A hydrophilic and lipophilic ultrafine titanium dioxide and its preparation method and application
Through the hydrophilic and lipophilic modified ultrafine titanium dioxide, the poor compatibility of physical sunscreens and the toxicology of chemical sunscreens are solved, and the excellent anti-ultraviolet effect and good skin feeling of sunscreen are achieved, reducing sensitization. Meet the needs of consumers.
Patent Information
- Application Number
- CN202411038637.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Existing physical sunscreens such as titanium dioxide have an average compatibility with the skin, which leads to poor skin feeling of sunscreen, and chemical sunscreens have toxicological and allergic problems, limiting their application in sunscreen products.
Using hydrophilic and lipophilic ultrafine titanium dioxide, through surface modification treatment, nano-scale titanium dioxide surfactant groups react with diisocyanate-capped lipophilic polyurethane prepolymer and hydrophilic surf modifier to form -NH- CO-NH-bond and -NH-CO-O-bond are grafted to ensure product safety and skin compatibility.
It achieves the excellent, long-lasting and safe anti-UV effect of sunscreen products, excellent skin feeling, reduces sensitization, expands the scope of use, and improves skin health.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of physical sunscreen preparation, and in particular to a hydrophilic and lipophilic ultrafine titanium dioxide and a preparation method and application thereof. Background Art
[0002] The ultraviolet rays in sunlight have a clear destructive effect on human skin. Short-term ultraviolet radiation damage is sunburn and erythema; long-term ultraviolet radiation damage includes the decline of skin self-repair ability, accelerated skin aging, damage to the stratum corneum protective layer, and easy occurrence of capillary dilation, allergies, ecchymosis and other skin problems. Therefore, it is very necessary to choose a good sunscreen with anti-ultraviolet effect, and sunscreen products with excellent sun protection performance are bound to be sought after by consumers.
[0003] At present, the sunscreens in sunscreen products are mainly divided into two categories: chemical sunscreens and physical sunscreens. Chemical sunscreens include benzotriazole anti-ultraviolet agents, benzophenone anti-ultraviolet agents, and triazine anti-ultraviolet agents. Considering the toxicological properties of chemical sunscreens, the chemical sunscreens that are actually maturely used in the cosmetics field are mainly 2-hydroxy-4-methoxybenzophenone UV-9, 2-hydroxy-4-methoxy-5-sulfobenzophenone UV-284, and 2-phenylbenzimidazole-5-sulfonic acid UV-T. Although the above-mentioned chemical sunscreens that are maturely used in the cosmetics field have a good sunscreen effect, their low toxicity problem limits their addition amount in sunscreen products. Not only are there threshold limits on sunscreen performance, but there are also certain allergy problems. It is a limitation and restriction for people with sensitive skin to choose sunscreen products containing chemical sunscreens, and their sunscreen lasting time is also relatively short.
[0004] Physical sunscreens include titanium dioxide, zinc oxide, aluminum oxide, white carbon black, calcium carbonate, zinc phosphate, hydrotalcite, etc. Titanium dioxide and zinc oxide are the most mature in sunscreen products, which have the advantages of being durable and safe. However, titanium dioxide and / or zinc oxide have average compatibility with the skin interface, resulting in average skin feel of such physical sunscreen products. To this end, the inventor provides a hydrophilic and lipophilic ultrafine titanium dioxide and its preparation method and application. Summary of the invention
[0005] In order to solve the technical defects of the above-mentioned prior art, the inventor provides a hydrophilic and lipophilic ultrafine titanium dioxide and a preparation method and application thereof.
[0006] The hydrophilic and lipophilic ultrafine titanium dioxide provided in this application is realized by the following technical scheme:
[0007] A hydrophilic and lipophilic ultrafine titanium dioxide comprises nano-scale titanium dioxide with active amino groups on the surface, wherein the active amino groups on the surface of the nano-scale titanium dioxide react with a diisocyanate-terminated lipophilic polyurethane prepolymer, wherein the diisocyanate groups at one end of the diisocyanate-terminated lipophilic polyurethane prepolymer react with the active amino groups on the surface of the nano-scale titanium dioxide to form -NH-CO-NH-bond grafting connection, and the diisocyanate groups at the other end of the diisocyanate-terminated lipophilic polyurethane prepolymer react with a hydrophilic surface modifier to form -NH-CO-O-bond and / or -NH-CO-NH-bond grafting connection; and the molar amount of the active matrix of the hydrophilic surface modifier is greater than the molar amount of the diisocyanate groups in the diisocyanate-terminated lipophilic polyurethane prepolymer.
[0008] In this application, an excess of hydrophilic surface modifier is used for end-capping treatment, and the hydrophilic and lipophilic ultrafine titanium dioxide surface obtained in the end does not contain -NCO groups, which effectively ensures the safety performance and skin-friendly and anti-sensitizing performance of this application. This application, as a physical sunscreen, gives sunscreen products excellent, long-lasting and safe anti-ultraviolet effects, and this application has good compatibility with the skin. The sunscreen products prepared using it have excellent skin feel and meet the use needs of consumers.
[0009] Preferably, the hydrophilic surface modifier includes at least one of dimethylsilanol hyaluronate, 3-hydroxypropanesulfonic acid sodium salt, sodium hyaluronate, potassium hyaluronate, sodium myristoyl glutamate, sodium cocoyl glutamate, sodium lauroyl glutamate, and dopamine.
[0010] By optimizing the design of the hydrophilic surface modifier, not only can the ultrafine titanium dioxide be given good hydrophilic and lipophilic properties and good compatibility with the skin, but the sunscreen products prepared therewith can also have excellent skin feel, and the allergenicity of the prepared sunscreen products can also be reduced. At the same time, the above-mentioned hydrophilic surface modifier has a certain skin repair effect, which is beneficial to improving skin health.
[0011] Preferably, the diisocyanate used for the end-capping of the oleophilic polyurethane prepolymer includes aromatic isocyanate and / or aliphatic isocyanate and / or alicyclic isocyanate and / or polyethylene glycol end-capped with isocyanate groups; the aliphatic isocyanate is one or more combinations of HDI, TMDI, and XDI; the alicyclic isocyanate is one or more combinations of IPDI, HMDI, and HTDI; the aromatic isocyanate is one or more combinations of MDI, TDI, NDI, and TODI.
[0012] Preferably, the diisocyanate used for capping the oleophilic polyurethane prepolymer is MDI and / or TDI.
