-ethylene-vinyl acetate terpolymer can effectively reduce the interfacial energy between polypropylene, ethylene-vinyl acetate copolymer and ethylene-acrylic acid type copolymer, thereby improving the compatibility between polypropylene, ethylene-vinyl acetate copolymer and ethylene-acrylic acid type copolymer and promoting film formation.

[0022] The epoxy grafted propylene-ethylene copolymer and the maleic anhydride grafted ethylene-vinyl acetate copolymer added in the present invention are both low-crystallinity materials. The terpolymer formed after the two react has lower crystallinity, can fully penetrate into the polypropylene with higher crystallinity, limit the spherulite growth of polypropylene, strengthen the compatibility of polypropylene and other polar components, and can effectively improve the appearance and transparency of the composite film.

[0023] The present invention can reduce the problems of decreased fluidity and deteriorated processing performance caused by cross-linking side reactions by controlling the reaction temperature and time of epoxy grafted propylene-ethylene copolymer and maleic anhydride grafted ethylene-vinyl acetate copolymer. At the same time, after optimizing the process, secondary granulation is avoided, thereby ensuring process stability and production efficiency.

[0024] The present invention can effectively enhance the compatibility of the interface as a whole to improve the surface polarity of the polypropylene composite film, overcome the problem of poor compatibility and difficulty in film formation between non-polar polypropylene and polar materials, and does not require the introduction of a multilayer structure. It can be produced by conventional casting equipment and has the advantages of easy processing and batch preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic structural diagram of the two-stage twin-screw extruder in Example 1 of the present invention.

[0026] Description of Reference Numerals

[0027] 1. Main unit, 2. Main feeding port, 3. Auxiliary unit, 4. Twin screw extruder, 5. Side feeding port. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0030] A polar polypropylene composite film in one embodiment of the present invention comprises the following raw materials in parts by weight: 50 to 85 parts of polypropylene, 5 to 15 parts of ethylene-vinyl acetate copolymer, 10 to 25 parts of ethylene-acrylic acid type copolymer, 0.5 to 5 parts of epoxy grafted propylene-ethylene copolymer, 0.5 to 5 parts of maleic anhydride grafted ethylene-vinyl acetate copolymer, 0.05 to 0.2 parts of catalyst and 0.1 to 1 parts of auxiliary agent.

[0031] In one embodiment, the thickness of the polar polypropylene composite film is 0.05 mm to 0.60 mm, preferably 0.15 mm to 0.50 mm. The present invention limits the thickness of the polar polypropylene composite film. If the thickness of the polar polypropylene composite film is too thin, it will lead to insufficient mechanical properties and easy damage; if the thickness of the polar polypropylene composite film is too thick, it will be used as a decorative film, and the adhesion performance to non-planar panels will be poor, and the cost will increase.

[0032] In one embodiment, the polar polypropylene composite film is a single-layer structure, a double-layer structure, or a multi-layer structure.

[0033] In one embodiment, when the polar polypropylene composite film is a single-layer structure, it is prepared by conventional film-forming processes, including but not limited to blow molding, casting, calendering and coating processes.

[0034] In one embodiment, when the polar polypropylene composite film is a double-layer structure or a multi-layer structure, the surface layer film is the polar polypropylene composite film described in the present invention, and the materials of the remaining layers can be appropriately adjusted according to specific product requirements. The obtained polar multi-layer film capable of water-based printing should also be regarded as within the scope of protection of the present invention, and the specific process will not be repeated here.

[0035] In one embodiment, the polypropylene is at least one of homopolymer polypropylene, block copolymer polypropylene, binary random copolymer polypropylene and ternary random copolymer polypropylene.

[0036] In one embodiment, the melt index of the polypropylene at 230° C. and 2.16 kg is (1-20) g / 10 min, preferably (3-15) g / 10 min.

[0037] In one embodiment, in the ethylene-vinyl acetate copolymer, the mass percentage of vinyl acetate in the ethylene-vinyl acetate copolymer is 15% to 45%, preferably 20% to 38%. Limiting the content of vinyl acetate can make the ethylene-vinyl acetate copolymer have better compatibility in the formulation system.

[0038] In one embodiment, the melt index of the ethylene-vinyl acetate copolymer at 230° C. and 2.16 kg is (1-40) g / 10 min, preferably (3-35) g / 10 min.

[0039] In one embodiment, the ethylene-acrylic acid type copolymer is at least one of an ethylene-acrylic acid copolymer and an ethylene-methacrylic acid copolymer.

