An online detection method and online detection device for lithium battery internal short circuit

By detecting the lithium deposition amount and lithium deposition area of ​​the lithium battery, calculating the equivalent height of the lithium dendrite layer, and determining whether the lithium battery has an internal short circuit, the thermal runaway problem caused by the internal short circuit of the lithium battery is solved and the safety of the lithium battery is improved.

CN118549825BActive Publication Date: 2024-10-22CHINA AVIATION LITHIUM BATTERY RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411027198.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-22
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The risk of thermal runaway caused by short circuits in lithium batteries is difficult to effectively detect and avoid with existing technology.

Method used

By detecting the current lithium deposition amount and lithium deposition area of ​​the lithium battery, the equivalent height of the lithium dendrite layer is calculated. If the equivalent height exceeds the threshold, it is determined to be an internal short circuit and measures are taken to avoid thermal runaway.

Benefits of technology

It achieves timely detection of short circuits in lithium batteries, improves the safety of lithium batteries, and reduces the risk of thermal runaway.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118549825B_ABST
    Figure CN118549825B_ABST
Patent Text Reader

Abstract

The present invention discloses an online detection method and an online detection device for internal short circuit of a lithium battery. The method determines the current equivalent height of a lithium dendrite layer generated in the lithium battery according to the current lithium deposition amount and the current lithium deposition area of ​​the lithium battery. When the current equivalent height is not less than a first threshold value, it indicates that the lithium dendrite layer is relatively large at the current height, and the probability that the lithium dendrite layer pierces a diaphragm and causes an internal short circuit is relatively high. Therefore, when the current equivalent height is not less than the first threshold value, it can be determined that an internal short circuit currently occurs in the lithium battery. At this time, timely measures can be taken to avoid thermal runaway of the lithium battery and improve the safety of the lithium battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an online detection method and an online detection device for internal short circuit of a lithium battery. Background Art

[0002] Lithium batteries have been widely used in production and life, so the safety performance of lithium batteries has become one of the key performances in practical applications. When a lithium battery has an internal short circuit, it means that a large amount of heat will be generated inside the lithium battery in a short period of time, causing the temperature inside the lithium battery to rise rapidly. The high temperature will further induce a chain reaction, and eventually cause the lithium battery to have thermal runaway. Therefore, the detection of internal short circuits in lithium batteries and the prevention of thermal runaway in lithium batteries have become urgent issues to be solved. Summary of the invention

[0003] The embodiment of the present invention provides an online detection method and an online detection device for internal short circuit of a lithium battery, which are used to detect whether an internal short circuit occurs in the lithium battery, thereby preventing the lithium battery from experiencing thermal runaway.

[0004] In a first aspect, an embodiment of the present invention provides an online detection method for internal short circuit of a lithium battery, comprising:

[0005] Determine the current equivalent height of the lithium dendrite layer generated in the lithium battery according to the current lithium deposition amount and the current lithium deposition area of ​​the lithium battery;

[0006] When the current equivalent height is not less than the first threshold, it is determined that an internal short circuit currently occurs in the lithium battery.

[0007] In a second aspect, an embodiment of the present invention provides an online detection device for internal short circuit of a lithium battery, comprising:

[0008] A memory for storing program instructions;

[0009] The processor is used to call the program instructions stored in the memory and execute the online detection method for internal short circuit of the lithium battery provided by the embodiment of the present invention according to the obtained program.

[0010] The beneficial effects of the present invention are as follows:

[0011] An online detection method and an online detection device for internal short circuit of a lithium battery provided by an embodiment of the present invention determine the current equivalent height of a lithium dendrite layer generated in the lithium battery according to the current lithium deposition amount and the current lithium deposition area of ​​the lithium battery; when the current equivalent height is not less than a first threshold value, it indicates that the lithium dendrite layer is relatively large at the current height, and the probability that the lithium dendrite layer pierces the diaphragm and causes an internal short circuit is relatively high. Therefore, when the current equivalent height is not less than the first threshold value, it can be determined that an internal short circuit has occurred in the lithium battery. At this time, timely measures can be taken to avoid thermal runaway of the lithium battery and improve the safety of lithium battery use. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 A flow chart of an online detection method for internal short circuit of a lithium battery provided in an embodiment of the present invention;