[0013] Preferably, the active amino groups on the surface of the nano-scale titanium dioxide react with a diisocyanate-terminated hydrophilic polyurethane prepolymer, the diisocyanate groups at one end of the diisocyanate-terminated hydrophilic polyurethane prepolymer react with the active amino groups on the surface of the nano-scale titanium dioxide to form -NH-CO-NH-bond grafting connection, and the diisocyanate groups at the other end of the diisocyanate-terminated lipophilic polyurethane prepolymer react with a lipophilic surface modifier to form -NH-CO-O-bond and / or -NH-CO-NH-bond grafting connection; the diisocyanate used for the termination of the hydrophilic polyurethane prepolymer is isocyanate-terminated polyethylene glycol and / or IPDI.
[0014] The lipophilic polyurethane prepolymer in the present application is terminated with MDI and / or TDI, which has relatively high reactivity and first reacts with the active amino groups on the surface of nano-scale titanium dioxide to generate -NH-CO-NH-bond grafting connection, while the hydrophilic polyurethane prepolymer is terminated with polyethylene glycol and / or IPDI with relatively low reactivity. After the lipophilic polyurethane prepolymer is consumed by reaction, it is then reacted with the active amino groups on the surface of nano-scale titanium dioxide to generate -NH-CO-NH-bond grafting connection, so that the lipophilic polyurethane chain segments and hydrophilic polyurethane chain segments can be grafted on the surface of nano-scale titanium dioxide, giving the prepared ultrafine titanium dioxide better hydrophilic and lipophilic properties, good compatibility with skin, and the sunscreen products prepared by using the same have excellent skin feel and can have excellent, long-lasting and safe anti-ultraviolet effect.
[0015] Preferably, the lipophilic surface modifier is at least one of an amino-terminated polysiloxane, a hydroxy-terminated polysiloxane, and a C8-C12 alcohol.
[0016] By adopting the above technical solution, the prepared ultrafine titanium dioxide has lower allergenicity, which expands its scope of use.
[0017] The present application provides a method for preparing hydrophilic and lipophilic ultrafine titanium dioxide, which is achieved by the following scheme:
[0018] A method for preparing hydrophilic and lipophilic ultrafine titanium dioxide comprises the following steps:
[0019] Step 1, preparation of nano-sized titanium dioxide having active amino groups on the surface;
[0020] Step 2: Nano-sized titanium dioxide with active amino groups on its surface is dispersed in acetone, and a diisocyanate-terminated oleophilic polyurethane prepolymer and a catalyst are added to react at 75-80° C. for 0.5-1.0 h;
[0021] Step 3, dropwise adding a hydrophilic surface modifier, reacting at 75-80° C. for 0.5-1.0 h, detecting the -NCO content until the -NCO content is 0, filtering, drying, and ball milling to obtain the product.
[0022] Or a method for preparing hydrophilic and lipophilic ultrafine titanium dioxide, comprising the following steps:
[0023] Step 1, preparation of nano-sized titanium dioxide having active amino groups on the surface;
[0024] Step 2: Nano-sized titanium dioxide with active amino groups on its surface is dispersed in acetone, and a diisocyanate-terminated oleophilic polyurethane prepolymer and a catalyst are added to react at 75-80° C. for 0.5-1.0 h;
[0025] Step 3, dropwise adding a hydrophilic surface modifier, reacting at 75-80° C. for 0.5-1.0 h, detecting the -NCO content until the -NCO content is 0, filtering, drying, and ball milling to obtain a semi-finished product;
[0026] Step 4: The obtained semi-finished product is dispersed in acetone, and after ultrasonic dispersion is uniform, a diisocyanate-terminated hydrophilic polyurethane prepolymer and a catalyst are added under magnetic stirring at 160-240 rpm, and the mixture is reacted at 80-85° C. for 0.5-1.0 h. Then, under nitrogen protection and magnetic stirring at 160-240 rpm, a lipophilic surface modifier is added at a rate of 0.1-0.2 g / 10 s. After the addition is completed, the mixture is continued to react at 80-85° C. for 1.5-2 h. After the -NCO content in the detection system is 0, the mixture is cooled to room temperature, and solid powder is obtained by suction filtration under nitrogen protection. The obtained solid powder is rinsed three times with acetone, and then rinsed three times with distilled water, and dried and ball-milled to obtain the finished hydrophilic and lipophilic ultrafine titanium dioxide.
[0027] The preparation method provided in this application is relatively simple, has low difficulty in production implementation, and is easy to realize industrial production. In this application, the ball milling method is used to complete the "unzipping" treatment of some chemically bonded titanium dioxide, thereby improving the fineness of the titanium dioxide finally obtained.
[0028] Preferably, the preparation method of the nano-scale titanium dioxide containing active amino groups on the surface in the step 1 is as follows: the nano-scale titanium dioxide prepared by the sol-gel method is subjected to surface modification treatment with aminosilane to obtain the nano-scale titanium dioxide; the aminosilane is at least one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, and γ-diethylenetriaminopropyltrimethoxysilane.
[0029] By adopting the above technical solution, the production cost of nano-scale titanium dioxide containing active amino groups on the surface can be reduced.
[0030] Preferably, the preparation method of the nano-scale titanium dioxide containing active amino groups on the surface in the step 1 is as follows: first, nano-TiO2 is prepared on a titanium sheet by an anodic oxidation method, and then the titanium sheet with the nano-TiO2 on the surface is placed in a plasma treatment machine, and a nitrogen-hydrogen mixed gas is used for plasma surface treatment for 5-30 minutes to generate active amino groups in the nano-TiO2. Finally, the nano-TiO2 containing active amino groups on the surface of the titanium sheet is washed by ultrasonic vibration for 1-2 hours with ultrapure water, acetone, and anhydrous ethanol respectively, and the nano-TiO2 containing active amino groups on the surface of the titanium sheet falls off, and the titanium sheet is collected and dried to obtain nano-scale titanium dioxide containing active amino groups on the surface.
[0031] By adopting the above technical scheme, more active amino groups can be given to the surface of nano-scale titanium dioxide, which can further improve the hydrophilic and lipophilic properties of the prepared ultrafine titanium dioxide, and has good compatibility with the skin. The sunscreen products prepared therefrom have long-lasting and safe anti-ultraviolet effects and good skin feel, which meet the usage needs of consumers.
[0032] A hydrophilic and lipophilic ultrafine titanium dioxide is used in the field of cosmetics. As a physical sunscreen in sunscreen products, it has an excellent, long-lasting and safe anti-ultraviolet effect. The hydrophilic and lipophilic modified ultrafine titanium dioxide has good compatibility with the skin. Sunscreen products prepared using the hydrophilic and lipophilic ultrafine titanium dioxide have excellent skin feel.
