A modified high-nickel positive electrode material and its preparation method and application
By using a combination of boron nitride and calcium-containing compounds in high-nickel positive electrode materials and combining the cladding layer, the problem of insufficient pressure resistance and cracking of high-nickel positive electrode materials is solved, and the pressure resistance and structural stability of the material are significantly improved. , improves electrochemical performance.
Patent Information
- Application Number
- CN202411001811.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-25
AI Technical Summary
High-nickel positive electrode materials have insufficient pressure resistance and cracking problems in battery applications. The existing modification research mainly focuses on other auxiliary effects of improved performance, and lacks specialized solutions for strength and cracking.
The combination of the matrix material LiNixMyM’zO2, boron nitride and calcium-containing compounds as interstitial substances, improve the pressure resistance and particle strength of the material through lubricity and adhesion effects, and significantly improve the mechanical properties of the material with the combination of the coating layer.
It significantly improves the pressure resistance and structural stability of high-nickel positive electrode materials, reduces the particle cracking ratio and crack width during the cycle, improves the collapse point and porosity of the material, and enhances the electrochemical performance.
Smart Images

Figure CN118553915B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy technology, and in particular to a modified high-nickel positive electrode material and a preparation method and application thereof. Background Art
[0002] Layered metal oxide cathode materials have formed a relatively systematic and mature system according to the different proportions of elements and components, among which nickel-cobalt-manganese or nickel-cobalt-aluminum material systems can be collectively referred to as ternary materials. When the molar amount of nickel in the layered metal oxide cathode material accounts for more than 80% of the molar amount of the transition metal, it is called a high-nickel material; high-nickel materials have the advantages of high capacity, high specific energy, stable performance and low cost, so they are considered to be attractive choices in fields such as power batteries, and are also cathode materials that are currently widely used and deeply developed. With the further increase in energy density requirements, the application of high-nickel and even ultra-high-nickel materials has become a more clear and urgent need. Inevitably, people need to overcome more technical difficulties to achieve effective applications. For example, the conditions for material synthesis become more stringent, the structural stability deteriorates, the safety decreases, and so on.
[0003] At the same time, new process technologies for battery applications are gradually emerging, such as blade batteries, tab-free technology, etc. People are also gradually putting forward higher requirements in the process of applying positive electrode materials, such as the pursuit of the ultimate available compaction density, the prediction and prevention of failure mechanisms during use, etc. Therefore, for high-nickel positive electrode materials, while solving the technical and cost problems of synthetic materials, people also need to consider the material processing properties, such as the material's hygroscopicity and pressure resistance, etc.; not only that, but also further improve the compatibility of material volume changes and the continuous occurrence of side reactions during the battery cycle, so that these characteristics can be recognized and even accepted.
[0004] In order to achieve high specific energy applications of high nickel cathode powder materials, the powder materials need to undergo a high-pressure compaction process during the production of the pole pieces, and a process of expansion and contraction during the battery cycle, during which particles are continuously embedded and released. Therefore, the improvement of the pressure resistance and material strength of high nickel / ultra-high nickel materials is crucial to the application of high nickel / ultra-high nickel materials and the technical development of high specific energy batteries.
[0005] At present, the performance improvement of high-nickel materials is mainly concentrated in two aspects: improving electrochemical performance and reducing costs through process improvement. On the one hand, developers improve the capacity and stability of materials by means of composition and size adjustment, doping and coating modification, sintering and post-processing optimization, etc. On the other hand, the purpose of performance improvement is achieved by controlling and optimizing the equipment and parameters of process such as mixing, sintering, washing and crushing.
[0006] As the nickel content increases, the pressure resistance and cracking problems of high-nickel materials become more serious due to the increase in the instability of the unit cell structure and the weakening of the synergistic effect of nickel, cobalt and manganese.
[0007] At present, there is still no in-depth research and systematic solution to the problem of insufficient particle strength in the production process of high-nickel positive electrode materials and the development of cracking during the cycle process. The few studies on improving the insufficient strength and cracking of high-nickel positive electrode materials currently focus on strengthening and modifying the grain boundaries of the materials by introducing oxides or fluorides, etc., and characterizing them through direct compaction experiments. There is a problem that the effect cannot be clearly defined, and the improvement effect is mainly a speculative conclusion based on the auxiliary effect of other performance improvements. There is no special strength and cracking modification work, and no proof of effectiveness. Summary of the invention
[0008] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a modified high-nickel positive electrode material, which can effectively improve the pressure resistance of the obtained high-nickel positive electrode material and significantly improve its powder strength and structural stability.
[0009] The present invention also provides a method for preparing the modified high-nickel positive electrode material.
[0010] The present invention also provides application of the modified high-nickel positive electrode material.
[0011] According to an embodiment of the first aspect of the present invention, a modified high-nickel positive electrode material is provided, wherein the modified high-nickel positive electrode material comprises:
[0012] Base material, the chemical formula of the base material is LiNi x M y M' z O2; wherein, 0.80≤x≤0.98, preferably 0.80≤x≤0.95, 0<y≤0.20, preferably 0.02≤y≤0.20, more preferably 0.04≤y≤0.20, 0<z≤0.02, preferably 0.002≤z≤0.02, x+y+z=1; M is at least two of Co, Mn, and Al, preferably a combination of Co and Mn, or a combination of Co and Al, and M' is at least two of Zr, Sr, Ca, Mg, Ba, Y, Nb, Ti, Mo, Sn, Ta, Sb, Bi, and W; the matrix material has pores;
[0013] a filling material, the filling material being present inside the pores; the filling material comprising a sintered substance derived from additive B,
[0014] The additive B comprises boron nitride and a calcium-containing compound.
[0015] In the modified high-nickel positive electrode material provided by the present invention, due to the combination of materials, the structure of the base material itself is stable, and its compressive performance can be improved to a certain extent;
[0016] Furthermore, in additive B, boron nitride is a lubricating substance, which is beneficial to the gap filling of the base material and can also improve the pressure resistance.
[0017] Furthermore, in additive B, the Ca ions in the calcium-containing compound can react with the polyanion (SO4 - The roots, residues of the preparation precursor, etc. adhere to each other, thereby improving the bonding strength between the filling material and the matrix material, and further improving the mechanical strength of the obtained modified high-nickel positive electrode material.
