A non-scribe perovskite solar cell unit, assembly and preparation method thereof

Perovskite solar cell units designed through the unmarked process use parallel structure and high-temperature annealing technology to solve the problems of cumbersome preparation process and low yield, achieving efficient utilization area and low maintenance costs. Industrialized production.

CN118555847BActive Publication Date: 2024-11-22SHENZHEN FUGUANG PHOTOVOLTAIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411025897.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The commercial production of perovskite solar cells faces problems such as cumbersome preparation process, expensive equipment, low yield, insufficient effective utilization area and high maintenance costs.

Method used

Perovskite solar cell units designed using a scribing process, including a transparent substrate and a conductive layer, form a parallel structure through a silver gate wire electrode and an insulating layer, simplifying the preparation process, improving the yield rate, and improving the silver gate wire through high-temperature annealing. Adhesion quality enables efficient utilization of large-area perovskite solar cells.

Benefits of technology

The effective utilization area of ​​perovskite solar cells has been greatly improved to 98%, reducing preparation and maintenance costs, simplifying process flow, facilitating industrial production, and improving yield and battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118555847B_ABST
    Figure CN118555847B_ABST
Patent Text Reader

Abstract

The present invention discloses a non-scribing perovskite solar cell unit, wherein a transparent substrate is divided into a first region and a second region arranged front and back; wherein a conductive layer is arranged in the first region, a first grid line is arranged at the front side edge of the conductive layer, and a second grid line is vertically connected to the first grid line and evenly spaced along its length direction; a third grid line parallel to the first grid line is arranged at the rear side edge of the second region; an insulating layer is coated on the first grid line, the second grid line and the third grid line respectively, and the first grid line, the second grid line and the third grid line are enclosed by the insulating layer to form a deposition groove, in which an electron transport layer, a perovskite active layer, a hole transport layer and a metal back electrode are sequentially arranged. The non-scribing perovskite solar cell unit provided by the present invention can effectively improve the effective utilization area of ​​the perovskite solar cell, greatly optimize the yield rate of solar cell production, and has the characteristic of being flexibly spliced ​​into a module, which is suitable for promotion and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solar cells, and in particular relates to a non-scribe perovskite solar cell unit, a component and a preparation method thereof. Background Art

[0002] Perovskite solar cells are solar cells that use perovskite-type organic metal halide semiconductors as light-absorbing materials. 2 ) has increased its photoelectric conversion efficiency from 3.8% in 2009 to 26.14% at present. The simple preparation process and low production cost make it have great potential for commercial application; in recent years, low-cost and high-efficiency new large-area perovskite solar cells have become the main research direction.

[0003] However, there are still many obstacles to the commercial production of perovskite solar cells, mainly including: 1) The most common perovskite solar cell modules currently need to go through P1, P2, P3, and P4 scribing before they can be made. The process involved is cumbersome, the equipment is expensive, and the yield is low; 2) The effective utilization area of ​​traditional large-area perovskite solar cells in a series structure is only 60~70%, which seriously affects the working efficiency of the solar cell; 3) The current mainstream perovskite solar modules are all made of a super-large-area perovskite solar cell. Once any part of the entire module is damaged, the module will be completely damaged and cannot be repaired. Summary of the invention

[0004] The main purpose of the present invention is to provide a perovskite solar cell unit and component structure without scribing process to address the problems and shortcomings of the existing solar cell module preparation process, such as complicated process, expensive equipment, low yield rate and high maintenance cost, which can effectively improve the effective utilization area of ​​perovskite solar cells, greatly optimize the yield rate of solar cell production, and have the characteristics of being able to be flexibly spliced ​​into modules; the preparation method involved is simple, with fewer steps, high yield rate, low maintenance cost, and convenient for industrial production.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A non-scribe perovskite solar cell unit, comprising a transparent substrate and a conductive layer, wherein the transparent substrate is divided into a first region and a second region arranged front and back; wherein the first region is coated with the conductive layer, a first grid line and a plurality of second grid lines are arranged on the conductive layer, the first grid lines are arranged at the front side edge of the conductive layer, and are arranged from left to right; the second grid lines are arranged at uniform intervals along the length direction of the first grid lines, and the second grid lines are vertically connected to the first grid lines;

[0007] A third grid line parallel to the first grid line is arranged at the rear side of the second area, and the third grid line is arranged from left to right;

[0008] An insulating layer (insulating glue that does not react with the silver grid line, etc.) is coated on the first grid line, the second grid line and the third grid line respectively, wherein the rear end of the insulating layer on each second grid line extends toward the third grid line until it is connected to the insulating layer on the third grid line;

[0009] Two adjacent second gate lines and the corresponding first gate line and third gate line are surrounded by an insulating layer to form a deposition groove, in which an electron transport layer, a perovskite active layer, a hole transport layer and a metal back electrode are sequentially arranged.

[0010] Furthermore, the thickness of the first grid line, the second grid line and the third grid line is 5-10 μm, and the conductivity of the silver grid line can be improved by optimizing the thickness of the silver grid line electrode.

[0011] Furthermore, the width of the first gate line is 1-3 mm; the width of the second gate line is 100-300 μm; and the width of the third gate line is 1-3 mm.

[0012] In the above solution, the coating thickness of the protective glue on the surface of the second grid line is 40-60 μm.