[0033] In summary, this application has the following advantages:
[0034] 1. The present application is applied in the field of cosmetics and is added to sunscreen products as a physical sunscreen agent to give sunscreen products excellent, long-lasting and safe anti-ultraviolet effects. The hydrophilic-lipophilic modified ultrafine titanium dioxide has good compatibility with the skin. The sunscreen products prepared using the hydrophilic-lipophilic ultrafine titanium dioxide have excellent skin feel and meet the needs of consumers.
[0035] 2. The lipophilic polyurethane prepolymer in the present application is terminated with aromatic diisocyanate, which has relatively high reactivity and will first react with the active amino groups on the surface of nano-scale titanium dioxide to produce -NH-CO-NH- bonds for graft connection; while the hydrophilic polyurethane prepolymer is terminated with aliphatic diisocyanate and / or alicyclic diisocyanate and / or polyethylene glycol with isocyanate groups, which has lower reactivity than the lipophilic polyurethane prepolymer. After the lipophilic polyurethane prepolymer is completely reacted and consumed, it will react with the active amino groups on the surface of nano-scale titanium dioxide to produce -NH-CO-NH- bonds for graft connection, so that the lipophilic polyurethane chain segments and hydrophilic polyurethane chain segments can be grafted on the surface of nano-scale titanium dioxide, giving the prepared ultrafine titanium dioxide better hydrophilic and lipophilic properties and good compatibility with the skin. The sunscreen products prepared by using the prepolymer have excellent skin feel and can play an excellent, long-lasting and safe anti-ultraviolet effect.
[0036] 3. The preparation method provided in this application is relatively simple, the difficulty of production implementation is relatively low, and it is easy to realize industrial production. DETAILED DESCRIPTION
[0037] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.
[0038] Example
[0039] A hydrophilic and lipophilic ultrafine titanium dioxide comprises nano-sized titanium dioxide with active amino groups on the surface, the active amino groups on the surface of the nano-sized titanium dioxide react with diisocyanate-terminated lipophilic polyurethane prepolymer, the diisocyanate groups at one end of the diisocyanate-terminated lipophilic polyurethane prepolymer react with the active amino groups on the surface of the nano-sized titanium dioxide to form -NH-CO-NH-bond grafting connection, and the diisocyanate groups at the other end of the diisocyanate-terminated lipophilic polyurethane prepolymer react with a hydrophilic surface modifier to form -NH-CO-O-bond and / or -NH-CO-NH-bond grafting connection. The molar amount of the active matrix of the hydrophilic surface modifier is greater than the molar amount of the diisocyanate groups in the diisocyanate-terminated lipophilic polyurethane prepolymer.
[0040] The hydrophilic surface modifier includes at least one of dimethylsilanol hyaluronate, 3-hydroxypropanesulfonic acid sodium salt, sodium hyaluronate, potassium hyaluronate, sodium myristoyl glutamate, sodium cocoyl glutamate, sodium lauroyl glutamate and dopamine.
[0041] The diisocyanate used for the end-capping of the oleophilic polyurethane prepolymer includes aromatic isocyanate and / or aliphatic isocyanate and / or alicyclic isocyanate and / or polyethylene glycol end-capped with an isocyanate group.
[0042] The aliphatic isocyanate is one or more combinations of HDI, TMDI and XDI.
[0043] The alicyclic isocyanate is one or more combinations of IPDI, HMDI and HTDI.
[0044] The aromatic isocyanate is one or more combinations of MDI, TDI, NDI and TODI.
[0045] Preferably, the diisocyanate used for capping the oleophilic polyurethane prepolymer is MDI and / or TDI.
[0046] In order to further improve the hydrophilicity and lipophilicity of ultrafine titanium dioxide, the active amino groups on the surface of nano-scale titanium dioxide react with the hydrophilic polyurethane prepolymer terminated with diisocyanate, the diisocyanate groups at one end of the hydrophilic polyurethane prepolymer terminated with diisocyanate react with the active amino groups on the surface of the nano-scale titanium dioxide to form -NH-CO-NH-bond grafting connection, and the diisocyanate groups at the other end of the lipophilic polyurethane prepolymer terminated with diisocyanate react with the lipophilic surface modifier to form -NH-CO-O-bond and / or -NH-CO-NH-bond grafting connection.
[0047] The diisocyanate used for the end-capping of the hydrophilic polyurethane prepolymer is polyethylene glycol and / or IPDI end-capped with an isocyanate group.
[0048] The lipophilic surface modifier is at least one of an amino-terminated polysiloxane, a hydroxy-terminated polysiloxane, and a C8-C12 alcohol.
[0049] The lipophilic polyurethane prepolymer in the present application is terminated with aromatic diisocyanate, which has relatively high reactivity and will first react with the active amino groups on the surface of nano-scale titanium dioxide to produce -NH-CO-NH- bonds for graft connection; while the hydrophilic polyurethane prepolymer is terminated with aliphatic diisocyanate and / or alicyclic diisocyanate and / or polyethylene glycol with isocyanate groups, which has lower reactivity than the lipophilic polyurethane prepolymer. After the lipophilic polyurethane prepolymer is completely reacted and consumed, it will react with the active amino groups on the surface of nano-scale titanium dioxide to produce -NH-CO-NH- bonds for graft connection, so that the lipophilic polyurethane chain segments and hydrophilic polyurethane chain segments can be grafted on the surface of nano-scale titanium dioxide, giving the prepared ultrafine titanium dioxide better hydrophilic and lipophilic properties and good compatibility with the skin. The sunscreen products prepared by using the prepolymer have excellent skin feel and can play an excellent, long-lasting and safe anti-ultraviolet effect.
[0050] A method for preparing hydrophilic and lipophilic ultrafine titanium dioxide comprises the following steps:
[0051] Step 1, preparation of nano-sized titanium dioxide having active amino groups on the surface;
[0052] Preparation method 1: Nano-sized titanium dioxide prepared by a sol-gel method is prepared by surface modification of the prepared nano-sized titanium dioxide with aminosilane; the aminosilane is at least one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, and γ-diethylenetriaminopropyltrimethoxysilane;
[0053] Preparation method 2: First, prepare nano-TiO2 on a titanium sheet by anodizing, then place the titanium sheet with nano-TiO2 on the surface in a plasma treatment machine, use nitrogen-hydrogen mixed gas for plasma surface treatment for 5-30 minutes, and the nano-TiO2 generates active amino groups. Finally, use ultrapure water, acetone, and anhydrous ethanol to ultrasonically clean for 1-2 hours, and the nano-TiO2 with active amino groups on the surface of the titanium sheet falls off. The titanium sheet is collected and dried to obtain nano-grade titanium dioxide with active amino groups on the surface.