[0018] By utilizing the combination of the boron nitride and the calcium-containing compound, a synergistic effect of lubrication, interstitial filling and adhesion bonding is exerted, and the pressure resistance and particle strength of the material of the present invention are unexpectedly improved.
[0019] On the whole, the internal porosity of the modified high-nickel positive electrode material can be significantly reduced through the limitation of materials and structures, and its mechanical properties such as pressure resistance and crack resistance can be improved, which ultimately significantly reduces the particle cracking ratio and cracking width of the modified high-nickel positive electrode material in long cycles or high-rate electrochemical processes.
[0020] According to some embodiments of the present invention, in the matrix material, 0.80≤x≤0.98, preferably 0.8≤x≤0.96, and more preferably 0.85≤x≤0.95. For example, it can be 0.80, 0.85, 0.90, 0.91, 0.92, 0.93, 0.94 or 0.95.
[0021] According to some embodiments of the present invention, in the matrix material, M is a combination of Co and Mn, wherein the molar ratio of Co to Mn is 1.5 to 2.5:1, for example, 1.6:1, 1.7:1, 1.8:1, 1.9:1 or about 2:1.
[0022] According to some embodiments of the present invention, in the matrix material, y may be 0.01≤y≤0.2, preferably 0.02≤y≤0.2, more preferably 0.04≤y≤0.2, and further preferably 0.045≤y≤0.2. For example, y may be about 0.02, 0.03, 0.04, 0.045, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19 or about 0.20.
[0023] According to some embodiments of the present invention, in the matrix material, z may be 0.002≤z≤0.02, preferably 0.005≤z≤0.018, for example, about 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.015 or about 0.018.
[0024] According to some embodiments of the present invention, in the matrix material, M' includes at least two of Zr, Sr, Y, Nb, Ca, Ti, Sb and W. As long as it can play a certain doping role, there is no particular limitation. Preferably, M' includes at least two of Zr, Sr, Y, Nb, Ti, Sb and W. More specifically, M' includes at least two or at least one of Zr, Sr, Y, Nb and W.
[0025] According to some embodiments of the present invention, in the matrix material, M' is selected from a combination of Zr, Sr, Y and W, or a combination of Zr, Sr, Nb and W. In M', the molar percentage of Zr is 50-60%. For example, it can be 54%, 55% or 56%, etc., or an end value, the same below. The molar percentage of Sr is 10-20%. For example, it can be 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18% or 19%, or an end value, the same below. The molar percentage of Y or Nb is 5-10%. For example, it can be 6%, 7%, 8% or 9%. The molar percentage of W is 15-30%. For example, it can be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or 30%.
[0026] According to some embodiments of the present invention, the matrix material has a divergent structure. Specifically, the matrix material is a secondary particle formed by arranging and stacking primary particles.
[0027] According to some embodiments of the present invention, the calcium-containing compound includes at least one of calcium carbonate, calcium hydroxide, calcium phosphate and calcium pyrophosphate.
[0028] According to some embodiments of the present invention, the concentration of the B element derived from the additive B in the modified high-nickel positive electrode material is 200-5000 ppm, preferably 250-4800 ppm. For example, it can be about 300 ppm, 500 ppm, 700 ppm, 800 ppm, 900 ppm, 1000 ppm, 2000 ppm, 3000 ppm, 4000 ppm, 4500 ppm, 4700 ppm, 4800 ppm or about 4900 ppm.
[0029] According to some embodiments of the present invention, the concentration of the Ca element derived from the additive B in the modified high-nickel positive electrode material is 100-2000 ppm, preferably 150-1800 ppm. For example, it can be about 150 ppm, 200 ppm, 250 ppm, 300 ppm, 350 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1000 ppm, 1500 ppm, 1700 ppm, 1800 ppm or about 1900 ppm.
[0030] According to some embodiments of the present invention, in the additive B, the structure of the boron nitride includes at least one of nanowires and nanosheets. Further, the average equivalent particle size of the boron nitride is 25-35 nm, for example, about 30 nm.
[0031] According to some embodiments of the present invention, the modified high-nickel positive electrode material further has a coating layer, and the coating layer contains a sintered product derived from the additive C.
[0032] According to some embodiments of the present invention, the coating layer is wrapped around the surface of the modified high-nickel positive electrode material.
[0033] The additive C comprises at least one of boric acid, aluminum oxide, aluminum hydroxide, cerium oxide, aluminum fluoride, cerium fluoride, magnesium oxide, and magnesium hydroxide.
[0034] By setting the coating layer and limiting the combination of the additive C, the capacity of the obtained modified high-nickel positive electrode material can be significantly improved.
[0035] According to some embodiments of the present invention, the additive C comprises boric acid and at least one of aluminum oxide, aluminum hydroxide, cerium oxide, aluminum fluoride, cerium fluoride, magnesium oxide, and magnesium hydroxide. Preferably, the additive C comprises boric acid and at least one of cerium fluoride, magnesium oxide, and aluminum fluoride. The mass ratio of the boric acid to other substances in the additive C is 0.025 to 5:1, preferably 0.1 to 4:1. For example, it can be 0.1:1, 0.2:1, 0.5:1, 1:1, 1.5:1, 2:1, 3:1, or 4:1.
[0036] According to some embodiments of the present invention, the mass percentage of the additive C relative to the primary sintered product is 0.3-3%, preferably 0.5-2%. In actual production, the mass of the additive C is close to that of the coating layer, and can also be determined according to the mass percentage of the coating layer in the modified high-nickel positive electrode material.
[0037] According to some embodiments of the present invention, the modified high-nickel cathode material actually has a core-shell structure, wherein:
[0038] The core includes a base material and a filling material disposed inside the pores of the base material;
[0039] The shell is a coating layer covering the surface of the core and includes a sintered product derived from the additive C.
[0040] According to some embodiments of the present invention, the mass percentage of the coating layer to the modified high-nickel positive electrode material is 0.1% to 4%, preferably 0.5% to 3.5%, and more preferably 0.5% to 2.0%. For example, it can be about 0.5%, 1.0%, 1.5%, 2.0%, 3.0% or about 3.5%.