[0013] Preferably, the thickness of the electron transport layer is 10-50 nm; the thickness of the perovskite active layer is 400-600 nm; and the thickness of the hole transport layer is 600-800 nm.

[0014] Furthermore, the electron transport layer can be made of SnO2, TiO2, ZnO or PCBM layer.

[0015] Furthermore, the hole transport layer can be made of spiro-OMeTAD, SAM small molecules (such as MeO-2PACz, MeO-4PACz, 2PACz, etc.), PTAA, NiO X or PEDOT:PSS layer, etc.

[0016] In the above solution, the material of the metal back electrode is one of gold, silver, copper and alloys.

[0017] In the above scheme, in the non-scribe perovskite solar cell unit, the perovskite cell small units formed in the deposition groove part are in a parallel structure.

[0018] The above-mentioned method for preparing a non-scribe perovskite solar cell unit comprises the following steps:

[0019] 1) providing a cleaned transparent conductive substrate according to the designed first area and second area;

[0020] 2) According to the designed first gate line, second gate line and third gate line structures, silver paste is printed on the surface of the first region conductive layer and the second region respectively, and annealed to obtain silver gate line electrodes; then an insulating layer is provided on the surface of the silver gate line electrodes;

[0021] 3) Arranging an electron transport layer on the surface of the deposition tank of the substrate obtained in step 2);

[0022] 4) preparing a perovskite active layer on the electron transport layer;

[0023] 5) providing a hole transport layer on the perovskite active layer;

[0024] 6) Preparing a metal back electrode on the hole transport layer to obtain the scribe-free perovskite solar cell unit.

[0025] Preferably, in step 1), the average light transmittance of the transparent conductive substrate is above 80%.

[0026] Furthermore, the transparent conductive substrate can be made of FTO glass or ITO glass.

[0027] Preferably, in step 2), the viscosity of the silver paste is 1000-20000 mPas, and the concentration of the silver element introduced into the silver paste is 50-98 mol%.

[0028] Furthermore, the viscosity of the silver paste is adjusted by using diethylene glycol monoethyl ether or the like.

[0029] In the above scheme, the printing method is screen printing, the screen distance between the screen and the substrate during the printing process is 1-3 mm, and the printing speed is 50-200 mm / s.

[0030] In the above scheme, the temperature of the annealing treatment is 400-500°C, the time of the annealing treatment is 5-10 min, the annealing heating rate is 5-30°C / min, and the cooling method is natural cooling.

[0031] Preferably, in step 3), the electron transport layer is prepared by chemical bath deposition, and the specific steps include: immersing the substrate obtained in step 2) in a SnCl2 solution, depositing under heating conditions, and then performing annealing heat treatment to form an electron transport layer on the surface of the substrate obtained in step 2).

[0032] In the above scheme, the concentration of the SnCl2 solution is 0.3~0.55g / L.

[0033] In the above scheme, the deposition time is 2.5-3 hours, and the deposition temperature is 70-90°C.

[0034] In the above scheme, the annealing heat treatment is performed at a temperature of 150-200° C. and a time of 0.5-2 h.

[0035] Preferably, in step 4), the preparation step of the perovskite active layer adopts a vacuum evaporation process and an ultrasonic spray process, and the specific steps include: vacuum evaporating a layer of cesium halogen salt (CsI, CsBr or CsCl) on the electron transport layer of the substrate, and then vacuum evaporating a layer of lead salt (PbI2, PbBr2 or PbCl2) on the cesium halogen salt, and then spraying a layer of methylamino salt solution thereon and performing annealing treatment to generate a perovskite active layer.

[0036] In the above scheme, the imidamide salt can be selected from one or more of FAI (formamidine hydroiodide), FABr (formamidine hydrobromide) and the like.

[0037] Preferably, the mass ratio of FAI (formamidine hydroiodide) to FABr (formamidine hydrobromide) is 0.9-10:1.

[0038] In the above scheme, the solvent used in the methylimidamine salt solution is a composite of n-butanol and N-methylpyrrolidone.

[0039] Furthermore, the volume ratio of n-butanol to N-methylpyrrolidone is 9-99:1.

[0040] In the above scheme, the concentration of the methylcarbazine salt solution is 20-30 mg / ml.

[0041] In the above scheme, the thickness of the cesium halogen salt is 25-35 nm, the thickness of the lead salt is 300-350 nm, and the thickness of the methylimidamine salt depends on the reaction conditions.

[0042] In the above scheme, the temperature used for the annealing treatment is 150-170° C. and the time is 30-90 min.

[0043] Preferably, in step 5), the hole transport layer is prepared by ultrasonic spraying, and the specific steps include: ultrasonically atomizing the prepared spiro-OMeTAD solution into droplets in the air, and uniformly covering the surface of the perovskite active layer.

[0044] Preferably, the thickness of the gold electrode layer is 50-70 nm.

[0045] The silver grid electrode designed in the present invention can quickly lead out the electrons generated by the perovskite absorbing light and reduce the series resistance of the perovskite solar cell; the prepared large-area perovskite solar cells with a parallel structure can be spliced ​​into a perovskite solar cell module of a designed size through the main grid line in the silver grid electrode; in addition, during the preparation process, the bonding quality of the particles inside the silver grid is improved by high-temperature annealing; and a layer of protective glue is set (printed) on the silver grid electrode to prevent the perovskite layer from contacting with silver and causing a short circuit.