[0040] In one embodiment, the epoxy-grafted propylene-ethylene copolymer refers to a propylene-ethylene copolymer grafted with an epoxy functional group, and in the propylene-ethylene copolymer, the mass percentage content of ethylene in the propylene-ethylene copolymer is 4% to 25%.

[0041] In one embodiment, the weight percentage of the epoxy functional group in the epoxy-grafted propylene-ethylene copolymer is 0.3% to 2%.

[0042] In one embodiment, the epoxy functional group is a small molecule compound having an epoxy group and a carbon-carbon double bond.

[0043] In one embodiment, the small molecule compound is at least one of allyl glycidyl ether, glycidyl acrylate and glycidyl methacrylate, preferably glycidyl methacrylate.

[0044] In one embodiment, the epoxy grafted propylene-ethylene copolymer has a melt index of (3-80) g / 10 min, preferably (15-60) g / 10 min at 230° C. and 2.16 kg.

[0045] In one embodiment, the maleic anhydride grafted ethylene-vinyl acetate copolymer refers to an ethylene-vinyl acetate copolymer grafted with a maleic anhydride functional group, and in the ethylene-vinyl acetate copolymer, the mass percentage content of vinyl acetate in the ethylene-vinyl acetate copolymer is 15% to 45%, preferably 20% to 38%.

[0046] In one of the embodiments, in the maleic anhydride grafted ethylene-vinyl acetate copolymer, the mass percentage content of the maleic anhydride group in the maleic anhydride grafted ethylene-vinyl acetate copolymer is 0.3% to 2%.

[0047] In one embodiment, the maleic anhydride grafted ethylene-vinyl acetate copolymer has a melt index of (1-40) g / 10 min, preferably (3-35) g / 10 min at 230° C. and 2.16 kg.

[0048] In one embodiment, the catalyst is a tertiary amine catalyst.

[0049] In one embodiment, the tertiary amine catalyst is at least one of N,N-dimethylbenzylamine, dimethylaminophenol, 2, 4,6-tris(dimethylaminomethyl)phenol, imidazole, 2-methylimidazole and 2-ethyl-4-methylimidazole.

[0050] In one embodiment, the auxiliary agent includes at least one of an antioxidant, a UV absorber, a nucleating agent, and a lubricant.

[0051] In addition, the present application also provides a method for preparing a polar polypropylene composite film, the preparation method comprising the following steps:

[0052] The polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer and additives are uniformly mixed, and added to the main unit of a twin-stage twin-screw extruder for first melt kneading to obtain a mixture A;

[0053] The epoxy grafted propylene-ethylene copolymer, the maleic anhydride grafted ethylene-vinyl acetate copolymer and the catalyst are uniformly mixed, and added to the auxiliary unit of the twin-stage twin-screw extruder for a second melt kneading to obtain a mixture B;

[0054] The mixture B is added to the mixture A through a side feeding port, and after being mixed evenly, the mixture is cooled and pelletized through a pelletizing system to obtain a polar polypropylene composite;

[0055] The polar polypropylene compound is added to a thermoplastic processing device, melt-casted into a film, and then cooled, corona-treated, slit, and rolled to obtain a polar polypropylene composite film.

[0056] In one embodiment, the two-stage twin-screw extruder is obtained by connecting and combining two twin-screw extruders, one of which is a main unit and the other is a sub-unit.

[0057] In one embodiment, the temperature of the first melt kneading is 190°C to 260°C.

[0058] In one embodiment, the temperature of the second melt mixing is 150° C. to 250° C., and the time is 10 s to 80 s.

[0059] In one embodiment, the temperature of the melt casting is 200°C to 250°C.

[0060] In one embodiment, the cooling temperature is 20°C~40°C.

[0061] The above scheme can effectively solve the problem of poor compatibility and difficulty in film formation between non-polar polypropylene and polar materials.

[0062] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0063] In the following examples, PP refers to polypropylene; EVA refers to ethylene-vinyl acetate copolymer; MFR refers to melt index; EAA refers to ethylene-acrylic acid copolymer; and EMAA refers to ethylene-methacrylic acid copolymer.