[0041] According to some embodiments of the present invention, the breakdown point P of the modified high nickel cathode material is τ The collapse point is 40~65Mpa. The collapse point refers to the collapse point that occurs when the compaction density is tested under continuously changing pressure and the pressure increases.
[0042] According to some embodiments of the present invention, the breakdown point P of the modified high nickel cathode material is τ The pressure is 45-62 MPa, preferably 49-62 MPa. More specifically, it may be about 46 MPa, 50 MPa, 51 MPa, 52 MPa, 53 MPa, 54 MPa, 55 MPa, 56 MPa, 57 MPa, 58 MPa, 59 MPa, 60 MPa or about 61 MPa.
[0043] The breakdown point of the modified high-nickel positive electrode material provided by the present invention is improved by more than 10% compared with the breakdown point of the existing high-nickel positive electrode material with the same nickel content. In actual production, the improvement can reach 20%, or even 40% or about 80% or more.
[0044] According to some embodiments of the present invention, the porosity of the modified high-nickel cathode material is ≤3%. Unless otherwise specified, in the present invention, pores refer to the percentage of blank area to the total area of the particle in the cross-sectional SEM image. Usually, it is necessary to count the cross-sectional SEM images of multiple modified high-nickel cathode materials.
[0045] According to some embodiments of the present invention, the porosity of the modified high nickel cathode material is 0.1% to 3.0%, preferably 0.1% to 2.0%, more preferably 0.1% to 1.0%, further preferably 0.25% to 0.8%, and further preferably 0.25% to 0.57%. Specifically, it can be about 0.1%, 0.15%, 0.2%, 0.25%, 0.28%, 0.3%, 0.31%, 0.32%, 0.33%, 0.35%, 0.4%, 0.5%, 0.6%, 0.55%, 1%, 1.1%, 1.2%, 1.3% or about 1.5%.
[0046] According to some embodiments of the present invention, the modified high-nickel cathode material has a divergent structure and a composite interstitial structure, that is, the primary particles are divergent from the inside to the outside, with better regularity, improved uniformity of pore distribution between primary particles, generally reduced pores, and filled with specific interstitial materials. After the button battery cycle test, the pole piece observed the particle profile of the modified high-nickel cathode material, and the results showed that compared with the conventional high-nickel cathode material, the degree of cracking was improved, and the number of cracks and the width of cracks were significantly reduced.
[0047] According to an embodiment of the second aspect of the present invention, a method for preparing a modified high-nickel positive electrode material is provided, the preparation method comprising: in an aerobic environment, a M b (OH)2, lithium source, additive A and additive B are mixed and sintered once to obtain a primary sintered product;
[0048] The primary sintered product contains a matrix material and a filling substance, wherein transition metal elements such as Ni, Co, and Mn come from a precursor and an additive A, M' comes from the additive A, and the filling substance comes from the additive B;
[0049] The precursor Ni a M b (OH)2, 0.80≤a≤0.98, specifically 0.80, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97 or 0.98, 0<b≤0.20, preferably 0.08~0.2, more preferably 0.08≤b≤0.15, a+b=1, usually a / b=x / y;
[0050] The additive A is at least two of the oxides, hydroxides or carbonates of Zr, Sr, Ca, Mg, Ba, Y, Nb, Ti, Mo, Sn, Ta, Sb, Bi and W;
[0051] The additive B comprises boron nitride and a calcium-containing compound;
[0052] The primary sintering includes a first insulation platform and a second insulation platform; the temperature of the first insulation platform is 350-650°C; the temperature of the second insulation platform is 680-900°C.
[0053] In the preparation method provided by the present invention, lithium salt, suitable additive A and additive B are added during the primary sintering process, and the temperatures of the specific first and second insulation platforms are limited; thus, additive A plays a doping role, and a small amount of additive A that is not doped into the lattice may exist in the gaps and surface of the modified high-nickel positive electrode material; additive B plays a role in filling the gaps, and a small amount may participate in preliminary doping and surface coating, and a small amount of sintered product of additive B may exist on the surface of the base material, but it does not affect the performance. The second insulation platform is conducive to the reshaping and growth of the crystal, and effectively releases the stress within the crystal.
[0054] Specifically, the temperature of the first insulation platform is limited, so that the lithium source and additive A can achieve the best melting effect and reaction activity, which is more conducive to the lithium salt and the additive A to melt into the gap of the precursor, and further, the additive A entering the gap, the element M' and the Li in the lithium salt penetrate into the primary particles and form part of the lattice, and obtain a sintered material with modified grain morphology; the first insulation platform can also significantly improve the temperature uniformity of the mixture to be sintered, and achieve sufficient micro-environment atmosphere oxygen concentration through sufficient exhaust for a certain period of time. The setting of the second insulation platform mainly takes into account the thermodynamic reaction conditions, and the constant temperature of this platform for a period of time is conducive to the full development of the crystal and the release of surface stress. Form a material with complete crystal form and stable surface structure.
[0055] Lithium salts and precursors also have the function of flux, which can reduce the melting / decomposition temperature of the additive B to a certain extent, decomposing it into smaller particles, so as to fully play the role of filling the gap. At the same time, additive B itself has a certain role as a sintering aid. For example, compared with lithium, the Ca element in the calcium-containing compound can combine with anions such as S during the sintering process to improve the utilization rate of lithium. It can also play the role of reducing the reaction energy barrier and modifying the crystal surface and grain interface at the same time, and can also promote the sintering product of the additive B to "adhere and bond" with the matrix material to enhance the filling effect; when additive B contains boron nitride, the NB bond in boron nitride is extremely strong, the material is very stable, and the melting point is about 3100 degrees, which can be used as a lubricant and interface stabilizing material. In addition, the melting / decomposition temperature of additive B is relatively high, and the high temperature of the second insulation platform can cause it to decompose into a smaller particle size, thereby achieving the role of filling the gap. On the whole, by utilizing the synergistic effect of the two substances in additive B and setting up two insulation platforms, the additive B can fully play the role of filling the gap.
[0056] The preparation method according to the embodiment of the present invention has at least the following beneficial effects: unexpectedly and significantly improving the particle strength of the obtained modified high-nickel positive electrode material, and ultimately achieving an improvement in its voltage resistance performance.