[0046] The present invention also provides a scribe-free perovskite solar cell assembly, which comprises a plurality of scribe-free perovskite solar cell units connected in series.

[0047] Furthermore, different un-scribed perovskite solar cell units are connected in parallel by providing welding beads between the first grid lines.

[0048] Furthermore, the effective utilization area of ​​the scribe-free perovskite solar cell unit can reach 98% of the substrate area.

[0049] The present invention can effectively reduce the difficulty of preparing perovskite solar cell modules, and does not require the traditional scribing process for the perovskite material layer or the conductive layer. Under the premise of effectively simplifying the preparation process, the effective utilization area of ​​large-area perovskite solar cells can be increased to more than 98%. The parallel structure can be spliced ​​and the characteristics of no scribing process effectively solve the problem of low yield rate of large-area perovskite solar cells in the production process, and can be spliced ​​into larger-area perovskite solar cell modules according to demand.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] 1. Full area: The present invention can increase the effective utilization area of ​​large-area perovskite solar cells (the percentage of the area covered by the perovskite active material to the substrate area) to more than 98%;

[0052] 2. Compared with the traditional perovskite solar cell module based on the scribing process and the series structure, the present invention can increase the light absorption area by 40%, and can effectively reduce the process and save costs; in addition, the present invention can further connect the perovskite solar cell units with a parallel structure in parallel or in series to form a solar cell module of the required area, which can effectively improve the yield and reduce the maintenance cost on the basis of ensuring and further improving the battery performance;

[0053] 3. The present invention does not require the traditional precise laser scribing process or etching process, and the preparation method involved is simple, the conditions are relatively mild, the operation is convenient, and it is convenient for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1A schematic diagram of the structure of the perovskite solar cell according to Example 1 of the present invention (the middle area is cut off);

[0055] In the figure, 1 is a glass substrate, 2 is a FTO conductive layer, 3 is an electron transport layer, 4 is a perovskite absorption layer, 5 is a hole transport layer, 6 is a metal back electrode, 7 is a silver grid line, and 8 is an insulating layer (protective glue);

[0056] Figure 2 (a) the region division of the transparent substrate and (b) the corresponding topography of the transparent conductive substrate used in Example 1;

[0057] Figure 3 The structure diagram of the silver grid line printed in Example 1, in which 1 is the exposed surface of the glass substrate, 2 is the FTO conductive layer, 7-1 is the first grid line, 7-2 is the second grid line, and 7-3 is the third grid line;

[0058] Figure 4 A schematic diagram of the structure of a perovskite solar cell unit with a parallel structure obtained in Example 1;

[0059] Figure 5 This is a schematic diagram of the splicing of the perovskite solar cell module described in Example 1;

[0060] Figure 6 This is a schematic diagram of the line structure described in Comparative Example 2;

[0061] Figure 7 The morphology diagrams of (a) Comparative Example 3 and (b) Example 2 after preparing the perovskite active layer. DETAILED DESCRIPTION

[0062] The present invention is further described in detail below through a specific implementation case. This implementation case is specifically implemented based on the technology of the present invention, and a detailed implementation method and specific operation process are now given, but the scope of protection of the present invention is not limited to the implementation case given below.

[0063] The present invention provides a non-scribe perovskite solar cell unit, which includes a transparent substrate 1 and a FTO conductive layer 2, wherein the transparent substrate 1 is divided into a first area and a second area arranged front and back; wherein the first area is coated with the conductive layer 2, and a first grid line 7-1 and a plurality of second grid lines 7-2 are arranged on the conductive layer 2, wherein the first grid line 7-1 is arranged at the front side edge of the conductive layer 2 and is arranged from left to right; the second grid lines 7-2 are evenly spaced along the length direction of the first grid lines 7-1, and the second grid lines 7-2 are vertically connected to the first grid lines 7-1;

[0064] A third grid line 7-3 parallel to the first grid line is arranged at the rear side of the second region, and the third grid line 7-3 is arranged in a full length from left to right;

[0065] The insulating layer 8 (not in contact with the silver) is coated on the first gate line 7-1, the second gate line 7-2 and the third gate line 7-3.

[0066] The insulating glue that reacts with the gate line), wherein the rear end of the insulating layer 8 on each second gate line 7-2 extends toward the direction of the third gate line 7-3 until it is connected to the insulating layer 8 on the third gate line 7-3;

[0067] Two adjacent second gate lines 7-2 and the corresponding first gate line 7-1 and third gate line 7-3 are surrounded by an insulating layer 8 to form a deposition groove, in which an electron transport layer 3, a perovskite active layer 4, a hole transport layer 5 and a metal back electrode 6 are arranged in sequence; a single grid cell is formed in each deposition groove.

[0068] The obtained large-area perovskite solar cell structure with parallel structure is as follows Figure 4 shown.