[0013] Figure 2 A schematic diagram of the height of a lithium dendrite layer provided in an embodiment of the present invention;

[0014] Figure 3 Schematic diagram of different morphologies of lithium dendrite layers provided in embodiments of the present invention;

[0015] Figure 4 A schematic diagram of self-discharge provided in an embodiment of the present invention;

[0016] Figure 5 A curve showing the relationship between the number of charging times and the first voltage difference provided in an embodiment of the present invention;

[0017] Figure 6 The test curves of normal lithium batteries corresponding to different shelf times provided in the embodiment of the present invention;

[0018] Figure 7 The test curves of abnormal lithium batteries corresponding to different storage times provided in the embodiment of the present invention are as follows;

[0019] Figure 8 A flowchart of another online detection method for internal short circuit of a lithium battery provided in an embodiment of the present invention;

[0020] Fig. 9 It is a schematic structural diagram of another online detection device for internal short circuit of a lithium battery provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0021] The following will be combined with the accompanying drawings to describe in detail the specific implementation of an online detection method for short circuit in a lithium battery and its online detection device provided by an embodiment of the present invention. It should be noted that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] The embodiment of the present invention provides an online detection method for short circuit in a lithium battery. Figure 1 As shown, it may include:

[0023] S101, determining a current equivalent height of a lithium dendrite layer generated in the lithium battery according to a current lithium deposition amount and a current lithium deposition area of ​​the lithium battery;

[0024] S102: When the current equivalent height is not less than a first threshold, determine that an internal short circuit currently occurs in the lithium battery.

[0025] In this way, when the current equivalent height is not less than the first threshold, it means that the lithium dendrite layer is relatively large at the current height, and the probability of the lithium dendrite layer piercing the diaphragm and causing an internal short circuit is relatively high. Therefore, when the current equivalent height is not less than the first threshold, it can be determined that the lithium battery currently has an internal short circuit. At this time, timely measures can be taken to avoid thermal runaway of the lithium battery and improve the safety of lithium battery use.

[0026] Furthermore, the technical solution provided by the embodiment of the present invention can realize online detection. During the use of the lithium battery after leaving the factory, it can be detected at any time whether an internal short circuit has occurred in the lithium battery. This can improve the safety of the use of the lithium battery and effectively reduce the risk of thermal runaway during the use of the lithium battery, thereby effectively improving the safety of the use of the lithium battery.

[0027] In actual situations, when lithium deposition occurs in lithium batteries, generally, lithium deposition occurs at the negative electrode and a lithium dendrite layer is generated. The formation of the lithium dendrite layer can include three stages. The first stage can be called the film formation stage, that is, during the charge and discharge process, lithium metal is highly active. The lithium metal at the negative electrode can react with the electrolyte to form an SEI film. The SEI film can isolate the electrolyte and lithium metal, thereby preventing the electrolyte and lithium metal from continuing to react. However, Li + It can be deposited on the negative electrode surface through the SEI film. The second stage can be called the nucleation stage, that is, Li + During the deposition process on the negative electrode surface, Li + It is reduced to lithium atoms, which aggregate to form small crystal nuclei. After that, it continues to deposit unevenly on the surface of the negative electrode to form irregular protrusions. The third stage can be called the growth stage. Under certain kinetic conditions, the growth of lithium deposition in length is significantly better than the growth in the radial direction, thus forming a lithium dendrite layer. The formed lithium dendrite layer increases the risk of breaking through the original SEI film and diaphragm.

[0028] Moreover, when the lithium dendrite layer is formed, a variety of morphologies will be formed, such as but not limited to: coral-shaped lithium dendrite layer, rod-shaped lithium dendrite layer, tree-like lithium dendrite layer, spherical lithium dendrite layer and other irregular morphologies, and the morphology of the lithium dendrite layer may be different under different working conditions. Among them, in actual situations, the morphology of the lithium dendrite layer in a lithium battery under a type of working condition is basically similar, and the morphology of the lithium dendrite layer in a lithium battery at a certain moment may have multiple morphologies, but generally one of the morphologies is dominant, and the proportion of other morphologies is small. At this time, the main morphology can be used as the morphology of the lithium dendrite layer in the lithium battery.