[0057] By testing the pressurization process of powder particles, the collapse point P is obtained. τ The results show that compared with the traditional high nickel positive electrode material, the P τ Greatly improved; not only that, after the modified high-nickel positive electrode material provided by the present invention was cycled under the same conditions, scanning electron microscopy testing showed that the cracking situation was significantly improved.
[0058] According to some embodiments of the present invention, according to the method for preparing the modified high-nickel positive electrode material in the embodiment of the second aspect of the present invention, the modified high-nickel positive electrode material in the embodiment of the first aspect of the present invention can be obtained.
[0059] According to some embodiments of the present invention, the precursor Ni a M b In (OH)2, a has a value in the range of 0.8 to 0.956, for example, about 0.81, 0.85, 0.88, 0.9, 0.91, 0.92, 0.93 or about 0.95.
[0060] According to some embodiments of the present invention, the precursor Ni a M b In (OH)2, the value range of b is 0.02 to 0.2, preferably 0.08 to 0.2. For example, it can be about 0.02, 0.03, 0.04, 0.045, 0.05, 0.06, 0.08, 0.1, 0.11, 0.12, 0.15 or about 0.2.
[0061] According to some embodiments of the present invention, the porosity of the precursor is 2% to 15%, preferably 3 to 10%, more preferably 3 to 5%, and specifically about 3%, 3.2%, 3.8%, 4%, 4.2%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, or about 10%. The porosity of the precursor is greater than the porosity in the modified high-nickel positive electrode material. The reason is that, on the one hand, the precursor will cause a decrease in porosity after the primary sintering, secondary sintering, etc., and another important reason is that the additive B has a filling effect, which ultimately significantly reduces the porosity.
[0062] According to some embodiments of the present invention, the particle size D50 of the precursor is 2-20 μm, preferably 4-15 μm, and more preferably 10 μm, 11 μm, 11.5 μm, 12 μm or about 12.5 μm.
[0063] According to some embodiments of the present invention, the source of the precursor is homemade or commercially available. Whether homemade or commercially available, the crystal growth can be carried out in stages, and the mixed metal salt flow / solid content ratio in different growth stages of the crystal can be regulated to make the crystal grow rapidly in the system, and finally obtain a high-porosity precursor with good sphericity, narrow distribution, and radial from the inside to the outside. The high-porosity precursor is beneficial to the mixing process of the first sintering, which is beneficial to the melt infiltration of the additive A, and is also beneficial to promote the filling of the additive B into the pores of the precursor, constructing a composite pressure-resistant structure of the primary particles and the secondary ball surface, achieving a significant improvement in powder strength and improvement in structural stability, and obtaining a modified high-nickel positive electrode material with excellent compression resistance and crack resistance.
[0064] According to some embodiments of the present invention, the additive A includes at least two of oxides, hydroxides or carbonates of Zr, Sr, Y and W.
[0065] According to some embodiments of the present invention, the additive A includes at least two of oxides, hydroxides or carbonates of Zr, Sr, Nb, and W.
[0066] In actual production, it is a routine operation to determine the type and amount of the additive A according to the chemical formula of the target base material. In other words, the chemical composition formula of the base material can usually be calculated from the raw materials and their addition amounts.
[0067] According to some embodiments of the present invention, the lithium source includes lithium carbonate and / or lithium hydroxide, preferably lithium hydroxide.
[0068] According to some embodiments of the present invention, the molar ratio of the lithium element of the lithium source to the precursor is 1-1.05:1, preferably 1.02-1.04:1. For example, it can be 1:1, 1.01:1, 1.02:1, 1.03:1, 1.04:1 or 1.05:1.
[0069] According to some embodiments of the present invention, the temperature of the first insulation platform is 350-650° C., preferably 400-600° C., and more preferably 450-600° C. For example, it may be about 420° C., 450° C., 480° C., 500° C. or 600° C.
[0070] According to some embodiments of the present invention, the insulation time of the first insulation platform is 2 to 6 hours, for example, it can be about 3 hours, 4 hours or about 5 hours.
[0071] According to some embodiments of the present invention, the temperature of the second insulation platform is 680-850° C., preferably 710-830° C. For example, it may be about 700° C., 710° C., 750° C., 780° C., 800° C. or 830° C.
[0072] According to some embodiments of the present invention, the insulation time of the second insulation platform is 6 to 16 hours, for example, it can be about 10 hours, 12 hours, 14 hours or 15 hours.
[0073] According to some embodiments of the present invention, in the primary sintering, the first heat preservation platform is performed first, and then the second heat preservation platform is performed. After the primary sintering, the temperature is cooled to room temperature, which can be cooled naturally, and crushing can be performed after cooling.
[0074] In actual production, the amount of additive B added in production is appropriately determined based on various specific conditions such as the concentration or porosity in the modified high-nickel positive electrode material.
[0075] According to some embodiments of the present invention, the preparation method further comprises washing the primary sintered product with water, and mixing the washed product with an additive C and then performing secondary sintering;
[0076] The additive C comprises at least one of boric acid, aluminum oxide, aluminum hydroxide, cerium oxide, aluminum fluoride, cerium fluoride, magnesium oxide, and magnesium hydroxide.
[0077] According to some embodiments of the present invention, in the water washing, the mass ratio of the water used to the mass ratio of the primary sintered product is 0.4-2.0:1, preferably 0.5-1.5:1. For example, it can be about 0.5:1, 1:1 or about 1.5:1. In this way, the residual alkali can be effectively removed, and the processing performance of the modified high-nickel positive electrode material can be improved.
[0078] According to some embodiments of the present invention, the water washing temperature is 5-30°C, preferably 10-25°C. For example, it can be about 10°C, 15°C, 20°C or about 25°C, or an end value, as above. In actual production, it can be selected and adjusted as needed; the present invention does not make a strict limitation.
[0079] According to some embodiments of the present invention, the duration of the water washing is 3 to 50 minutes, preferably 5 to 45 minutes. For example, it can be about 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 40 minutes or about 45 minutes. The duration of the water washing is the time taken from when the product obtained by the primary sintering is completely infiltrated by water to when the solid-liquid separation is completed. The method of the solid-liquid separation includes at least one of filtration and centrifugation.
[0080] According to some embodiments of the present invention, the preparation method further comprises drying the obtained water-washed product after the water-washing.