[0069] The present invention also provides a method for preparing a perovskite solar cell module without a scribing process, which specifically comprises the following steps:

[0070] 1) Provide substrate: Provide Figure 2 The transparent conductive substrate shown has an average light transmittance of 80%;

[0071] 2) Substrate treatment: Clean the glass substrate; when cleaning, use detergent solution, deionized water and ethanol to ultrasonically clean for 15 to 20 minutes each, blow dry with nitrogen flow, and then place in a plasma cleaning machine for 10 to 15 minutes;

[0072] 3) Preparation of silver grid electrode: Use a screen printer to print silver paste on the treated substrate. The printed silver grid structure is as follows: Figure 3 As shown, each silver paste is then annealed for 5 to 30 minutes according to the corresponding curing temperature (such as annealing at 180°C for low-temperature silver paste and 500°C for high-temperature silver paste) to prepare a silver grid line electrode, wherein the first grid line width of the silver grid line is 1 to 3 mm and the thickness is 5 to 10 μm; the second grid line width is 100 to 300 μm and the thickness is 5 to 10 μm;

[0073] 4) Preparing a protective glue: printing a protective glue sleeve on the surface of the silver grid line to prevent the silver grid line from contacting the perovskite and causing a short circuit, and then curing it at 180° C. for 5 minutes; the protective glue has a width of 350 μm (±50 μm) and a thickness of 50 μm (±10 μm);

[0074] 5) Preparation of electron transport layer: soak the substrate printed with protective glue in SnCl2 aqueous solution, deposit at 90℃ for 2.5~3 hours, and then anneal at 180℃ for 1 hour to complete the preparation of electron transport layer SnO2; wherein, the SnCl2 aqueous solution is prepared by mixing 100ml deionized water and 20ml SnCl2 mother liquor, and the SnCl2 mother liquor is prepared by 548mg stannous chloride dihydrate, 50μl thioglycolic acid, 2.5ml concentrated hydrochloric acid, 2.5g urea and 200ml deionized water;

[0075] 6) Preparation of perovskite active layer: thermally evaporate a layer of cesium halogen salt (CsI or CsBr or CsCl) on the electron transport layer of the substrate, then evaporate a layer of lead salt (PbI2 or PbBr2 or PbCl2) on the cesium halogen salt, and then spray a layer of methyl imidamine salt thereon and anneal, and the three react to form a perovskite active layer 4; the thickness of the cesium halogen salt is 25~35nm, the thickness of the lead salt is 300~350nm, and the thickness of the methyl imidamine salt depends on the reaction conditions; the thickness of the perovskite active layer is 400~600nm;

[0076] 7) Preparation of hole transport layer: spraying a layer of spiro-OMeTAD on the corresponding area of ​​the perovskite active layer of the substrate to form a hole transport layer. The specific steps are: using an ultrasonic spray process to spray the prepared spiro-OMeTAD solution onto the corresponding area of ​​the perovskite active layer;

[0077] 8) Preparation of metal back electrode: a layer of metal gold is deposited on the surface of the perovskite to form a metal back electrode 6. Specifically, the substrate is fixed in the co-evaporation coating system using a mask plate, and the vacuum degree in the chamber reaches 10 -4 ~10 -3 After 30 Å / s, the metal gold is heated and a layer of gold electrode is deposited on the surface of the spiro-OMeTAD layer at an evaporation rate of 1.5-2.5 Å / s to complete the preparation of the entire perovskite solar cell; the thickness of the metal back electrode is 50-70 nm;

[0078] 9) Splice the prepared devices by welding ribbons, such as Figure 5 As shown, a solar cell module of a required area size can be spliced;

[0079] 10) Encapsulation of perovskite solar cell modules: specifically, encapsulation is performed using a laminator.

[0080] In the following embodiments, the conductive silver paste BY-0665PF provided by Foshan Zhongkexing New Materials Co., Ltd. was diluted with diethylene glycol monoethyl ether, wherein the dilution volume ratio of the silver paste to diethylene glycol monoethyl ether was 9.5:0.5; the viscosity of the diluted silver paste was 10000 mPas, wherein the concentration of silver ions was 95 mol%.

[0081] Example 1

[0082] A perovskite solar cell unit and module structure without scribing process, the structural schematic diagram of which is shown in Figure 1 ; Using a 5cm×5cm parallel structure perovskite solar cell element as the power generation unit (photoelectric conversion efficiency is about 15%), the specific preparation steps are as follows:

[0083] 1) Providing a substrate: providing a 5 cm×5 cm FTO transparent conductive glass substrate, wherein the first region of the transparent glass substrate of the FTO transparent conductive glass substrate is provided with an FTO conductive layer, and the second region is an exposed glass substrate. For specific structure, see Figure 2 ;

[0084] 2) Processing substrate: Clean the glass substrate; when cleaning, use detergent solution, deionized water and ethanol to ultrasonically clean for 15 to 20 minutes each, and blow dry the substrate with dry nitrogen gas flow for later use;

[0085] 3) Preparation of silver grid lines: Silver paste (viscosity of 10000 mPas, silver ion concentration of 95 mol%) is printed on the treated substrate using a screen printer. The structure of the silver grid lines is as follows: Figure 2 Then, annealing is performed at 500°C for 5 minutes to prepare silver grid lines, the thickness of the silver grid lines is 5-10 μm, the width of the silver grid lines of the first grid line part is 1-3 mm, and the width of the silver grid lines of the second grid line part is 50-200 μm;

[0086] 4) Prepare protective glue: print the protective glue sleeve on the surface of the silver grid line to protect the silver grid line. Specifically, print the protective glue on the area where the silver grid line of the substrate is located. In the second grid line part, the protective glue can completely cover the silver grid line. The width of the protective glue is wider than the silver grid line. In the first grid line part, the protective glue only needs to cover half of the silver grid line. The width of the protective glue is 300-400 μm and the thickness is 40-60 μm.