[0054] Step 2: Nano-sized titanium dioxide with active amino groups on its surface is dispersed in acetone, and a diisocyanate-terminated oleophilic polyurethane prepolymer and a catalyst are added to react at 75-80° C. for 0.5-1.0 h;
[0055] Step 3, dropwise adding a hydrophilic surface modifier, reacting at 75-80°C for 0.5-1.0h, detecting the -NCO content until the -NCO content is 0, filtering, drying, and ball milling to obtain hydrophilic and lipophilic ultrafine titanium dioxide.
[0056] The prepared hydrophilic and lipophilic ultrafine titanium dioxide is used in the cosmetics field and is added to sunscreen products as a physical sunscreen agent to give sunscreen products excellent, long-lasting and safe anti-ultraviolet effects. The hydrophilic and lipophilic modified ultrafine titanium dioxide has good compatibility with the skin. Sunscreen products prepared using the above hydrophilic and lipophilic ultrafine titanium dioxide have excellent skin feel and meet the needs of consumers.
[0057] Embodiment 1: A hydrophilic and lipophilic ultrafine titanium dioxide comprises nano-sized titanium dioxide having active amino groups on its surface, an active amino group on the surface of the nano-sized titanium dioxide and an lipophilic polyurethane prepolymer terminated with a highly active diisocyanate, and an active amino group on the surface of the nano-sized titanium dioxide and a hydrophilic polyurethane prepolymer terminated with a low active diisocyanate.
[0058] The diisocyanate group at one end of the highly active diisocyanate (MDI)-terminated lipophilic polyurethane prepolymer reacts with the active amino group on the surface of nano-sized titanium dioxide to form a -NH-CO-NH- bond graft connection, while the diisocyanate group at the other end of the highly active diisocyanate (MDI)-terminated lipophilic polyurethane prepolymer reacts with the hydrophilic surface modifier to form a -NH-CO-O- bond graft connection. The hydrophilic surface modifier is sodium hyaluronate.
[0059] The diisocyanate group at one end of the hydrophilic polyurethane prepolymer terminated with low-activity diisocyanate (IPDI) reacts with the active amino group on the surface of nano-sized titanium dioxide to form -NH-CO-NH- bond grafting connection, and the diisocyanate group at the other end of the lipophilic polyurethane prepolymer terminated with low-activity diisocyanate (IPDI) reacts with the lipophilic surface modifier to form -NH-CO-O- bond grafting connection. The lipophilic surface modifier is a hydroxyl-terminated polysiloxane, specifically the alcohol hydroxyl mono-terminated long-chain alkyl silicone oil IOTA 8861 produced by Anhui Iota Silicone Oil Co., Ltd., with an average molecular weight of 1300 and a hydroxyl value of 40.5KOHmg / g.
[0060] A method for preparing hydrophilic and lipophilic ultrafine titanium dioxide comprises the following steps:
[0061] Step 1, preparation of nano-scale titanium dioxide with active amino groups on the surface: first, prepare nano-scale titanium dioxide by conventional sol-gel method: 28g of TiCl4 solution with a mass concentration of 25% and 0.5L of sodium hydroxide aqueous solution with a mass concentration of 20wt% are mixed at 400rpm, and then 56g of TiCl4 solution with a mass concentration of 25% is added at a dropping speed of 1g / 10s, reacted for 5h, and then aged for 36h to obtain aged titanium sol. The solid product after filtration and washing is first heated in a muffle furnace at a heating rate of 100 ℃ to obtain an aged titanium sol. The temperature was raised to 400°C at a rate of 4°C / min and calcined for 0.5h, and then the temperature was raised to 940°C at a rate of 8°C / min and calcined for 1h. After naturally cooling to room temperature, nano-scale titanium dioxide was obtained. 5g of the obtained nano-scale titanium dioxide was placed in 100mL of a 2wt% KH540 aqueous solution, and ultrasonically dispersed for 30min at an ultrasonic frequency of 44kHz and a power of 1200W. After the ultrasonic dispersion was completed, the nano-scale titanium dioxide was taken out and dried in a transposed oven at 60°C for 4h to obtain nano-scale titanium dioxide with active amino groups on the surface.
[0062] The preparation method of a highly active diisocyanate (MDI) terminated oleophilic polyurethane prepolymer is as follows: accurately measuring 280g of polytetrahydrofuran diol with a molecular weight of 2000, 284g of double-terminal alcohol hydroxyl long-chain alkyl silicone oil IOTA-8865H, 5g of antioxidant BHT, 0.08g of bismuth isooctanoate, 500g of dimethylformamide DMF, 300g of acetone and 84.1g of hexamethylene diisocyanate prepolymer HDI, reacting at 88°C until the viscosity reaches 6000-8000mPa·s / 25°C, adding 7.6g of MDI-50 for termination, adjusting the temperature to 70°C for reaction for 30min, and cooling to room temperature to obtain the prepolymer;
[0063] The preparation method of a hydrophilic polyurethane prepolymer terminated with low-activity diisocyanate (IPDI) is as follows: accurately measuring 240g of polytetrahydrofuran diol with a molecular weight of 2000, 100g of polycarbonate diol with a molecular weight of 1000, 4g of antioxidant BHT, 0.12g of bismuth isooctanoate, 400g of dimethylformamide DMF, 200g of acetone and 84.1g of hexamethylene diisocyanate prepolymer HDI are prepolymerized, reacting at 88°C until the viscosity reaches 6000-8000mPa·s / 25°C, and then end-capping with 7.8g of isophorone diisocyanate IPDI at a blocking temperature of 78°C for 45min, adjusting the pH value to neutral with ammonia water, and cooling to room temperature to obtain the prepolymer;
[0064] Step 2: Under nitrogen protection, weigh 5 g of the nano-scale titanium dioxide with active amino groups on the surface prepared in step 1 and disperse it in 200 mL of acetone, add 2.18 g of the highly active oleophilic polyurethane prepolymer of diisocyanate (MDI) prepared in step 1 and 0.02 g of tetrabutyl titanate under magnetic stirring at 200 rpm, and heat to 75° C. to react for 0.5 h;
[0065] Step three, adjust the temperature to 80°C, under nitrogen protection and 200rpm magnetic stirring, add 4g of sodium hyaluronate (Shandong Liyang Biotechnology Co., Ltd., cosmetic grade molecular weight 3000) at 0.02g / 5s, continue to react at 80°C for 0.5h after the addition is completed, and cool to room temperature after the -NCO content in the detection system is 0. Filter under nitrogen protection to obtain solid powder, then rinse with acetone three times, and after drying, place the powder in a planetary ball mill for wet ball milling at 160rpm / 2h, dry, and set aside.