[0029] Due to different morphologies, under the condition of the same amount of lithium deposition, the height of the lithium dendrite layer produced by accumulation on the negative electrode surface will be different, and the height of the lithium dendrite layer has a strong correlation with the probability of triggering an internal short circuit in the lithium battery. Therefore, when determining the equivalent height of the lithium dendrite layer, the morphology of the lithium dendrite layer can be taken into account. By combining the equivalent heights of lithium dendrite layers with different morphologies, it is possible to determine whether an internal short circuit has occurred in the lithium battery, thereby improving the accuracy of the detection results.

[0030] Based on this, in the above S101, according to the current lithium deposition amount and the current lithium deposition area of ​​the lithium battery, the current equivalent height of the lithium dendrite layer generated in the lithium battery is determined, including:

[0031] Process 1: Determine the current reference height of the lithium dendrite layer generated in the lithium battery according to the current lithium deposition amount and the current lithium deposition area of ​​the lithium battery;

[0032] Process 2: Determine the current morphology of the lithium dendrite layer;

[0033] Process 3: According to the correction coefficient corresponding to the current morphology, the current reference height is corrected to obtain the current equivalent height of the lithium dendrite layer.

[0034] For example, the specific implementation process of the above process 1 may include: dividing the current lithium deposition amount by the density of the lithium dendrite layer to obtain the current volume of the lithium dendrite layer; dividing the current volume by the current lithium deposition area to obtain the current reference height of the lithium dendrite layer. It should be understood that the density of the lithium dendrite layer can be obtained based on experiments, and the density of the lithium dendrite layer can be, but is not limited to, 0.535 g / cm 3 .

[0035] In the above process 2, determining the current morphology of the lithium dendrite layer specifically includes: searching for the current morphology corresponding to the current working condition in a pre-configured mapping table of working conditions and morphologies; and using the found current morphology as the current morphology of the lithium dendrite layer. In other words, a mapping table can be pre-configured, and the mapping table can include morphologies under various working conditions, so that the current morphology corresponding to the current working condition can be found by looking up the table, thereby improving the detection effect. It should be understood that in order to distinguish it from the mapping table mentioned later, the mapping table mentioned in this paragraph can be referred to as the first mapping table.

[0036] The specific implementation process of the above process 3 may include: calculating the product of the correction coefficient corresponding to the current morphology and the current reference height, and using the calculated structure as the current equivalent height. Of course, the specific correction method is not limited to the method of calculating the product, and other calculation methods can also be used, such as but not limited to calculating the sum of the correction coefficient corresponding to the current morphology and the current reference height, etc., which can be set according to actual needs and is not limited here.

[0037] Among them, in the above process 3, different morphologies correspond to different correction coefficients. Specifically, when the current morphology is a coral-type lithium dendrite layer, the correction coefficient of the coral-type lithium dendrite layer is 9.7-14.5; when the current morphology is a rod-shaped lithium dendrite layer, the correction coefficient of the rod-shaped lithium dendrite layer is 20.4-25.6; when the current morphology is a tree-like lithium dendrite layer, the correction coefficient of the tree-like lithium dendrite layer is 3.8-5.4; when the current morphology is a spherical lithium dendrite layer, the correction coefficient of the spherical lithium dendrite layer is 0.5-1.5. Of course, the correction coefficient corresponding to each morphology is not limited to the above range, and can also be other ranges set according to actual needs, which is not limited here.

[0038] Taking a lithium battery as an example, the current equivalent height of the lithium dendrite layer in the lithium battery calculated by the above process 1 to process 3 is 6.76μm. Figure 2 The height obtained through actual measurement is shown to be 6.922 μm, with an error rate of 2.4%, indicating that through the above processes 1 to 3, the current equivalent height of the lithium dendrite layer can be estimated more accurately, thereby improving the accuracy of detection.