[0087] 5) Preparation of electron transport layer: Soak the substrate with the printed protective glue in a SnCl2 aqueous solution (concentration of 0.46 g / L) at 90°C for 2.5-3 hours to complete the preparation of the electron transport layer SnO2 (thickness of 10 nm);

[0088] 6) Preparation of perovskite active layer: thermally evaporate a 30 nm thick CsBr layer on the electron transport layer of the substrate, then thermally evaporate a 300 nm thick PbI2 layer, and then spray a layer of amine salt solution (concentration of 20 mg / mL) thereon, in which the ammonium salt is a mixture of FAI (formamidine hydroiodide) and FABr formamidine hydrobromide), the mass ratio of FAI and FABr is 19:21 (0.9:1), and the solvent used is a mixture of n-butanol and NMP in a volume ratio of 99:1; then heat-treat at 150-170°C for 30-90 min, and the amine salt, cesium bromide and lead iodide react to form a perovskite active layer (thickness of 500 nm);

[0089] 7) Preparation of hole transport layer: spray a layer of spiro-OMeTAD on the corresponding area of ​​the perovskite active layer of the substrate to form a hole transport layer; the specific steps are: use ultrasonic spray to spray the prepared spiro-OMeTAD solution on the corresponding area of ​​the perovskite active layer, and then dry it naturally at a temperature of 25°C and a humidity of 30% to obtain a hole transport layer with a thickness of 700nm;

[0090] 8) Preparation of metal back electrode: deposit a layer of metal gold on the surface of the solar cell preform to form a metal back electrode; the specific steps are: use a mask plate to fix the substrate in the co-evaporation coating system, wait until the vacuum degree in the chamber reaches 10 -4 ~10 -3 After 100 Pa, the metal gold was heated and a layer of gold electrode (60 nm thick) was deposited on the surface of the hole transport layer at an evaporation rate of 2 Å / s to complete the preparation of the line-free perovskite solar cell unit;

[0091] 9) The prepared non-scribe perovskite solar cell units are spliced ​​by welding (setting welds between the first grid lines), such as Figure 5 As shown, the area that can be spliced ​​is 1m 2 Solar cell modules;

[0092] 10) Use a laminator to encapsulate the perovskite solar cell modules.

[0093] Example 2

[0094] A perovskite solar cell unit and module structure without scribing process, with a 10cm×10cm parallel structure perovskite solar cell element as a power generation unit (photoelectric conversion efficiency is about 10%), and the specific preparation steps are as follows:

[0095] 1) Provide substrate: Provide 10cm×10cm FTO transparent conductive substrate;

[0096] 2) Processing substrate: Clean the glass substrate; when cleaning, use detergent solution, deionized water and ethanol to ultrasonically clean for 15 to 20 minutes each, and blow dry the substrate with dry nitrogen gas flow for later use;

[0097] 3) Preparation of silver grid lines: Silver paste (viscosity of 10000 mPas, silver ion concentration of 95 mol%) is printed on the treated substrate using a screen printer. The structure of the silver grid lines is as follows: Figure 2 Then, annealing is performed at 500°C for 5 minutes to prepare silver grid lines, wherein the thickness of the silver grid lines is 5-10 μm, the width of the silver grid lines of the first grid line part is 1-3 mm, and the width of the silver grid lines of the second sub-grid line part is 50-200 μm;

[0098] 4) Prepare protective glue: print the protective glue sleeve on the surface of the silver grid line to protect the silver grid line, specifically: print the protective glue on the area where the silver grid line of the substrate is located, in the second grid line part, the protective glue can cover all the silver grid lines, the width of the protective glue is wider than the silver grid line, in the first grid line part, the protective glue only needs to cover half the width of the silver grid line, the width of the protective glue is 300~400μm, and the thickness is 40~60μm;

[0099] 5) Preparation of electron transport layer: Soak the substrate with the printed protective glue in a SnCl2 aqueous solution (concentration of 0.46 g / L) at 90°C for 2.5-3 hours to complete the preparation of the electron transport layer SnO2 (thickness of 10 nm);

[0100] 6) Preparation of perovskite active layer: vacuum thermal evaporation of a 30 nm thick CsBr layer on the electron transport layer of the substrate, thermal evaporation of a 300 nm thick PbI2 layer, and then spraying a layer of amine salt solution (concentration of 20 mg / mL) thereon, wherein the ammonium salt in the amine salt solution is a mixture of FAI (formamidine hydroiodide) and FABr formamidine hydrobromide), the mass ratio of FAI to FABr is 19:21 (0.9:1), and the solvent used is a mixture of n-butanol and NMP in a volume ratio of 99:1; then heating treatment at 150-170°C for 30-90 min, the amine salt, cesium bromide and lead iodide react to form a perovskite active layer (thickness of 500 nm);

[0101] 7) Preparation of hole transport layer: spray a layer of spiro-OMeTAD on the corresponding area of ​​the perovskite active layer of the substrate, dry it, and form a hole transport layer; the specific steps are: use ultrasonic spray to spray the prepared spiro-OMeTAD solution on the corresponding area of ​​the perovskite active layer, and then dry it naturally at a temperature of 25°C and a humidity of 30% to obtain a hole transport layer with a thickness of 700nm;