[0066] Step 4: Under nitrogen protection, the powder obtained in step 3 is dispersed in 200 mL of acetone, and ultrasonic dispersion is performed for 30 min at an ultrasonic frequency of 44 kHz and a power of 1200 W. Then, 2.31 g of the hydrophilic polyurethane prepolymer of low-activity diisocyanate (IPDI) prepared in step 1 and 0.03 g of tetrabutyl titanate are added under magnetic stirring at 200 rpm. The temperature is raised to 80 ° C and reacted for 45 min. The temperature is adjusted to 80 ° C. Under nitrogen protection and magnetic stirring at 200 rpm, 6.5 g of alcohol hydroxyl mono-terminated long-chain alkyl silicone oil IOTA is added dropwise at a rate of 0.2 g / 10 s. 8861, after the addition is completed, the reaction is continued at 80°C for 2h. After the -NCO content in the detection system is 0, it is cooled to room temperature and filtered under nitrogen protection to obtain a solid powder. The obtained solid powder is rinsed three times with acetone and then rinsed three times with distilled water. After drying, the powder is placed in a planetary ball mill for wet ball milling at 160rpm / 2h. After drying, hydrophilic and lipophilic ultrafine titanium dioxide can be obtained.
[0067] The difference between Example 2 and Example 1 is that the hydrophilic surface modifier is dimethylsilanol hyaluronate. The difference in the preparation method of hydrophilic and lipophilic ultrafine titanium dioxide is that: Step 3, adjust the temperature to 80°C, under nitrogen protection and 200rpm magnetic stirring, add 4.8g of dimethylsilanol hyaluronate (CAS No.: 135507-00-5) at 0.02g / 5s, continue to react at 80°C for 0.5h after the addition is completed, cool to room temperature after the -NCO content in the detection system is 0, filter under nitrogen protection to obtain solid powder, and rinse the obtained solid powder with acetone three times for standby use.
[0068] The difference between Example 3 and Example 1 is that the hydrophilic surface modifier is 3-hydroxypropanesulfonic acid sodium salt. The difference in the preparation method of hydrophilic and lipophilic ultrafine titanium dioxide is that: Step 3, adjust the temperature to 80°C, under nitrogen protection and 200rpm magnetic stirring, add 0.24g of 3-hydroxypropanesulfonic acid sodium salt (CAS No.: 3542-44-7) at 0.02g / 5s, continue to react at 80°C for 0.5h after the addition is completed, cool to room temperature after the -NCO content in the detection system is 0, filter under nitrogen protection to obtain solid powder, rinse the obtained solid powder with acetone three times, and place the powder in a planetary ball mill for wet ball milling at 160rpm / 2h after drying, and dry it for use.
[0069] The difference between Example 4 and Example 1 is that the hydrophilic surface modifier is sodium myristoyl glutamate. The difference in the preparation method of hydrophilic and lipophilic ultrafine titanium dioxide is that: Step 3, adjust the temperature to 80°C, under nitrogen protection and 200rpm magnetic stirring, add 0.49g of sodium myristoyl glutamate (CAS No.: 38517-37-2) at 0.02g / 5s, continue to react at 80°C for 0.5h after the addition is completed, cool to room temperature after the -NCO content in the detection system is 0, filter under nitrogen protection to obtain solid powder, rinse the obtained solid powder with acetone three times, and place the powder in a planetary ball mill for wet ball milling at 160rpm / 2h after drying, and dry it for use.
[0070] The difference between Example 5 and Example 1 is that the hydrophilic surface modifier is sodium cocoyl glutamate. The difference in the preparation method of hydrophilic and lipophilic ultrafine titanium dioxide is that: Step 3, adjust the temperature to 80°C, under nitrogen protection and 200rpm magnetic stirring, add 0.25g of sodium cocoyl glutamate (CAS No.: 68187-32-6) at 0.02g / 5s, continue to react at 80°C for 0.5h after the addition is completed, cool to room temperature after the -NCO content in the detection system is 0, filter under nitrogen protection to obtain solid powder, rinse the obtained solid powder with acetone three times, and place the powder in a planetary ball mill for wet ball milling at 160rpm / 2h after drying, and dry it for use.
[0071] The difference between Example 6 and Example 1 is that the hydrophilic surface modifier is sodium lauroyl glutamate. The difference in the preparation method of hydrophilic and lipophilic ultrafine titanium dioxide is that: Step 3, adjust the temperature to 80°C, under nitrogen protection and 200rpm magnetic stirring, add 0.46g of sodium cocoyl glutamate (CAS No.: 29923-31-7) at 0.02g / 5s, continue to react at 80°C for 0.5h after the addition is completed, cool to room temperature after the -NCO content in the detection system is 0, filter under nitrogen protection to obtain solid powder, rinse the obtained solid powder with acetone three times, and place the powder in a planetary ball mill for wet ball milling at 160rpm / 2h after drying, and dry it for use.
[0072] The difference between Example 7 and Example 1 is that the hydrophilic surface modifier is dopamine. The difference in the preparation method of hydrophilic and lipophilic ultrafine titanium dioxide is that: Step 3, adjust the temperature to 80°C, under nitrogen protection and 200rpm magnetic stirring, add 0.2g of dopamine (CAS No.: 51-61-6) at 0.02g / 5s, continue to react at 80°C for 0.5h after the addition is completed, cool to room temperature after the -NCO content in the detection system is 0, filter under nitrogen protection to obtain solid powder, and rinse the obtained solid powder with acetone three times for standby use.
[0073] The difference between Example 8 and Example 1 is that the lipophilic surface modifier is a hydroxyl-terminated polysiloxane, specifically FM-0411 hydroxyl-terminated polysiloxane from Japan JNC, Mn=1000, CAS No.: 191920-47-5.