[0039] The following is an introduction to the process of obtaining the morphology of the lithium dendrite layer in the first mapping table:

[0040] Step 1.1, in a disassembly room with a dew point temperature not less than -30°C, disassemble the lithium battery with 100% SOC and collect the negative electrode;

[0041] Step 1.2: Cut out a sample of a certain size from the gray area (i.e., lithium deposition area) on the surface of the negative electrode;

[0042] Step 1.3: Scan the sample obtained in step 1.2 to obtain a morphological image, such as a coral-like lithium dendrite layer (e.g. Figure 3 As shown in the dashed circle in (a), the rod-shaped lithium dendrite layer (such as Figure 3 As shown in the dashed circle in (b), the dendritic lithium dendrite layer (such as Figure 3 As shown in the dashed circle in (c), the spherical lithium dendrite layer (such as Figure 3 (shown in the dashed circle in (d)).

[0043] Of course, the method for obtaining the morphology of the lithium dendrite layer is not limited to the above steps 1.1 to 1.3, and may also be other methods known to those skilled in the art, which are not limited here.

[0044] Optionally, when determining the current equivalent height, in addition to combining the morphology of the lithium dendrite layer, it is also possible not to combine the morphology of the lithium dendrite layer, such as using the current reference height mentioned in the above content as the current equivalent height, which can reduce the amount of calculation in the detection process and thus improve the efficiency of the detection.

[0045] Optionally, in the above S102, the first threshold value can be determined according to the thickness of the diaphragm in the lithium battery, for example but not limited to the first threshold value being equal to the thickness of the diaphragm, or the first threshold value being the thickness of the diaphragm ± a constant value a, or the first threshold value being the product of the thickness of the diaphragm and a constant value b, etc. It can be set according to actual needs and is not specifically limited here.

[0046] Moreover, in the embodiment of the present invention, when selecting the thickness of the diaphragm, it can be selected according to actual needs, such as but not limited to: when the energy density requirement of the lithium battery is high, the thickness of the selected diaphragm is relatively small, and the first threshold setting is also relatively small; or, when the safety requirement of the lithium battery is high, the thickness of the selected diaphragm is relatively large, and the first threshold setting is also relatively large, which is not limited here.

[0047] When determining the current lithium deposition area, the current lithium deposition area corresponding to the current working condition can be found in the pre-configured working condition and lithium deposition area mapping table, and then the result of the search is used as the current lithium deposition area of ​​the lithium battery, so as to obtain the current lithium deposition area by the table lookup method, thereby improving the detection effect. In addition, the mapping table can be called the second mapping table, and the second mapping table and the first mapping table mentioned in the above content can be different tables, or the second mapping table and the first mapping table mentioned in the above content are combined into a mapping table including working conditions, morphology, lithium deposition area, lithium deposition amount and other information, so that a variety of information can be found through this mapping table.

[0048] The following is an introduction to the process of obtaining the lithium deposition area in the second mapping table:

[0049] Step 2.1, in a disassembly room with a dew point temperature of not less than -30°C, disassemble the lithium battery with 100% SOC, and when the battery cell in the lithium battery is a wound structure, select the negative electrode plates at three different positions;

[0050] Step 2.2, photograph the surface of each negative electrode to obtain three images;

[0051] Step 2.3, for each image, the gray area (i.e., the lithium deposition area) is colorized, and the area of ​​the area with the same color as the colorized color is determined to account for the proportion of the negative electrode in the image. This is repeated three times and the average value is calculated. When the average value is defined as the first value, each image will obtain a first value.

[0052] Step 2.4, taking an average value of the three first values, and using the average value as the lithium deposition area of ​​the lithium battery.

[0053] Of course, the method for determining the lithium deposition area is not limited to the above steps 2.1 to 2.4, and other methods known to those skilled in the art may also be used, which are not limited here.

[0054] When determining the current amount of lithium deposition, a table lookup method can be used, such as looking up a mapping table including other information such as operating conditions, morphology, lithium deposition area, and lithium deposition amount; or, it can be obtained by other methods known to those skilled in the art, such as but not limited to obtaining the current amount of lithium deposition based on the charge and discharge curve, which is not limited here.