[0102] 8) Preparation of metal back electrode: deposit a layer of metal gold on the surface of the solar cell preform to form a metal back electrode (thickness of 60nm); the specific steps are: use a mask to fix the substrate in the co-evaporation coating system, wait until the vacuum degree in the chamber reaches 10 -4 ~10 -3 After 1000 Pa, the metal gold was heated and a layer of gold electrode was deposited on the surface of the hole transport layer at an evaporation rate of 2 Å / s to complete the preparation of the line-free perovskite solar cell unit;

[0103] 9) The prepared non-scribe perovskite solar cell units are spliced ​​by welding (setting welds between the first grid lines), such as Figure 5 As shown, the area that can be spliced ​​is 1m 2 Solar cell modules;

[0104] 10) Use a laminator to encapsulate the perovskite solar cell modules.

[0105] Comparative Example 1

[0106] A perovskite solar cell with an area of ​​10 cm×10 cm prepared by a slit coating process, wherein the preparation steps are as follows:

[0107] 1) Substrate treatment: Clean a 10 cm × 10 cm FTO transparent conductive glass substrate; use detergent solution, deionized water and ethanol for ultrasonic cleaning for 15 to 20 minutes each, and blow dry the substrate with a dry nitrogen gas flow for later use;

[0108] 2) Preparation of electron transport layer: The substrate printed with protective glue (the specific preparation method is the same as step 3) and step 4) of Example 1) is immersed in a SnCl2 aqueous solution (concentration of 0.46 g / L) at 90°C for 2.5-3 hours to complete the preparation of the electron transport layer SnO2 (thickness of 10 nm);

[0109] 3) Preparation of perovskite active layer: Prepare a 1.2M FAPbI3 precursor solution, use a 1ml syringe to load the precursor solution into a 3D printed slot mold (the slot mold has a 20 mm gasket and a 13 mm curved guide), control the distance between the substrate and the curved guide after setting the electron transport layer SnO2 to 100μm, and keep the slit coating speed at 1.5mm / s; finally, anneal at 150℃ for 30min to obtain a perovskite active layer (thickness 500nm);

[0110] 4) Preparation of hole transport layer: spray a layer of spiro-OMeTAD on the corresponding area of ​​the perovskite active layer of the substrate to form a hole transport layer; specifically, use ultrasonic spray to spray the prepared spiro-OMeTAD solution on the corresponding area of ​​the perovskite active layer; then naturally dry it at a temperature of 25°C and a humidity of 30% to obtain a perovskite active layer with an average thickness of 1 μm;

[0111] 5) Preparation of metal back electrode: Deposit a layer of metal gold on the surface of the solar cell preform to form a metal back electrode (thickness of 60nm); specifically, use a mask to fix the substrate in the co-evaporation coating system, and wait until the vacuum degree in the chamber reaches 10 -4 ~10 -3 After 3 Pa, the metal gold is heated and a layer of gold electrode is deposited on the surface of the hole transport layer at an evaporation rate of 2Å / s to complete the preparation of the entire perovskite solar cell.

[0112] Comparative Example 2

[0113] A perovskite solar cell using a scribing process is prepared by using a vacuum evaporation + ultrasonic spray process with an area of ​​10cm×10cm. The specific preparation steps are as follows:

[0114] 1) Provide substrate: Provide 10cm×10cm FTO transparent conductive glass substrate

[0115] 2) Processing substrate: Clean the glass substrate; when cleaning, use detergent solution, deionized water and ethanol to ultrasonically clean for 15 to 20 minutes each, and blow dry the substrate with dry nitrogen gas flow for later use:

[0116] 3) Preparation of electron transport layer: Soak the treated substrate in SnCl2 aqueous solution (concentration of 0.46 g / L) at 90°C for 2.5-3 hours to complete the preparation of electron transport layer SnO2 (thickness of 10 nm);

[0117] 6) Preparation of perovskite active layer: thermally evaporate a 30 nm thick CsBr layer and a 300 nm thick PbI2 layer on the electron transport layer of the substrate, and then spray a layer of amine salt solution thereon, wherein the ammonium salt in the amine salt solution (concentration of 20 mg / mL) is a mixture of FAI (formamidine hydroiodide) and FABr formamidine hydrobromide), the mass ratio of FAI to FABr is 19:21 (0.9:1), and the solvent used is a mixture of n-butanol and NMP in a volume ratio of 99:1; then heat-treat at 150-170°C for 30-90 min, and the amine salt, cesium bromide and lead iodide react to form a perovskite active layer (thickness of 500 nm);

[0118] 7) Preparation of hole transport layer: spray a layer of spiro-OMeTAD on the corresponding area of ​​the perovskite active layer of the substrate, dry it, and form a hole transport layer; the specific steps are: use ultrasonic spray to spray the prepared spiro-OMeTAD solution on the corresponding area of ​​the perovskite active layer, and then dry it naturally at a temperature of 25°C and a humidity of 30% to obtain a hole transport layer with a thickness of 700nm;

[0119] 8) Preparation of metal back electrode: deposit a layer of metal gold on the surface of the solar cell preform to form a metal back electrode; the specific steps are: use a mask plate to fix the substrate in the co-evaporation coating system, wait until the vacuum degree in the chamber reaches 10 -4 ~10 -3 After 100 Pa, the metal gold was heated and a layer of gold electrode (60 nm thick) was deposited on the surface of the hole transport layer at an evaporation rate of 2 Å / s to complete the preparation of the line-free perovskite solar cell unit;

[0120] 9) Perform laser scribing, using a laser beam to Figure 6 The metal electrode, hole transport layer, perovskite active layer, electron transport layer, and FTO conductive layer in the middle crossed-out part are removed, and then the insulating material is filled into the crossed-out part (the effective utilization area of ​​the resulting perovskite solar cell is about 60%).