[0074] The difference in the preparation method of hydrophilic and lipophilic ultrafine titanium dioxide is that: Step 4, under nitrogen protection, the solid powder obtained in step 3 is dispersed in 200 mL of acetone, 2.31 g of the hydrophilic polyurethane prepolymer of low-activity diisocyanate (IPDI) prepared in step 1 and 0.03 g of tetrabutyl titanate are added under 200 rpm magnetic stirring, the temperature is raised to 80 ° C and the reaction is carried out for 45 minutes, the temperature is adjusted to 80 ° C, and the mixture is stirred under nitrogen protection and 200 rpm magnetic stirring. Stir, add 5 g of FM-0411 hydroxyl-terminated polysiloxane at a rate of 0.2 g / 10s, continue to react at 80°C for 2 h, detect that the -NCO content in the system is 0, then cool to room temperature, filter under nitrogen protection to obtain solid powder, rinse the solid powder three times with acetone, then rinse three times with distilled water, and after drying, place the powder in a planetary ball mill for wet ball milling at 160 rpm / 2 h, and dry to obtain hydrophilic and lipophilic ultrafine titanium dioxide.
[0075] The difference between Example 9 and Example 1 is that the lipophilic surface modifier is an amino-terminated polysiloxane, specifically FM-3311 amino-terminated polysiloxane from Japan JNC, Mn=1000, CAS No.: 106214-84-0.
[0076] The difference in the preparation method of hydrophilic and lipophilic ultrafine titanium dioxide is that: Step 4, under nitrogen protection, the solid powder obtained in step 3 is dispersed in 200 mL of acetone, 2.31 g of the hydrophilic polyurethane prepolymer of low-activity diisocyanate (IPDI) prepared in step 1 and 0.03 g of tetrabutyl titanate are added under 200 rpm magnetic stirring, the temperature is raised to 80 ° C and the reaction is carried out for 45 minutes, the temperature is adjusted to 80 ° C, and the mixture is stirred under nitrogen protection and 200 rpm magnetic stirring. Stir, add 5 g of FM-3311 amino-terminated polysiloxane at a rate of 0.2 g / 10s, continue to react at 80°C for 2 h, detect that the -NCO content in the system is 0, then cool to room temperature, filter under nitrogen protection to obtain solid powder, rinse the solid powder three times with acetone, then rinse three times with distilled water, and after drying, place the powder in a planetary ball mill for wet ball milling at 160 rpm / 2 h, and dry to obtain hydrophilic and lipophilic ultrafine titanium dioxide.
[0077] The difference between Example 10 and Example 1 is that the lipophilic surface modifier is decanol (CAS No.: 1502-05-2).
[0078] The difference in the preparation method of hydrophilic and lipophilic ultrafine titanium dioxide is that: Step 4, under nitrogen protection, disperse the solid powder obtained in step 3 in 200 mL of acetone, add 2.31 g of the hydrophilic polyurethane prepolymer of low-activity diisocyanate (IPDI) prepared in step 1 and 0.03 g of tetrabutyl titanate under 200 rpm magnetic stirring, heat to 80°C and react for 45 minutes, adjust the temperature to 80°C, under nitrogen protection and 200 rpm magnetic stirring, add 0.78 g of decanol at 0.02 g / 5s, continue to react at 80°C for 2 hours after the addition is completed, cool to room temperature after the -NCO content in the detection system is 0, filter under nitrogen protection to obtain solid powder, rinse the obtained solid powder with acetone three times, and then rinse with distilled water three times. After drying, the powder is placed in a planetary ball mill for wet ball milling at 160 rpm / 2h, and dried to obtain hydrophilic and lipophilic ultrafine titanium dioxide.
[0079] The difference between Example 11 and Example 1 is that a hydrophilic and lipophilic ultrafine titanium dioxide includes nano-sized titanium dioxide with active amino groups on the surface, and the active amino groups on the surface of the nano-sized titanium dioxide react with the lipophilic polyurethane prepolymer terminated with high-activity diisocyanate. The diisocyanate group at one end of the lipophilic polyurethane prepolymer terminated with high-activity diisocyanate (MDI) reacts with the active amino groups on the surface of the nano-sized titanium dioxide to form a -NH-CO-NH-bond graft connection, and the diisocyanate group at the other end of the lipophilic polyurethane prepolymer terminated with high-activity diisocyanate (MDI) reacts with the hydrophilic surface modifier to form a -NH-CO-O-bond graft connection, and the diisocyanate group at the other end of the lipophilic polyurethane prepolymer terminated with high-activity diisocyanate (MDI) reacts with the lipophilic surface modifier to form a -NH-CO-O-bond graft connection. The hydrophilic surface modifier is sodium hyaluronate. The lipophilic surface modifier is FM-0411 hydroxyl-terminated polysiloxane from Japan JNC.
[0080] A method for preparing hydrophilic and lipophilic ultrafine titanium dioxide comprises the following steps:
[0081] Step 1, preparation of nano-scale titanium dioxide with active amino groups on the surface: first, prepare nano-scale titanium dioxide by conventional sol-gel method: 28g of TiCl4 solution with a mass concentration of 25% and 0.5L of sodium hydroxide aqueous solution with a mass concentration of 20wt% are mixed at 400rpm, and then 56g of TiCl4 solution with a mass concentration of 25% is added at a dropping speed of 1g / 10s, reacted for 5h, and then aged for 36h to obtain aged titanium sol. The solid product after filtration and washing is first heated in a muffle furnace at a heating rate of 100 ℃ to obtain an aged titanium sol. The temperature was raised to 400°C at a rate of 4°C / min and calcined for 0.5h, and then the temperature was raised to 940°C at a rate of 8°C / min and calcined for 1h. After naturally cooling to room temperature, nano-scale titanium dioxide was obtained. 5g of the obtained nano-scale titanium dioxide was placed in 100mL of a 2wt% KH540 aqueous solution, and ultrasonically dispersed for 30min at an ultrasonic frequency of 44kHz and a power of 1200W. After the ultrasonic dispersion was completed, the nano-scale titanium dioxide was taken out and dried in a transposed oven at 60°C for 4h to obtain nano-scale titanium dioxide with active amino groups on the surface.