[0064] Embodiment 1:

[0065] A polar polypropylene composite film includes the following raw materials in parts by weight:

[0066] Table 1: Preparation of raw materials

[0067]

[0068] A method for preparing a polar polypropylene composite film comprises the following steps:

[0069] The polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer and additives are uniformly mixed, added to the main unit of a two-stage twin-screw extruder, and first melt-kneaded at 200° C. for 30 seconds to obtain a mixture A;

[0070] The epoxy grafted propylene-ethylene copolymer, the maleic anhydride grafted ethylene-vinyl acetate copolymer and the catalyst were mixed uniformly, added to the auxiliary unit of the twin-stage twin-screw extruder, and subjected to a second melt kneading at 180° C. for 45 seconds to obtain a mixture B;

[0071] The mixture B is added to the mixture A through a side feeding port, and after being mixed evenly, the mixture is cooled and pelletized through a pelletizing system to obtain a polar polypropylene composite;

[0072] The polar polypropylene composite is added to a thermoplastic processing device, melt-casted at 220° C. to form a film, and then cooled, corona-treated, slit and rolled at 20° C. to obtain a polar polypropylene composite film.

[0073] After testing, the thickness of the polar polypropylene composite film prepared in Example 1 is 0.15 mm.

[0074] Embodiment 2:

[0075] A polar polypropylene composite film includes the following raw materials in parts by weight as shown in Table 2;

[0076] Table 2: Preparation of raw materials

[0077]

[0078] A method for preparing a polar polypropylene composite film comprises the following steps:

[0079] The polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer and additives are uniformly mixed, added to the main unit of a two-stage twin-screw extruder, and first melt-kneaded at 190° C. for 30 seconds to obtain a mixture A;

[0080] The epoxy grafted propylene-ethylene copolymer, the maleic anhydride grafted ethylene-vinyl acetate copolymer and the catalyst were mixed uniformly, added to the auxiliary unit of the twin-stage twin-screw extruder, and subjected to a second melt kneading at 210° C. for 23 seconds to obtain a mixture B;

[0081] The mixture B is added to the mixture A through a side feeding port, and after being mixed evenly, the mixture is cooled and pelletized through a pelletizing system to obtain a polar polypropylene composite;

[0082] The polar polypropylene composite is added to a thermoplastic processing device, melt-casted at 250° C. to form a film, and then cooled, corona-treated, slit and rolled at 25° C. to obtain a polar polypropylene composite film.

[0083] After testing, the thickness of the polar polypropylene composite film prepared in Example 2 is 0.28 mm.

[0084] Embodiment 3:

[0085] A polar polypropylene composite film includes the following raw materials in parts by weight:

[0086] Table 3: Preparation of raw materials

[0087]

[0088] A method for preparing a polar polypropylene composite film comprises the following steps:

[0089] The polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer and additives are uniformly mixed, added to the main unit of a twin-stage twin-screw extruder, and first melt-kneaded at 230° C. for 45 seconds to obtain a mixture A;

[0090] The epoxy grafted propylene-ethylene copolymer, the maleic anhydride grafted ethylene-vinyl acetate copolymer and the catalyst were mixed uniformly, added to the auxiliary unit of the twin-stage twin-screw extruder, and subjected to a second melt kneading at 155° C. for 65 seconds to obtain a mixture B;

[0091] The mixture B is added to the mixture A through a side feeding port, and after being mixed evenly, the mixture is cooled and pelletized through a pelletizing system to obtain a polar polypropylene composite;

[0092] The polar polypropylene composite is added to a thermoplastic processing device, melt-casted at 230° C. to form a film, and then cooled, corona-treated, slit and rolled at 40° C. to obtain a polar polypropylene composite film.

[0093] After testing, the thickness of the polar polypropylene composite film prepared in Example 3 is 0.50 mm.

[0094] Embodiment 4:

[0095] A polar polypropylene composite film includes the following raw materials in parts by weight:

[0096] Table 4: Preparation of raw materials

[0097]

[0098] A method for preparing a polar polypropylene composite film comprises the following steps:

[0099] The polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer and additives were mixed uniformly, added to the main unit of a two-stage twin-screw extruder, and first melt-kneaded at 260° C. for 15 seconds to obtain a mixture A;

[0100] The epoxy grafted propylene-ethylene copolymer, the maleic anhydride grafted ethylene-vinyl acetate copolymer and the catalyst were uniformly mixed, added to the auxiliary unit of the twin-stage twin-screw extruder, and subjected to a second melt kneading at 235° C. for 12 seconds to obtain a mixture B;

[0101] The mixture B is added to the mixture A through a side feeding port, and after being mixed evenly, the mixture is cooled and pelletized through a pelletizing system to obtain a polar polypropylene composite;

[0102] The polar polypropylene composite is added to a thermoplastic processing device, melt-casted at 250° C. to form a film, and then cooled, corona-treated, slit and rolled at 35° C. to obtain a polar polypropylene composite film.