[0081] According to some embodiments of the present invention, the drying temperature is 100-160° C. For example, it may be about 100° C., 110° C., 120° C., 130° C., 140° C., 150° C. or about 160° C., preferably 100-130° C.
[0082] According to some embodiments of the present invention, the constant temperature of the secondary sintering is 200-400° C., preferably 250-350° C. For example, it may be about 250° C., 300° C. or about 350° C.
[0083] According to some embodiments of the present invention, the secondary sintering time is 5 to 10 hours, preferably 6 to 8 hours.
[0084] According to some embodiments of the present invention, the preparation method comprises the following steps:
[0085] S1 in an oxygen environment, the precursor Ni a M b (OH)2, lithium source, additive A and additive B are mixed and sintered once;
[0086] S2. washing the primary sintered product and drying;
[0087] S3. The product obtained in step S2 is mixed with additive C and then subjected to secondary sintering.
[0088] According to an embodiment of the third aspect of the present invention, a lithium secondary battery is provided, wherein the raw materials for preparing the lithium secondary battery include the modified high-nickel positive electrode material, or the modified high-nickel positive electrode material prepared by the preparation method.
[0089] Since the lithium secondary battery adopts all the technical solutions of the modified high-nickel positive electrode material of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, that is, the lithium secondary battery has excellent volume energy density and excellent cycle performance.
[0090] According to some embodiments of the present invention, the lithium secondary battery includes at least one of a button battery, a soft pack battery, a square shell battery and a cylindrical battery.
[0091] According to some embodiments of the present invention, the lithium secondary battery includes at least one of a symmetrical battery, a half cell, and a full cell.
[0092] According to some embodiments of the present invention, the capacity retention rate of the lithium secondary battery after 50 cycles of 1C is ≥ 91%, for example, 91%, 92%, 93%, 94%, 95%, 96% or about 97%.
[0093] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.
[0094] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values 2 and 3.
[0095] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0096] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0097] Figure 1 This is a cross-sectional SEM image of the modified high-nickel positive electrode material obtained in Example 1 of the present invention.
[0098] Figure 2 This is a cross-sectional SEM image of the modified high-nickel positive electrode material obtained in Comparative Example 1 of the present invention.
[0099] Figure 3 It is a diagram of the voltage resistance performance of the modified high-nickel positive electrode material obtained in Example 1 of the present invention and Comparative Example 1.
[0100] Figure 4 This is a cross-sectional SEM image of the modified high-nickel positive electrode material obtained in Example 1 of the present invention after cycling.
[0101] Figure 5 This is a cross-sectional SEM image of the modified high-nickel positive electrode material obtained in Comparative Example 1 of the present invention after cycling.
[0102] Figure 6 1 is a cycle performance diagram of Example 1 of the present invention and Comparative Example 1.
[0103] Figure 7 It is the EDS spectrum of the high nickel positive electrode material obtained in Example 1 (a~b) of the present invention and Comparative Example 1 (c~d).
[0104] Figure 8 This is a surface SEM image of the modified high-nickel positive electrode material obtained in Example 1 of the present invention.
[0105] Fig. 9 This is a surface SEM image of the high-nickel positive electrode material obtained in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0106] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0107] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0108] Example 1
[0109] Step S1
[0110] In an oxygen concentration environment of 90%, according to the chemical formula of the target matrix material, LiNi 0.90 Co 0.05 Mn 0.03 M' 0.02 O2, where M'=Zr 0.012 Sr 0.004 Y 0.001 W 0.003 , calculate the feed amount, and mix the precursor Ni a M b (OH)2, lithium hydroxide monohydrate, additive A and additive B are mixed, then sintered once, and then crushed after cooling to obtain a primary sintered product;
[0111] Wherein, the primary sintering product comprises a matrix material and a filling material;
[0112] The chemical formula of the above matrix material is LiNi 0.90 Co 0.05 Mn 0.03 M' 0.02 In O2, transition metal elements Ni, Co, and Mn come from the precursor, doping element M' comes from additive A, and interstitial material comes from additive B;
[0113] Precursor Ni a M b The chemical formula of (OH)2 is Ni 0.918 Co 0.051 Mn 0.031(OH)2; D50 particle size is about 11.5μm; porosity is about 3.8%.
[0114] The molar ratio of lithium element in the lithium salt to the precursor is 1.03:1;
[0115] Additive A is a mixture of zirconium oxide, strontium oxide, yttrium oxide, and tungsten trioxide, and the mixing ratio is calculated according to the composition of M';
[0116] Additive B is a mixture of boron nitride (flake-shaped, with an average equivalent particle size of about 30 nm) and calcium hydroxide, and the amount of addition is calculated according to the concentrations of B element and Ca element in the product obtained in this step shown in Table 1;
[0117] The primary sintering includes the first insulation platform and the second insulation platform in sequence; the temperature is increased to the first insulation platform at 2°C per minute and then insulation is carried out, and then the temperature is increased to the second insulation platform at 2°C per minute and then insulation is carried out again, wherein the constant temperature of the first insulation platform is 450°C; the duration is 3 hours, and the constant temperature of the second insulation platform is 750°C, and the duration is 12 hours.
[0118] Step S2
[0119] The primary sintered product obtained in step S1 is washed with pure water, wherein the mass ratio of pure water to the primary sintered product is 1:1, the washing temperature is 15° C., and the washing time is 20 min; and then dried at 120° C.
[0120] Step S3
[0121] The product obtained in step S2 was mixed with additive C and subjected to secondary sintering at 310° C. for 7 h. The product was sieved through a 325-mesh sieve to obtain the modified high-nickel positive electrode material of the present invention. The porosity is shown in Table 2.
[0122] As shown in Table 1, the additive C includes boric acid and cerium fluoride, the mass ratio of boric acid to cerium fluoride is 3:1, and the addition amount is 1.5% by mass relative to the primary sintered product.