[0082] The preparation method of a highly active diisocyanate (MDI) terminated oleophilic polyurethane prepolymer is as follows: accurately measuring 280g of polytetrahydrofuran diol with a molecular weight of 2000, 284g of double-terminal alcohol hydroxyl long-chain alkyl silicone oil IOTA-8865H, 5g of antioxidant BHT, 0.08g of bismuth isooctanoate, 500g of dimethylformamide DMF, 300g of acetone and 84.1g of hexamethylene diisocyanate prepolymer HDI, reacting at 88°C until the viscosity reaches 6000-8000mPa·s / 25°C, adding 7.6g of MDI-50 for termination, adjusting the temperature to 70°C for reaction for 30min, and cooling to room temperature to obtain the prepolymer;
[0083] Step 2: Under nitrogen protection, weigh 5 g of the nano-scale titanium dioxide with active amino groups on the surface prepared in step 1 and disperse it in 200 mL of acetone, add 2.18 g of the highly active oleophilic polyurethane prepolymer of diisocyanate (MDI) prepared in step 1 and 0.02 g of tetrabutyl titanate under magnetic stirring at 200 rpm, and heat to 75° C. to react for 0.5 h;
[0084] Step three, adjust the temperature to 80°C, under nitrogen protection and 200rpm magnetic stirring, add 2g of sodium hyaluronate (Shandong Liyang Biotechnology Co., Ltd., cosmetic grade molecular weight 3000) at 0.02g / 5s, continue to react at 80°C for 0.5h after the addition is completed, then add 2.5g of FM-0411 hydroxyl-terminated polysiloxane, continue to react at 80°C for 0.5h after the addition is completed, and cool to room temperature after the -NCO content in the detection system is 0. Filter under nitrogen protection to obtain solid powder, then rinse with acetone three times, and then rinse with distilled water three times. After drying, the powder is placed in a planetary ball mill for wet ball milling at 160rpm / 2h, and dried to obtain hydrophilic and lipophilic ultrafine titanium dioxide.
[0085] The difference between Example 12 and Example 1 is: Step 1, preparation of nano-scale titanium dioxide containing active amino groups on the surface: first, nano-TiO2 is prepared on a titanium sheet by anodizing method, at 25°C, a titanium sheet is used as an anode, a nickel sheet is used as a cathode, an ethylene glycol solution with a mass fraction of 0.5% ammonium chloride and a volume fraction of 1% ultrapure water is used as an electrolyte, the control voltage is 40V, and the electrolytic oxidation treatment is performed for 40 minutes to produce nano-TiO2 on the surface of the titanium sheet; then the titanium sheet containing nano-TiO2 on the surface is placed in a plasma treatment machine, and a nitrogen-hydrogen mixed gas (the volume ratio of nitrogen to hydrogen is 4:1) is used for plasma surface treatment for 0.5h, and the nano-TiO2 generates active amino groups. Finally, the nano-TiO2 containing active amino groups on the surface of the titanium sheet is washed with ultrapure water, acetone, and anhydrous ethanol for 1h, respectively, with an ultrasonic frequency of 80kHz and an ultrasonic power of 1600W, and the nano-TiO2 containing active amino groups on the surface of the titanium sheet falls off, and is collected and dried to obtain nano-scale titanium dioxide containing active amino groups on the surface.
[0086] The difference between Comparative Example 1 and Example 1 is that the preparation method of ultrafine titanium dioxide is as follows: first, nano-scale titanium dioxide is prepared by conventional sol-gel method: 28g of TiCl4 solution with a mass concentration of 25% and 0.5L of sodium hydroxide aqueous solution with a mass concentration of 20wt% are mixed at 400rpm, and then 56g of TiCl4 solution with a mass concentration of 25% is added at a dropping speed of 1g / 10s, reacted for 5h, and then aged for 36h to obtain aged titanium sol. The solid product after filtration and washing is first heated in a muffle furnace with The temperature was raised to 400°C at a rate of 4°C / min and calcined for 0.5h, and then raised to 940°C at a rate of 8°C / min and calcined for 1h. After naturally cooling to room temperature, nano-scale titanium dioxide was obtained. 5g of the obtained nano-scale titanium dioxide was placed in 100mL of 2wt% KH540 aqueous solution, and ultrasonically dispersed for 30min at an ultrasonic frequency of 44kHz and a power of 1200W. After the ultrasonic dispersion was completed, the product was taken out and dried in a transposed oven at 60°C for 4h to obtain nano-scale titanium dioxide with hydrophilic and lipophilic effects.
[0087] The performance test standard is in accordance with GB 27599-2011 Titanium Dioxide for Cosmetics. 1. The water-absorbance measurement method is: dissolve 1% titanium dioxide in water, stir it thoroughly, and measure the absorbance of the solution after standing for 30 minutes. 2. The ultraviolet absorption capacity detection method is: according to G = 0.5g / m 2 The viscose film was prepared under the conditions of , and the transmittance of UVA (wavelength 320nm) and ultraviolet light with a radiation intensity of 50W / m 2 through the viscose film was tested. The ultraviolet transmittance value of the blank viscose film was 74.5%.
[0088] Table 1: Test parameters of hydrophilic and lipophilic ultrafine titanium dioxide in Examples 1-12 and Comparative Example 1-1
[0089]
[0090] The hydrophilic and lipophilic ultrafine titanium dioxide in Examples 1-12 and Comparative Example 1-1 was used to prepare a test cosmetic sunscreen lotion. The preparation method of the test cosmetic sunscreen lotion is as follows: 5 g of hydrophilic and lipophilic ultrafine titanium dioxide was mixed with 93 g of deionized water at 500 rpm for 15 min, and then 2 g of polyvinyl alcohol was added, and then the mixture was mixed at 500 rpm for 15 min, and 25 g of polydimethylsiloxane was added, and the mixture was ultrasonically treated for 20 min at an ultrasonic frequency of 44 Hz and an ultrasonic power of 600 W, and finally placed in a homogenizer for homogenization and emulsification at a speed of 12000 rpm for 15 min to obtain an ultrafine titanium dioxide sunscreen lotion product.
[0091] The specific test method for UV shielding effect is as follows: Test the cosmetic sunscreen lotion and evaluate the UV shielding effect of the sunscreen lotion by measuring the UV transmittance. Specifically, apply the test cosmetic sunscreen lotion to a high-transmittance quartz glass slide to make the area 5×10cm and the thickness 50μm. Fix a UV spotlight 10cm above the UV irradiator, and place each sample quartz glass slide 1cm above the UV irradiator probe. Use a blank high-transmittance quartz glass slide as a blank control. The calculation method is: UV transmittance = sample group UV intensity / blank control UV intensity × 100%, and the specific UV shielding effect is shown in Table 2.