[0103] After testing, the thickness of the polar polypropylene composite film prepared in Example 4 is 0.34 mm.

[0104] Comparative Example 1:

[0105] Compared with Example 1, Comparative Example 1 differs in that, in Comparative Example 1, the epoxy grafted propylene-ethylene copolymer and the maleic anhydride grafted ethylene-vinyl acetate copolymer are replaced with propylene-ethylene copolymer and ethylene-vinyl acetate copolymer, respectively, and the remaining composition and preparation process parameters are the same as those in Example 1, thereby obtaining the polypropylene composite film of Comparative Example 1.

[0106] Comparative Example 2:

[0107] The difference between Comparative Example 2 and Example 1 is that no catalyst (tertiary amine catalyst) is added in Comparative Example 2, and the other steps are the same as those in Example 1, thereby obtaining the polypropylene composite film of Comparative Example 2.

[0108] Comparative Example 3:

[0109] Comparative Example 3 refers to the method disclosed in Chinese Patent No. CN201210362145.7 and is prepared by a co-extrusion casting method. The three-layer structure is a polyamide layer, an adhesive layer and a polypropylene layer, thereby obtaining the polypropylene composite film of Comparative Example 3.

[0110] Comparative Example 4:

[0111] The surface of a commercially available common polypropylene film was polarized by high-voltage corona treatment to make its surface dyne value greater than or equal to 50, thereby obtaining the polypropylene film of this comparative example 4.

[0112] The polar polypropylene composite film samples prepared in Examples 1 to 4 and the polypropylene film comparison samples prepared in Comparative Examples 1 to 4 were evaluated for appearance and printing performance. The specific method is as follows:

[0113] (1) Appearance evaluation is used to judge the appearance of the product. The test method is: visual evaluation, requiring the film surface to be flat and smooth, without visible pores, crystal points and foreign matter.

[0114] (2) Printing performance evaluation is used to evaluate the adhesion of water-based printing ink on the film. The test method is as follows: cut the above sample film and fix the film size to 30cm*30cm. Use commercially available water-based ink to coat the center of the film sample, the coating area is 20cm*20cm, the ink layer thickness is 0.02mm, place it in a 100°C oven for 1 hour, take it out and place it at room temperature for 24 hours before testing. The ink adhesion is tested using the cross-cutting method according to the national standard GB / T 9286. The adhesion level is divided into six levels from 0 to 5 from good to bad. Randomly select no less than 5 areas of the same sample for testing, and record the lowest adhesion level as the test result. The test results are shown in Table 5.

[0115] Table 5: Test results

[0116] Group Appearance Adhesion grade Reprint Adhesion* Example 1 The surface is flat and smooth, without pores or foreign matter 0 0 Example 2 The surface is flat and smooth, without pores or foreign matter 1 0 Example 3 The surface is flat and smooth, without pores or foreign matter 0 0 Example 4 The surface is flat and smooth, without pores or foreign matter 0 0 Comparative Example 1 There are a lot of uneven flow lines on the surface 5 5 Comparative Example 2 The surface has uneven flow lines and crystal points 4 5 Comparative Example 3 Film warping and unevenness 1 1 Comparative Example 4 The surface is flat and smooth, without pores or foreign matter 1 5

[0117] It should be noted that: * Re-printing adhesion is to place the sample at room temperature for six months and then use the same method to print the ink to evaluate the adhesion.

[0118] It can be seen from the test results in Table 5 that, compared with Example 1, Comparative Example 1 does not contain epoxy-grafted propylene-ethylene copolymer and maleic anhydride-grafted ethylene-vinyl acetate, and cannot form propylene-ethylene-vinyl acetate terpolymer, and cannot overcome the poor compatibility of PP, EVA and ethylene-acrylic acid type copolymers, resulting in poor film appearance and insufficient surface polarity.

[0119] Compared with Example 1, Comparative Example 2 lacks a tertiary amine catalyst, and the epoxy grafted propylene-ethylene copolymer and the maleic anhydride grafted ethylene-vinyl acetate react insufficiently, and cannot produce an effective compatibility effect, resulting in poor film appearance and insufficient surface polarity.

[0120] Compared with Example 1, although the composite film has good printing performance, due to the use of a three-layer asymmetric structure, the different crystallinity of polyamide and polypropylene leads to different surface stresses, causing the film to warp and be uneven.

[0121] Comparing Example 4 with Example 1, the surface polarity of the commercially available ordinary polypropylene decorative film can be improved in a short time after corona treatment, thereby improving the surface printing performance, but the surface polarity decreases with time, and the ink adhesion printed six months later is significantly reduced.