[0123] Example 2
[0124] Step S1
[0125] In an oxygen concentration environment of 90%, according to the chemical formula of the target matrix material, LiNi 0.8 Co 0.12 Mn 0.078 M' 0.002 O2, where M'=Zr 0.001 Sr 0.0002 Y 0.0002 W 0.0006 , calculate the feed amount, and mix the precursor Ni s Mb (OH)2, lithium hydroxide monohydrate, additive A and additive B are mixed, then sintered once, and then crushed after cooling to obtain a primary sintered product;
[0126] Wherein, the primary sintering product comprises a matrix material and a filling material;
[0127] The chemical formula of the above matrix material is LiNi 0.8 Co 0.12 Mn 0.078 M' 0.002 In O2, transition metal elements Ni, Co, and Mn come from the precursor, doping element M' comes from additive A, and interstitial material comes from additive B;
[0128] Precursor Ni a M b The chemical formula of (OH)2 is Ni 0.802 Co 0.12 Mn 0.078 (OH)2; D50 particle size is about 12.5μm; porosity is about 3.2%.
[0129] The molar ratio of lithium element in the lithium salt to the precursor is 1.04:1;
[0130] Additive A is a mixture of zirconium oxide, strontium oxide, yttrium oxide and tungsten trioxide, and the mixing ratio is calculated according to the composition of M';
[0131] Additive B is a mixture of boron nitride (flake-shaped, with an average equivalent particle size of about 30 nm) and calcium hydroxide, and the amount of addition is calculated according to the concentrations of B element and Ca element in the product obtained in this step shown in Table 1;
[0132] The primary sintering includes the first insulation platform and the second insulation platform in sequence; the temperature is increased to the first insulation platform at 2°C per minute and then insulation is carried out, and then the temperature is increased to the second insulation platform at 2°C per minute and then insulation is carried out again, wherein the constant temperature of the first insulation platform is 600°C; the duration is 2h, and the constant temperature of the second insulation platform is 830°C, and the duration is 6h.
[0133] Step S2
[0134] The primary sintered product obtained in step S1 is washed with pure water, wherein the mass ratio of pure water to the primary sintered product is 1.5:1, the washing temperature is 25° C., and the washing time is 15 min; and then dried at 130° C.
[0135] Step S3
[0136] The product obtained in step S2 is mixed with additive C, and then subjected to secondary sintering at 350° C. for 6 h. The mixture is sieved through a 325-mesh sieve to obtain the modified high-nickel positive electrode material of the present invention;
[0137] As shown in Table 1, the additive C includes boric acid and cerium fluoride, the mass ratio of boric acid to cerium fluoride is 0.5:1, and the addition amount is 0.5% by mass relative to the primary sintered product.
[0138] Example 3
[0139] Step S1
[0140] In an oxygen concentration environment of 90%, according to the chemical formula of the target matrix material, LiNi 0.948 Co 0.029 Mn 0.015 M' 0.008 O2, where M'=Zr 0.0044 Sr 0.00116 Nb 0.00064 W 0.0018 , calculate the feed amount, and mix the precursor Ni a M b (OH)2, lithium hydroxide monohydrate, additive A and additive B are mixed, then sintered once, and then crushed after cooling to obtain a primary sintered product;
[0141] Wherein, the primary sintering product comprises a matrix material and a filling material;
[0142] The chemical formula of the above matrix material is LiNi 0.948 Co 0.029 Mn 0.015 M' 0.008 In O2, transition metal elements Ni, Co, and Mn come from the precursor, doping element M' comes from additive A, and interstitial material comes from additive B;
[0143] Precursor Ni a M b The chemical formula of (OH)2 is Ni 0.956 Co 0.029 Mn 0.015 (OH)2; D50 particle size is about 11.0μm; porosity is about 4.2%.
[0144] The molar ratio of lithium element in the lithium salt to the precursor is 1.02:1;
[0145] Additive A is a mixture of zirconium oxide, strontium oxide, niobium oxide and tungsten trioxide, and the mixing ratio is calculated according to the composition of M';
[0146] Additive B is a mixture of boron nitride (flake-shaped, with an average equivalent particle size of about 30 nm) and calcium hydroxide, and the amount of addition is calculated according to the concentrations of B element and Ca element in the product obtained in this step shown in Table 1;
[0147] The primary sintering includes a first insulation platform and a second insulation platform in sequence; the temperature is increased to the first insulation platform at 2°C per minute and then insulation is carried out, and then the temperature is increased to the second insulation platform at 2°C per minute and then insulation is carried out again, wherein the constant temperature of the first insulation platform is 480°C; the duration is 6 hours, and the constant temperature of the second insulation platform is 710°C, and the duration is 15 hours.
[0148] Step S2
[0149] The primary sintered product obtained in step S1 is washed with pure water, wherein the mass ratio of pure water to the primary sintered product is 0.5:1, the washing temperature is 10° C., and the washing time is 30 min; and then dried at 100° C.
[0150] Step S3
[0151] The product obtained in step S2 is mixed with additive C, and then subjected to secondary sintering at 250° C. for 8 h. The mixture is sieved through a 325-mesh sieve to obtain the modified high-nickel positive electrode material of the present invention;
[0152] As shown in Table 1, the additive C includes boric acid and cerium fluoride, the mass ratio of boric acid to cerium fluoride is 4:1, and the addition amount is 2.0% by mass relative to the primary sintered product.
[0153] Example 4
[0154] On the basis of Example 1, in step S3, cerium fluoride in additive C is replaced by magnesium oxide. Other than that, the preparation raw materials, preparation method, parameter conditions, etc. are basically the same as those in Example 1.
[0155] Example 5
[0156] On the basis of Example 1, in step S3, cerium fluoride in additive C is replaced by aluminum fluoride. Other than that, the preparation raw materials, preparation method, parameter conditions, etc. are basically the same as those in Example 1.
[0157] Example 6
[0158] On the basis of Example 1, in step S1, the calcium hydroxide Ca(OH)2 in additive B is replaced by calcium pyrophosphate Ca2O7P2. Apart from this, the preparation raw materials, preparation method and parameter conditions are basically the same as those in Example 1.
[0159] Example 7
[0160] On the basis of Example 1, after drying in step S2, the material is directly crushed and passed through a 325-mesh sieve to obtain the modified high-nickel positive electrode material of the present invention, that is, there is no mixing and secondary sintering in step S3. Apart from this, the preparation raw materials, preparation method, parameter conditions, etc. are basically the same as those in Example 1.
[0161] As shown below, some parameters of Examples 1 to 7 are given in Table 1.