[0055] Optionally, in an embodiment of the present invention, the online detection method may further include: before determining the current equivalent height of the lithium dendrite layer, determining the current voltage appreciation, and determining that the current voltage appreciation is not greater than a second threshold value; wherein, when calculating the current difference between the charging cut-off voltage when currently charging to a preset state of charge and the static voltage after the current charging is completed and the preset time is left standing, and the previous difference between the charging cut-off voltage when the last charging to the preset state of charge was completed and the static voltage after the last charging was completed and the preset time is left standing, the current voltage appreciation is determined according to the change value between the current difference and the previous difference.

[0056] That is to say, before executing the above S101, a preliminary judgment can also be made, such as making a judgment based on the current voltage appreciation. If the current voltage appreciation is not greater than the second threshold, it means that the current voltage appreciation is not high or small. At this time, it can be temporarily considered that there is no internal short circuit in the lithium battery, and further judgment is needed, that is, further judgment is needed based on the current equivalent height.

[0057] In this way, two judgments can be made based on the current voltage appreciation and the current equivalent height respectively, and the judgment based on the current voltage appreciation can be regarded as the first judgment, and the judgment based on the current equivalent height can be regarded as the second judgment. The accuracy of the judgment result can be increased through the two judgments to avoid misjudgment.

[0058] Moreover, in the first judgment, if it is determined that the current voltage increase is greater than the second threshold value, it is determined that an internal short circuit has occurred in the lithium battery. At this time, there is no need to perform a second judgment. It is sufficient to determine that an internal short circuit has occurred in the lithium battery based on the result of the first judgment. This can improve the efficiency of online detection.

[0059] Among them, when determining the current voltage appreciation, the specific process may include: calculating the current difference between the charging cut-off voltage when currently charging to a preset state of charge and the static voltage after the current charging is completed and the static voltage is left for a preset time; when calculating the last difference between the charging cut-off voltage when the last charging to the preset state of charge and the static voltage after the last charging is completed and the static voltage is left for a preset time, determine the current voltage appreciation according to the change value between the current difference and the last difference.

[0060] Specifically, determining the current voltage increment according to the change value between the current difference and the previous difference may specifically include: determining the current voltage increment according to the difference between the current difference and the previous difference; or determining the current voltage increment according to the ratio of the current difference to the previous difference. The specific setting may be based on actual needs and is not limited here.

[0061] It should be understood that the preset state of charge can be, but is not limited to, 70% SOC-100% SOC, where SOC is the state of charge. The SOC at the time of charging completion can be any value within this range. If the SOC at the time of current charging completion is 80%, and the SOC at the time of the last charging completion is 100%, since the difference in the charging cut-off voltage corresponding to different SOCs is small, in the embodiment of the present invention, the difference in SOC at each charging completion is not distinguished, as long as it is within the range of the preset state of charge. The preset time of standing still can be, but is not limited to, 20s, 30s, 1min, and other times, which can be set according to actual needs and is not limited here.

[0062] The principles for judging based on the current voltage increase include: the internal short circuit of a lithium battery mainly refers to the self-discharge phenomenon caused by the internal potential difference; during the abuse of lithium batteries, it is easy for a lithium dendrite layer to form at the negative electrode, and the electrolyte decomposes to generate gas. The generated gas causes the distance between the positive electrode and the negative electrode to change, and lithium deposition is more likely to occur in areas such as the edge of the negative electrode, causing the lithium dendrite layer to continue to grow, and eventually penetrate the diaphragm to cause an internal short circuit. In addition, the presence of foreign matter in the lithium battery (such as foreign matter introduced during the manufacturing process) can also cause an internal short circuit in the lithium battery.

[0063] When a lithium battery has a slight internal short circuit, it will show abnormal self-discharge, such as Figure 4 As shown in the figure, the horizontal axis is time, the vertical axis is the voltage of the lithium battery, and the voltage drop caused by self-discharge when fully charged and left alone (that is, the first voltage difference mentioned in the above content) is represented by △V; as the lithium battery is used, the number of charge and discharge times increases, if the charge state when charging is completed is in the preset charge state, a first voltage difference is obtained, so that a relationship curve between the number of charge times and the first voltage difference can be established, such as Figure 5 As shown in the figure, when the internal short circuit begins to be triggered (such as point A), the curve increases suddenly, and when the internal short circuit is stable (such as point B), the curve returns to a flat state. Therefore, it can be judged whether the lithium battery has an internal short circuit based on this characteristic. Figure 5 The slope of the curve between point A and point B is determined by the difference between the ordinates of any two points in the curve.