[0121] Comparative Example 3

[0122] A perovskite solar cell unit and module structure without scribing process, with a 10cm×10cm parallel structure perovskite solar cell element as a power generation unit, and the specific preparation steps are as follows:

[0123] 1) Providing a substrate: providing a 10 cm×10 cm FTO transparent conductive glass substrate, wherein the first region of the transparent glass substrate of the FTO transparent conductive glass substrate is provided with an FTO conductive layer, and the second region is an exposed glass substrate. For specific structure, see Figure 2 ;

[0124] 2) Processing substrate: Clean the glass substrate; when cleaning, use detergent solution, deionized water and ethanol to ultrasonically clean for 15 to 20 minutes each, and blow dry the substrate with dry nitrogen gas flow for later use:

[0125] 3) Preparation of silver grid lines: Silver paste (viscosity of 10000 mPas, silver ion concentration of 95 mol%) is printed on the treated substrate using a screen printer. The structure of the silver grid lines is as follows: Figure 2 Then, annealing is performed at 500°C for 5 minutes to prepare silver grid lines, the thickness of the silver grid lines is 5-10 μm, the width of the silver grid lines of the first grid line part is 1-3 mm, and the width of the silver grid lines of the second grid line part is 50-200 μm;

[0126] 4) Prepare protective glue: print the protective glue sleeve on the surface of the silver grid line to protect the silver grid line. Specifically, print the protective glue on the area where the silver grid line of the substrate is located. In the second grid line part, the protective glue can completely cover the silver grid line. The width of the protective glue is wider than the silver grid line. In the first grid line part, the protective glue only needs to cover half of the silver grid line. The width of the protective glue is 300-400 μm and the thickness is 40-60 μm.

[0127] 5) Preparation of electron transport layer: Soak the substrate with the printed protective glue in a SnCl2 aqueous solution (concentration of 0.46 g / L) at 90°C for 2.5-3 hours to complete the preparation of the electron transport layer SnO2 (thickness of 10 nm);

[0128] 6) Preparation of perovskite active layer: thermally evaporate a 30 nm thick CsBr layer on the electron transport layer of the substrate, then thermally evaporate a 300 nm thick PbI2 layer, and then spray a layer of amine salt solution (concentration of 20 mg / mL) thereon, wherein the ammonium salt in the amine salt solution is a mixture of FAI (formamidine hydroiodide) and FABr formamidine hydrobromide), the mass ratio of FAI to FABr is 19:21 (0.9:1), and the solvent used is a mixture of isopropanol and NMP in a volume ratio of 99:1, and heat treatment is carried out at 150-170°C for 30-90 min, and the amine salt, cesium bromide and lead iodide react to form a perovskite active layer (thickness of 500 nm);

[0129] 7) Preparation of hole transport layer: spray a layer of spiro-OMeTAD on the corresponding area of ​​the perovskite active layer of the substrate to form a hole transport layer; the specific steps are: use ultrasonic spray to spray the prepared spiro-OMeTAD solution on the corresponding area of ​​the perovskite active layer, and then dry it naturally at a temperature of 25°C and a humidity of 30% to obtain a hole transport layer with a thickness of 700nm;

[0130] 8) Preparation of metal back electrode: deposit a layer of metal gold on the surface of the solar cell preform to form a metal back electrode; the specific steps are: use a mask plate to fix the substrate in the co-evaporation coating system, wait until the vacuum degree in the chamber reaches 10 -4 ~10 -3 After 30 0.5 Pa, the metal gold was heated and a layer of gold electrode (60 nm thick) was deposited on the surface of the hole transport layer at an evaporation rate of 2 Å / s to complete the preparation of the line-free perovskite solar cell unit.

[0131] Figure 7 The morphology of the perovskite solar cell unit described in Comparative Example 3 (a) and Example 2 (b) after the perovskite active layer is prepared in step 6). It can be seen that the present invention can effectively improve the hole problem generated in Comparative Example 3.

[0132] The performance test results of the perovskite solar cell units obtained in Examples 1-2 and Comparative Examples 1-3 are shown in Table 1, respectively.

[0133] Table 1 Perovskite solar cell unit performance test results

[0134]

[0135] The above results show that the perovskite solar cell unit obtained by the present invention has a high photoelectric conversion efficiency and short-circuit current; the perovskite solar cell unit obtained by the comparative example is not suitable for further splicing to prepare a larger-sized perovskite solar cell module. The silver grid line structure involved in the present invention has obvious protrusions relative to the substrate. The conventional process methods for preparing large-area perovskite solar cells such as scraping or slit coating cannot effectively solve this problem and cannot form a uniform and high-quality perovskite film, especially in the edge area of ​​the grid line, where the perovskite film fails to cover the grid line. The present invention adopts a perovskite active layer preparation process based on "evaporation + spraying" and further combines improved means such as complex amine salts to effectively ensure the composite effect of the corresponding functional layer and the performance of the obtained non-scribed perovskite solar cell unit and module.