[0122] On the whole, Examples 1-4 of the present invention form propylene-ethylene-vinyl acetate terpolymer in situ by epoxy-grafted propylene-ethylene copolymer and maleic anhydride-grafted ethylene-vinyl acetate under the catalysis of tertiary amine, which can effectively reduce the interfacial energy of PP, EVA and ethylene-acrylic acid type copolymer and improve the compatibility of the three. The prepared polar polypropylene composite film has a good appearance; the well-dispersed EVA and ethylene-acrylic acid type copolymer give the film good printing properties; the product can be produced by conventional casting equipment, and has the characteristics of easy processing and batch preparation.

[0123] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0124] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A polar polypropylene composite film, characterized in that: The polar polypropylene composite film comprises the following raw materials in parts by weight: 50 to 85 parts of polypropylene, 5 to 15 parts of ethylene-vinyl acetate copolymer, 10 to 25 parts of ethylene-acrylic acid type copolymer, 0.5 to 5 parts of epoxy grafted propylene-ethylene copolymer, 0.5 to 5 parts of maleic anhydride grafted ethylene-vinyl acetate copolymer, 0.05 to 0.2 parts of catalyst and 0.1 to 1 parts of auxiliary agent; wherein the catalyst is a tertiary amine catalyst.

2. The polar polypropylene composite film according to claim 1, characterized in that: In the ethylene-vinyl acetate copolymer, the mass percentage of vinyl acetate in the ethylene-vinyl acetate copolymer is 15% to 45%.

3. The polar polypropylene composite film according to claim 1, characterized in that: The ethylene-acrylic acid type copolymer is at least one of an ethylene-acrylic acid copolymer and an ethylene-methacrylic acid copolymer.

4. The polar polypropylene composite film according to claim 1, characterized in that: The epoxy-grafted propylene-ethylene copolymer refers to a propylene-ethylene copolymer grafted with an epoxy functional group, and in the propylene-ethylene copolymer, the mass percentage content of ethylene in the propylene-ethylene copolymer is 4% to 25%.

5. The polar polypropylene composite film according to claim 4, characterized in that: The mass percentage of the epoxy functional group in the epoxy-grafted propylene-ethylene copolymer is 0.3% to 2%.

6. The polar polypropylene composite film according to claim 1, characterized in that: The maleic anhydride grafted ethylene-vinyl acetate copolymer refers to an ethylene-vinyl acetate copolymer grafted with a maleic anhydride functional group, and in the ethylene-vinyl acetate copolymer, the mass percentage content of vinyl acetate in the ethylene-vinyl acetate copolymer is 15% to 45%.

7. The polar polypropylene composite film according to claim 1, characterized in that: The tertiary amine catalyst is at least one of N,N-dimethylbenzylamine, dimethylaminophenol, 2, 4, 6-tris(dimethylaminomethyl)phenol, imidazole, 2-methylimidazole and 2-ethyl-4-methylimidazole.

8. A method for preparing a polar polypropylene composite film, characterized in that: The preparation method is used to prepare the polar polypropylene composite film according to any one of claims 1 to 7, and the preparation method comprises the following steps: The polypropylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer and additives are uniformly mixed, and added to the main unit of a twin-stage twin-screw extruder for first melt kneading to obtain a mixture A; The epoxy grafted propylene-ethylene copolymer, the maleic anhydride grafted ethylene-vinyl acetate copolymer and the catalyst are uniformly mixed, and added to the auxiliary unit of the twin-stage twin-screw extruder for a second melt kneading to obtain a mixture B; The mixture B is added to the mixture A through a side feeding port, and after being mixed evenly, it is cooled and pelletized through a pelletizing system to obtain a polar polypropylene composite; The polar polypropylene compound is added to a thermoplastic processing device, melt-casted into a film, and then cooled, corona-treated, slit, and rolled to obtain a polar polypropylene composite film.

9. The preparation method according to claim 8, characterized in that: The temperature of the second melt kneading is 150° C. to 250° C., and the time is 10 s to 80 s.

Citation Information

Patent Citations

  • High-surface-energy double-direction stretching polypropylene thin film and manufacturing method thereof

    CN102873950A

  • Modified PP (polypropylene) decorative film

    CN107142035A

  • A kind of polar polypropylene decorative film and preparation method thereof

    CN117946528B

  • A polarity-modified polypropylene composite material and a preparing method thereof

    CN104086894A

  • Polypropylene composite material as well as preparation method and application thereof

    CN114773727A