[0064] In order to make a clear comparison, normal lithium batteries and abnormal lithium batteries are tested separately, such as Figure 6The test curves of normal lithium batteries corresponding to different storage times are shown in the figure. The figure shows the relationship curves between the number of charging times and the first pressure difference when four lithium batteries are stored for 30 seconds and 30 minutes after being fully charged, respectively. Figure 6 (a) Figure 6 (b) Figure 6 (c) and Figure 6 (d) in the figure corresponds to four lithium batteries. It can be seen from the figure that the curve is relatively flat, the first voltage difference is relatively stable, and no mutation occurs. This shows that the curve of a normal lithium battery (that is, a lithium battery without internal short circuit) will not undergo mutation.

[0065] like Figure 7 The test curves of abnormal lithium batteries corresponding to different shelf times are shown. The abnormal lithium battery is a lithium battery with internal short circuit. The figure shows the relationship curves between the number of charging times and the first pressure difference of four lithium batteries when they are fully charged and shelf for 30 seconds and 30 minutes respectively. Figure 7 (a) Figure 7 (b) Figure 7 (c) and Figure 7 (d) in the figure corresponds to four lithium batteries. It can be seen from the figure that each curve has a mutation, as shown in the dotted circle, and tends to be stable after the mutation, which indicates that an internal short circuit occurs inside the lithium battery.

[0066] The online detection method provided by the embodiment of the present invention is introduced below in conjunction with specific embodiments.

[0067] Combination Figure 8 The specific process may include:

[0068] S801, determining whether the current voltage increment is greater than a second threshold; if not, executing S802; if yes, determining that the lithium battery is an abnormal battery and an internal short circuit occurs;

[0069] S802, determining whether lithium plating occurs in the lithium battery; if not, determining that the lithium battery is a normal battery and no internal short circuit occurs; if so, executing S803;

[0070] S803, determining the current lithium deposition amount, lithium deposition area and current morphology of the lithium dendrite layer;

[0071] S804, determining the current equivalent height of the lithium dendrite layer;

[0072] S805. Determine whether the current equivalent height is not less than a first threshold value; if so, determine that the lithium battery is a normal battery and no internal short circuit occurs; if not, determine that the lithium battery is an abnormal battery and an internal short circuit occurs.

[0073] The following is an explanation based on specific test data.

[0074] The positive electrode system of the lithium battery is Ni56, the negative electrode system is graphite, the operating voltage range of the lithium battery is 2.75V-4.35V, and the performance parameters of the lithium battery are shown in Table 1 below, where DCR@50%SOC represents the DC internal resistance of the lithium battery tested at 50%SOC, and the specific test steps when testing the DC internal resistance are shown in Table 2 below.

[0075] Table 1

[0076]

[0077] Table 2

[0078]

[0079] The parameters of each working condition of the lithium battery are shown in Table 3 below, where CC-CV, 1.7C / 1C, 30+1.2C / 1C, 120 means that the charging mechanism is constant current charging + constant voltage charging, firstly, the charging rate is 1.7C, the discharge rate is 1C, and the cycle charging is 30 cycles, and then the charging rate is 1.2C, and the discharge rate is 1C, and the cycle charging is 120 cycles; similarly, the meanings of the steps of No. 8 and No. 9 are similar to those of No. 7, and will not be described in detail here. In addition, CC means constant current charging, CV means constant voltage charging, and the state of charge at the end of the machine refers to the state of charge when charging is completed.

[0080] Table 3

[0081]

[0082] The test data corresponding to lithium batteries under different working conditions are shown in Table 4 below, where taking the lithium battery cell with a wound structure as an example, the large surface refers to the surface with the largest area among the surfaces of the part of the negative electrode sheet that is in a straight shape when wound, and the R angle refers to the corner formed by the negative electrode sheet when it is wound.