[0092] Table 2: UV shielding effect test parameters of cosmetic sunscreen lotions prepared using the hydrophilic and lipophilic ultrafine titanium dioxide in Examples 1-12 and Comparative Example 1-1
[0093] UV transmittance (%) Example 1 8.31 Example 2 8.09 Example 3 8.71 Example 4 7.87 Example 5 8.15 Example 6 8.07 Example 7 8.41 Example 8 8.14 Example 9 8.72 Example 10 9.24 Embodiment 11 9.67 Example 12 7.69 Comparative Example 1 12.84
[0094] Consumer evaluation: 10 volunteers were tested. Test method: Each cosmetic sunscreen lotion was used at a standard dosage of 2 mg / cm 2 , that is, 0.8 g (mL) was applied to the back of the volunteer's hand, and then the application performance was evaluated based on the usage experience. See Table 3 for details.
[0095] Table 3: Consumer test parameters of cosmetic sunscreen lotions prepared using the hydrophilic and lipophilic ultrafine titanium dioxide in Examples 1-12 and Comparative Example 1-1
[0096]
[0097] It can be seen from Examples 1-12 and Comparative Example 1 and Tables 1-3 that the present application, as a physical sunscreen, imparts excellent, long-lasting and safe anti-ultraviolet effects to sunscreen products, and the present application has good compatibility with the skin. The sunscreen products prepared using the present application have excellent skin feel and meet the use needs of consumers.
[0098] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A hydrophilic and lipophilic ultrafine titanium dioxide, characterized in that: The invention comprises nano-scale titanium dioxide with active amino groups on the surface, wherein the active amino groups on the surface of the nano-scale titanium dioxide are connected with a diisocyanate-terminated oleophilic polyurethane prepolymer, the diisocyanate groups at one end of the diisocyanate-terminated oleophilic polyurethane prepolymer react with the active amino groups on the surface of the nano-scale titanium dioxide to form -NH-CO-NH-bond graft connection, and the diisocyanate groups at the other end of the diisocyanate-terminated oleophilic polyurethane prepolymer react with a hydrophilic surface modifier to form -NH-CO-O-bond and / or -NH-CO-NH-bond graft connection; the molar amount of the active matrix of the hydrophilic surface modifier is greater than the molar amount of the diisocyanate groups in the diisocyanate-terminated oleophilic polyurethane prepolymer; the diisocyanate used for the end-capping of the oleophilic polyurethane prepolymer is MDI and / or TDI; The active amino groups on the surface of the nano-scale titanium dioxide are connected with the hydrophilic polyurethane prepolymer terminated with diisocyanate, the diisocyanate groups at one end of the hydrophilic polyurethane prepolymer terminated with diisocyanate react with the active amino groups on the surface of the nano-scale titanium dioxide to form -NH-CO-NH-bond graft connection, the diisocyanate groups at the other end of the hydrophilic polyurethane prepolymer terminated with diisocyanate react with the lipophilic surface modifier to form -NH-CO-O-bond and / or -NH-CO-NH-bond graft connection; the diisocyanate used for the termination of the hydrophilic polyurethane prepolymer is polyethylene glycol and / or IPDI terminated with isocyanate groups.
2. The hydrophilic and lipophilic ultrafine titanium dioxide according to claim 1, characterized in that: The hydrophilic surface modifier includes at least one of dimethylsilanol hyaluronate, 3-hydroxypropanesulfonic acid sodium salt, sodium hyaluronate, potassium hyaluronate, sodium myristoyl glutamate, sodium cocoyl glutamate, sodium lauroyl glutamate and dopamine.
3. The hydrophilic and lipophilic ultrafine titanium dioxide according to claim 1, characterized in that: The lipophilic surface modifier is at least one of amino-terminated polysiloxane, hydroxyl-terminated polysiloxane, and C8-C12 alcohol.
4. A method for preparing the hydrophilic and lipophilic ultrafine titanium dioxide according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1, preparation of nano-sized titanium dioxide having active amino groups on the surface; Step 2: Nano-sized titanium dioxide with active amino groups on its surface is dispersed in acetone, and a diisocyanate-terminated oleophilic polyurethane prepolymer and a catalyst are added to react at 75-80° C. for 0.5-1.0 h; Step 3, dropwise adding a hydrophilic surface modifier, reacting at 75-80° C. for 0.5-1.0 h, detecting the -NCO content until the -NCO content is 0, filtering, drying, and ball milling to obtain a semi-finished product; Step 4: The obtained semi-finished product is dispersed in acetone, and after ultrasonic dispersion is uniform, a diisocyanate-terminated hydrophilic polyurethane prepolymer and a catalyst are added under magnetic stirring at 160-240 rpm, and the mixture is reacted at 80-85° C. for 0.5-1.0 h. Then, under nitrogen protection and magnetic stirring at 160-240 rpm, a lipophilic surface modifier is added at a rate of 0.1-0.2 g / 10 s. After the addition is completed, the mixture is continued to react at 80-85° C. for 1.5-2 h. After the -NCO content in the detection system is 0, the mixture is cooled to room temperature, and solid powder is obtained by suction filtration under nitrogen protection. The obtained solid powder is rinsed three times with acetone, and then rinsed three times with distilled water, and dried and ball-milled to obtain the finished hydrophilic and lipophilic ultrafine titanium dioxide.
5. The method for preparing a hydrophilic and lipophilic ultrafine titanium dioxide according to claim 4, characterized in that: The preparation method of the nano-scale titanium dioxide containing active amino groups on the surface in the step 1 is as follows: the nano-scale titanium dioxide prepared by the sol-gel method is surface-modified by aminosilane to obtain the nano-scale titanium dioxide; the aminosilane is at least one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, and γ-diethylenetriaminopropyltrimethoxysilane.
6. The method for preparing a hydrophilic and lipophilic ultrafine titanium dioxide according to claim 4, characterized in that: The preparation method of the nano-scale titanium dioxide with active amino groups on the surface in the step 1 is as follows: first, nano-TiO2 is prepared on a titanium sheet by an anodic oxidation method, and then the titanium sheet with the nano-TiO2 on the surface is placed in a plasma treatment machine, and a nitrogen-hydrogen mixed gas is used for plasma surface treatment for 5-30 minutes to generate active amino groups in the nano-TiO2. Finally, the nano-TiO2 with active amino groups on the surface of the titanium sheet is washed by ultrasonic vibration for 1-2 hours with ultrapure water, acetone, and anhydrous ethanol respectively, so that the nano-TiO2 with active amino groups on the surface of the titanium sheet falls off, and the nano-scale titanium dioxide with active amino groups on the surface is collected and dried to obtain the nano-scale titanium dioxide with active amino groups on the surface.
7. Use of the hydrophilic and lipophilic ultrafine titanium dioxide according to any one of claims 1 to 3 in the preparation of physical sunscreen products in the cosmetics field.