[0136] The performance test results of the perovskite solar cell module obtained in Example 1 are shown in Table 2.

[0137] Table 2 Performance test results of the assembled perovskite solar cell modules

[0138]

[0139] After testing, the output voltage of the perovskite solar cell unit obtained in Example 1 was 1.07V, and the output current was 820mA; the voltage of the perovskite solar cell module obtained was 0.98V, and the module current was 3.09A.

[0140] It should be understood by those skilled in the art that one of the features or purposes of the present invention is: 1. Full area: The structure of the present invention can make the effective area of ​​large-area perovskite solar cells reach more than 98%; 2. The present invention is different from other large-area perovskite solar cell devices in that: the present invention can splice the prepared perovskite solar cells into solar cell modules of the required size, and the module has the characteristics of low maintenance cost. If a certain area of ​​the module is damaged, only the damaged device in that area needs to be replaced; 3. The present invention does not require precise laser scribing during the preparation process, and the preparation process is easy to implement, which is conducive to large-scale industrial production; 4. The present invention is prepared in the air, and the preparation process is easy to implement, which is convenient for industrial production.

[0141] Finally, it should be noted that the above are only preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to replace some of the technical features therein with equivalents. However, any modifications, equivalent replacements, improvements, etc. made on the basis of the structure of the present invention within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A non-scribe perovskite solar cell unit, comprising a transparent substrate and a conductive layer, characterized in that: The transparent substrate is divided into a first area and a second area arranged front and back; wherein the first area is provided with a conductive layer, and a first grid line and a plurality of second grid lines are provided on the conductive layer, wherein the first grid line is arranged at the front side edge of the conductive layer and is arranged in the left and right directions; and the second grid lines are vertically connected to the first grid lines and are evenly spaced along the length direction thereof; A third gate line parallel to the first gate line is arranged at the rear side edge of the second region, and the third gate line is arranged in a full length from left to right; an insulating layer is coated on the first gate line, the second gate line and the third gate line respectively, wherein the insulating layer on the first gate line is connected to the insulating layer on the second gate line; the insulating layer on the second gate line completely covers the second gate line, the width of the insulating layer is wider than that of the second gate line, and the rear side end of the insulating layer on the second gate line extends in the direction of the third gate line until it is connected to the insulating layer on the third gate line; the insulating layer coated on the third gate line is distributed between the second gate line and the third gate line; Two adjacent second gate lines and the corresponding first gate line and third gate line are surrounded by an insulating layer to form a deposition groove, in which an electron transport layer, a perovskite active layer, a hole transport layer and a metal back electrode are arranged in sequence; the perovskite battery cells formed in the deposition groove are in a parallel structure.

2. The scribe-free perovskite solar cell unit according to claim 1, characterized in that: The thickness of the first gate line, the second gate line or the third gate line is 5-10 μm.

3. The scribe-free perovskite solar cell unit according to claim 1, characterized in that: The width of the first grid line is 1-3 mm; the width of the second grid line is 100-300 μm; and the width of the third grid line is 1-3 mm.

4. The scribe-free perovskite solar cell unit according to claim 1, characterized in that: The thickness of the electron transport layer is 10-50 nm; the thickness of the perovskite active layer is 400-600 nm; and the thickness of the hole transport layer is 600-800 nm.

5. The method for preparing a scribe-free perovskite solar cell unit according to claim 1, characterized in that: The steps include: 1) providing a cleaned transparent conductive substrate according to the designed first area and second area; 2) According to the designed first gate line, second gate line and third gate line structures, silver paste is printed on the surface of the first region conductive layer and the second region respectively, and annealed to obtain silver gate line electrodes; then an insulating layer is provided on the surface of the silver gate line electrodes; 3) Arranging an electron transport layer on the surface of the deposition tank of the substrate obtained in step 2); 4) preparing a perovskite active layer on the electron transport layer; 5) providing a hole transport layer on the perovskite active layer; 6) Preparing a metal back electrode on the hole transport layer to obtain the scribe-free perovskite solar cell unit.

6. The preparation method according to claim 5, characterized in that: The annealing treatment is performed at a temperature of 400-500° C. and for a time of 5-10 minutes.

7. The preparation method according to claim 5, characterized in that: The electron transport layer is prepared by chemical bath deposition method; the hole transport layer is prepared by ultrasonic spray method.

8. The preparation method according to claim 5, characterized in that: The perovskite active layer is prepared by vacuum evaporation process and ultrasonic spray process; the specific preparation steps include: vacuum evaporating a layer of cesium halogen salt on the electron transport layer, then evaporating a layer of lead salt, and then spraying a layer of methylamino salt by ultrasonic spray process, and annealing to generate a perovskite active layer.

9. The preparation method according to claim 8, characterized in that: The methyl imidamine salt spraying process uses a methyl imidamine salt solution, and the solvent used is a composite of n-butanol and N-methyl pyrrolidone.

10. A scribe-free perovskite solar cell module prepared by using the scribe-free perovskite solar cell unit according to any one of claims 1 to 4 or the scribe-free perovskite solar cell unit obtained by the preparation method according to any one of claims 5 to 8, characterized in that: The solar cell comprises a plurality of scribe-free perovskite solar cells connected in series or in parallel.