[0162] Table 1 Some parameters of Examples 1 to 7
[0163]
[0164] Comparative Example 1
[0165] This example prepares a modified high-nickel positive electrode material, which differs from Example 1 in that:
[0166] In step S1, additive B is not added.
[0167] Comparative Example 2
[0168] This example prepares a modified high-nickel positive electrode material, which differs from Example 1 in that:
[0169] In step S1 , the additive B does not contain boron nitride.
[0170] Comparative Example 3
[0171] This example prepares a modified high-nickel positive electrode material, which differs from Example 1 in that:
[0172] In step S1, the additive B does not contain calcium hydroxide.
[0173] Comparative Example 4
[0174] This example prepares a modified high-nickel positive electrode material, which differs from Example 1 in that:
[0175] In step S1, the first heat preservation platform is not set, that is, the temperature is directly raised from room temperature to the constant temperature of 780° C. of the second heat preservation platform, and the temperature is kept for 12 hours.
[0176] Comparative Example 5
[0177] This example prepares a modified high-nickel positive electrode material, which differs from Example 1 in that:
[0178] In step S1, the temperature of the first insulation platform is set to 700°C.
[0179] Comparative Example 6
[0180] This example prepares a modified high-nickel positive electrode material, which differs from Example 1 in that:
[0181] In step S1, the insulation temperature of the first insulation platform is 300°C.
[0182] Comparative Example 7
[0183] This example prepares a modified high-nickel positive electrode material, which differs from Example 1 in that:
[0184] In step S1, additive A is not added.
[0185] Application Examples
[0186] This example provides a lithium secondary battery, the details of which are as follows.
[0187] The positive electrode material, conductive agent SuperP, binder polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP) prepared above were mixed and stirred in a mass ratio of 90:5:5 to prepare a positive electrode slurry (solid content of about 40%), which was coated on the current collector aluminum foil, dried at 105°C, and then rolled at room temperature to a surface density of 2.8-3.3 g / cm 3 , and then punched and cut into φ14mm discs to make positive electrode sheets; wherein the positive electrode material comes from the embodiment or the comparative example.
[0188] The button cell was assembled in the glove box. The assembly was carried out in the order of "negative electrode shell - nickel foam - lithium sheet (φ18mm) - 8 drops of electrolyte - diaphragm (φ22mm, thickness 16μm) - 8 drops of electrolyte - positive electrode sheet - positive electrode shell", wherein the electrolyte was composed of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) (EC:EMC:DMC volume ratio = 1:1:1), containing 1.0M LiPF6; the size of the battery shell (positive electrode shell and negative electrode shell) was 24mm. The assembled button cell was placed in the mold groove of the hydraulic sealing machine (purchased from Shenzhen Kejing Zhida Technology Co., Ltd.), locked, and the pressure was >450kg / cm 2 , then unlock it and take out the sealed button battery, which is the lithium secondary battery obtained in this example.
[0189] Test Case
[0190] This example tests the cross-sectional morphology of the modified high-nickel positive electrode materials obtained in the examples and comparative examples. The testing method is to perform SEM testing after cutting. The cross-sectional SEM images of Example 1 and Comparative Example 1 are shown in FIG. Figure 1~2 As shown in the figure, the test results show that the cross-sectional morphology of the modified high-nickel positive electrode materials obtained in the examples of the present invention is similar, both of which have radially arranged primary particles, and the primary particles aggregate to form a secondary spherical structure; the gaps between the primary particles are filled with pore fillers derived from additive B. From the appearance, the cross-sectional morphology of the modified high-nickel positive electrode material obtained in Example 1 is more compact. In contrast, the cross-sectional morphology of the comparative example 1 lacks pore fillers, and there are significantly more pores in the cross-section.
[0191] This example also tests the cross-sectional EDS spectra of the positive electrode materials obtained in Example 1 and Comparative Example 1. Figure 7As shown, (a) is a cross-sectional SEM image of the positive electrode material obtained in Example 1, and (b) is a B element distribution mapping diagram of the cross-sectional positive electrode material obtained in Example 1. The white dots represent the B element, which is evenly distributed in the inner and outer layers. (c) is a cross-sectional SEM image of the positive electrode material obtained in Comparative Example 1, and (d) is a B element distribution mapping diagram of the cross-sectional positive electrode material obtained in Comparative Example 1. The white dots represent the B element, which is faintly visible in the outer layer. According to the cross-sectional EDS energy spectrum of Comparative Example 1, it can be seen that the boron element from additive C is mainly enriched on the surface of the material; according to the cross-sectional EDS energy spectrum of Example 1, it can be seen that the modified high-nickel positive electrode material of Example 1, including the core, also has a relatively rich boron element inside. Therefore, it can be seen that the sintered material containing the boron element from additive B does have a filling effect.
[0192] This example also tests the pressure resistance of the modified high-nickel positive electrode materials obtained in the examples and comparative examples. The specific test method is: gradually pressurize the positive electrode materials obtained in the examples and comparative examples to obtain the mutation point of dρ / dP, and the pressure applied at the corresponding position is the collapse point; wherein ρ is the density, and P is the pressure applied during the process; the test results are shown in FIG. Figure 3 As shown in Table 2; Figure 3 The position indicated by the arrow in the middle is the collapse point.
[0193] The cross-sectional SEM images and surface SEM images of Example 1 and Comparative Example 1 are shown as follows: Figure 1~2 , Figures 8 and 9 As shown, it can be reflected that the porosity of Example 1 is less than that of Comparative Example 1. The porosity statistics are shown in Table 2.
[0194] Table 2 Performance of high nickel positive electrode materials obtained in Examples and Comparative Examples
[0195]
[0196] The above results show that compared with Comparative Example 1, the Pτ of Example 1 is increased by more than 10%, and the increase can reach about 60%, and in some cases can even reach more than about 80%. This indicates that the present invention significantly improves the processing pressure resistance of the obtained modified high-nickel positive electrode material by allowing the additive B to infiltrate into the pores between the primary particles.
[0197] This example also tests the cycle performance of the lithium secondary battery obtained in the application example. After the cycle is completed, the battery is disassembled and the cross-sectional structure of the high-nickel positive electrode material after the cycle is completed is photographed with SEM. The test method for the cycle performance is as follows.