[0083] Table 4

[0084]

[0085] From the results shown in Table 4, it can be seen that the equivalent height of the lithium dendrite layer generated in the lithium batteries No. 2 to No. 6, No. 10 and No. 12 is greater than the thickness of the separator, indicating that internal short circuits have occurred in these lithium batteries, while other lithium batteries have not. Therefore, the equivalent height can quickly and accurately detect whether a lithium battery has an internal short circuit, providing a data reference for the safe use of lithium batteries.

[0086] Based on the same inventive concept, an embodiment of the present invention further provides an online detection device for short circuit in a lithium battery. The implementation principle of the online detection device is basically similar to the implementation principle of the aforementioned online detection method. Therefore, the specific implementation method of the online detection device can refer to the embodiment of the aforementioned online detection method, and the repeated parts will not be repeated.

[0087] Specifically, an embodiment of the present invention provides an online detection device for short circuit in a lithium battery, such as Fig. 9 As shown, including:

[0088] Memory 901, used for storing program instructions;

[0089] The processor 902 is used to call the program instructions stored in the memory 901, and execute the online detection method for internal short circuit of a lithium battery provided by the embodiment of the present invention according to the obtained program.

[0090] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. An online detection method for internal short circuit of a lithium battery, characterized in that: include: Determining a current equivalent height of a lithium dendrite layer generated in the lithium battery according to a current lithium deposition amount and a current lithium deposition area of ​​the lithium battery; When the current equivalent height is not less than a first threshold, determining that an internal short circuit currently occurs in the lithium battery; Wherein, determining the current equivalent height of the lithium dendrite layer generated in the lithium battery according to the current lithium deposition amount and the current lithium deposition area of ​​the lithium battery includes: Determining a current reference height of a lithium dendrite layer generated in the lithium battery according to a current lithium deposition amount and a current lithium deposition area of ​​the lithium battery; determining a current morphology of the lithium dendrite layer; The current reference height is corrected according to the correction coefficient corresponding to the current morphology to obtain the current equivalent height of the lithium dendrite layer.

2. The online detection method according to claim 1, characterized in that: When the current morphology is a coral-type lithium dendrite layer, the correction coefficient of the coral-type lithium dendrite layer is 9.7-14.

5.

3. The online detection method according to claim 1, characterized in that: When the current morphology is a rod-shaped lithium dendrite layer, the correction coefficient of the rod-shaped lithium dendrite layer is 20.4-25.

6.

4. The online detection method according to claim 1, characterized in that: When the current morphology is a tree-like lithium dendrite layer, the correction coefficient of the tree-like lithium dendrite layer is 3.8-5.

4.

5. The online detection method according to claim 1, characterized in that: When the current morphology is a quasi-spherical lithium dendrite layer, the correction coefficient of the quasi-spherical lithium dendrite layer is 0.5-1.

5.

6. The online detection method according to claim 1, characterized in that: Determining the current morphology of the lithium dendrite layer specifically includes: In the pre-configured mapping table of working conditions and morphologies, find the current morphology corresponding to the current working condition; The found current morphology is used as the current morphology of the lithium dendrite layer.

7. The online detection method according to claim 1, characterized in that: The first threshold is determined according to the thickness of the separator in the lithium battery.

8. The online detection method according to any one of claims 1 to 7, characterized in that: Also includes: Before determining the current equivalent height of the lithium dendrite layer, determining a current voltage increment, and determining that the current voltage increment is not greater than a second threshold; Among them, when calculating the current difference between the charging cut-off voltage when currently charging to a preset state of charge and the static voltage after the current charging is completed and the preset time is left standing, and the previous difference between the charging cut-off voltage when the last charging to the preset state of charge and the static voltage after the last charging is completed and the preset time is left standing, the current voltage increment is determined according to the change value of the current difference and the previous difference.

9. The online detection method according to claim 8, characterized in that: Also includes: When it is determined that the current voltage increment is greater than the second threshold, it is determined that an internal short circuit occurs in the lithium battery.

10. An online detection device for internal short circuit of a lithium battery, characterized in that: include: A memory for storing program instructions; A processor is used to call the program instructions stored in the memory and execute the online detection method for internal short circuit of a lithium battery as described in any one of claims 1 to 9 according to the obtained program.