[0198] At 25°C, use the Blue Electric test cabinet to test the charge and discharge cycle characteristics of the button battery, setting 1C=200mAh / g. Charge and discharge at a charge and discharge rate of 1C in the voltage range of 2.8V~4.25V. Specifically, charge to 4.25V at a constant current of 1C, then charge to a cut-off current of 0.02C at a constant voltage of 4.25V, leave for 5 minutes, discharge to 2.8V at 1C, leave for 5 minutes, and record the charge and discharge capacity after the first cycle. Cycle in sequence as above, charge / discharge 50 times, and record the charge and discharge capacity after the 50th cycle.
[0199] Cycle capacity retention rate (%) = (50th cycle discharge capacity / 1st cycle discharge capacity) × 100%.
[0200] The test results of the cycle performance are shown in Table 3.
[0201] Table 3 Cyclic performance results of high nickel cathode materials obtained in Examples and Comparative Examples
[0202]
[0203] The cycle process of Example 1 and Comparative Example 1 shows that compared with Example 1, Comparative Example 1 decays faster in the first 50 weeks and has a faster overall decay rate. The specific results are as follows: Figure 6 shown.
[0204] Comparison of cross-sectional morphology of high nickel positive electrode materials after cycling in Example 1 and Comparative Example 1 Figures 4 and 5 As shown. According to the cross-sectional test results of the high-nickel positive electrode material after cycling, the number and width of cracks in the modified high-nickel positive electrode material obtained in the embodiment are significantly reduced. This shows that the modified high-nickel positive electrode material provided by the present invention can significantly improve the cycle structure stability and ultimately significantly improve the cycle performance.
[0205] In summary, the present invention unexpectedly obtains a modified high-nickel positive electrode material with excellent pressure resistance and cycle stability by giving play to the synergistic effect of additives A, additive B, etc., preferably by giving play to the synergistic effect of additives A, additive B, additive C, etc., and precisely controlling the process parameter conditions in each step such as the sintering system and sintering temperature in step S1. When a lithium secondary battery is prepared using the modified high-nickel positive electrode material of the present invention, the cyclability of the lithium secondary battery can be significantly improved. Furthermore, lithium secondary batteries are expected to be widely used in the fields of power batteries, energy storage technology, and 3C small household appliances technology.
[0206] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A modified high-nickel positive electrode material, characterized in that: The modified high-nickel positive electrode material comprises: Base material, the chemical formula of the base material is LiNi x M y M' z O2, wherein 0.80≤x≤0.98, 0<y≤0.20, 0<z≤0.02, x+y+z=1; M is at least two of Co, Mn, and Al, and M' is at least two of Zr, Sr, Ca, Mg, Ba, Y, Nb, Ti, Mo, Sn, Ta, Sb, Bi, and W; and the matrix material has pores; a filling material, the filling material being present inside the pores, the filling material comprising a sintered material derived from the additive B, The additive B comprises boron nitride and a calcium-containing compound.
2. The modified high-nickel positive electrode material according to claim 1, characterized in that: The modified high-nickel positive electrode material further has a coating layer, The coating layer comprises a sintered product derived from the additive C, The additive C comprises at least one of boric acid, aluminum oxide, aluminum hydroxide, cerium oxide, aluminum fluoride, cerium fluoride, magnesium oxide, and magnesium hydroxide.
3. The modified high-nickel positive electrode material according to claim 2, characterized in that: The additive C comprises boric acid and at least one of aluminum oxide, aluminum hydroxide, cerium oxide, aluminum fluoride, cerium fluoride, magnesium oxide, and magnesium hydroxide.
4. The modified high-nickel positive electrode material according to any one of claims 1 to 3, characterized in that: The matrix material has a divergent structure.
5. The modified high-nickel positive electrode material according to any one of claims 1 to 3, characterized in that: The collapse point P of the modified high nickel positive electrode material τ 40~65Mpa.
6. The modified high-nickel positive electrode material according to any one of claims 1 to 3, characterized in that: The porosity inside the modified high-nickel positive electrode material is ≤3%.
7. The modified high-nickel positive electrode material according to any one of claims 1 to 3, characterized in that: The concentration of the B element derived from the additive B in the modified high-nickel positive electrode material is 200-5000 ppm.
8. The modified high-nickel positive electrode material according to any one of claims 1 to 3, characterized in that: The concentration of the Ca element derived from the additive B in the modified high-nickel positive electrode material is 100-2000 ppm.
9. A method for preparing a modified high-nickel positive electrode material according to any one of claims 1 to 8, characterized in that: The preparation method comprises: in an oxygen environment, a M b (OH)2, lithium source, additive A and additive B are mixed and sintered once; The precursor Ni a M b In (OH)2, 0.8≤a≤0.98, 0<b≤0.20, a+b=1; The additive A is at least two of the oxides, hydroxides or carbonates of Zr, Sr, Ca, Mg, Ba, Y, Nb, Ti, Mo, Sn, Ta, Sb, Bi and W; The primary sintering includes a first insulation platform and a second insulation platform; the temperature of the first insulation platform is 350-650°C; the temperature of the second insulation platform is 680-900°C.
10. The preparation method according to claim 9, characterized in that: The insulation time of the first insulation platform is 2 to 6 hours.
11. The preparation method according to claim 9, characterized in that: The insulation time of the second insulation platform is 6 to 16 hours.
12. The preparation method according to any one of claims 9 to 11, characterized in that: The preparation method further comprises: washing the product of the primary sintering with water, and mixing the washed product with an additive C and then performing secondary sintering; The additive C comprises at least one of boric acid, aluminum oxide, aluminum hydroxide, cerium oxide, aluminum fluoride, cerium fluoride, magnesium oxide, and magnesium hydroxide.
13. The preparation method according to claim 12, characterized in that: The constant temperature of the secondary sintering is 200-450°C.
14. The preparation method according to claim 12, characterized in that: The constant temperature time of the secondary sintering is 5 to 10 hours.
15. A lithium secondary battery, characterized in that: The raw material for preparing the lithium secondary battery includes the modified high-nickel positive electrode material as described in any one of claims 1 to 8, or includes the modified high-nickel positive electrode material prepared by the preparation method as described in any one of claims 9 to 14.