A method for preparing a semi-solid magnesium alloy with low porosity
By heating, rotating and tilting the semi-solid magnesium alloy slurry, combined with the introduction of protective gas, the problem of pores in the semi-solid magnesium alloy is solved, and its mechanical properties and casting quality are improved.
Patent Information
- Application Number
- CN202411029107.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-30
AI Technical Summary
There are a large number of pores in semi-solid magnesium alloys, which leads to a decrease in mechanical properties, corrosion resistance and appearance quality. It is difficult to effectively solve the pore problem with existing technology.
By heating the semi-solid magnesium alloy billet to be formed above the liquidus line, controlling its cooling to the semi-solid temperature range, using the rotation and tilt of the container to form a laminar flow of the semi-solid slurry, combined with the introduction of protective gas to promote shear force The bubbles escape, the size and viscosity of the crystal nucleus are controlled, and the bubbles are separated simultaneously.
It effectively reduces the number of pores in semi-solid magnesium alloy, improves its mechanical properties, ensures the high quality of castings, and does not change the pulping process.
Smart Images

Figure CN118558975B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semi-solid magnesium alloys, and in particular to a method for preparing a low-porosity semi-solid magnesium alloy. Background Art
[0002] Porosity is one of the common defects in the alloy preparation process. The presence of pores will significantly reduce the mechanical properties, corrosion resistance and appearance quality of alloy castings. According to research, the sources of pores are various, such as mold design, impurities in the alloy, and air entrainment during casting.
[0003] Semi-solid magnesium alloy die-casting has fewer pores than traditional liquid alloy die-casting. On the one hand, this is because the semi-solid magnesium alloy has a certain solid content, which effectively avoids the formation of shrinkage cavities during die-casting. On the other hand, it is because the semi-solid magnesium alloy flows in a laminar manner during the die-casting process, which helps to reduce the involvement of gas and thus reduce the occurrence of pores.
[0004] However, in the process of preparing the semi-solid magnesium alloy slurry, the slurry is subjected to intense stirring, and the gas in the environment is easily mixed into the slurry, and these gases become the main source of bubbles in the semi-solid magnesium alloy castings. In particular, the gas-induced semi-solid forming technology requires continuous introduction of high-speed gas to provide stirring and cooling effects, so the gas is easily mixed into the semi-solid magnesium alloy slurry to form bubbles, and because the semi-solid magnesium alloy slurry has a high viscosity, the bubbles mixed in the semi-solid magnesium alloy slurry are difficult to discharge, and eventually this part of the gas enters the die-casting process with the slurry, forming a casting with a large number of pores. Summary of the invention
[0005] Based on this, it is necessary to provide a method for preparing a semi-solid magnesium alloy with low porosity.
[0006] In a first aspect, a method for preparing a semi-solid magnesium alloy with low porosity is provided, comprising the following steps:
[0007] Heating a semi-solid magnesium alloy billet to be formed to a temperature above the liquidus to obtain a melt, and placing the melt in a container;
[0008] The melt is cooled to a range of a semi-solid temperature interval by bubbling or stirring to obtain a semi-solid slurry. Specifically, by controlling the temperature of the semi-solid slurry, the solid content of the semi-solid slurry is controlled to be 10-15%. The semi-solid slurry with a solid content within this range has good fluidity and can generate laminar flow during container rotation. Controlling the cooling rate can make the crystal nucleus size of the semi-solid slurry within a certain range. By controlling the content and size of the crystal nucleus, the semi-solid slurry can be kept at a suitable viscosity. Specifically, too high a viscosity is not conducive to the flow of the semi-solid slurry, and too low a viscosity makes it difficult for the semi-solid slurry to be layered. Appropriate viscosity helps the semi-solid slurry to form a laminar flow to promote the escape of bubbles.
[0009] The container is rotated and gradually tilted, so that the rotational linear speed of the lowest point at the opening of the container is 0.1-1 m / s, the semi-solid slurry flows along the circumferential laminar flow of the container, and the semi-solid slurry is poured from the opening of the container into the mold for casting as the container gradually tilts, so as to obtain the low-porosity semi-solid magnesium alloy. In this step, as the container gradually tilts, the semi-solid slurry gradually flows toward the opening of the container, and gradually pours into the mold when reaching the opening of the container.
[0010] The above-mentioned method for preparing a semi-solid magnesium alloy with low porosity is that the semi-solid slurry with certain viscosity and fluidity flows in a laminar flow along the circumference of the container under the action of gravity by rotating the container. The semi-solid slurry near the inner wall of the container has a relatively low flow rate due to friction, while the semi-solid slurry far from the inner wall has a relatively higher flow rate, so that the semi-solid slurry flows in layers during the flow process, so as to spread out. The relative movement of the solid phase particles in each layer of the semi-solid slurry makes it easier for bubbles to leave the semi-solid slurry, and at the same time, the path for deep bubbles to leave the semi-solid slurry can be shortened. The weak shear force generated by the rotation of the above-mentioned linear speed will not have a negative impact on the growth of the crystal nucleus in the semi-solid slurry, but will be conducive to the formation of a better crystal nucleus morphology. At the same time, the semi-solid slurry is not easy to be involved in the gas during the laminar flow process. The semi-solid magnesium alloy is prepared by the above-mentioned preparation method without changing the pulping process. By making full use of the characteristics of the large viscosity of the semi-solid slurry, the semi-solid slurry is made to flow in layers by rotating the container, so as to spread out, so that the semi-solid slurry can simultaneously complete the separation of bubbles during the transfer process to the mold, and finally a semi-solid magnesium alloy with low porosity is obtained. If the linear speed is too low, the flow rate of each layer cannot be separated, which weakens the relative movement of each layer and is not conducive to gas separation. However, too fast rotational linear speed can easily lead to turbulence in semi-solid slurry, which in turn generates air entrainment and reduces the performance of the casting.
[0011] In one embodiment, the preparation method includes: introducing a protective gas into the container, and cooling the melt to a semi-solid temperature range by bubbling the protective gas to obtain a semi-solid slurry.
[0012] In this embodiment, a protective gas is introduced into the melt to stir the melt and take away the heat of the melt, thereby cooling the melt to a semi-solid temperature range, so that the melt solidifies into crystal nuclei near the bubbles, and the shear force provided by the bubbles can be conducive to producing crystal nuclei with higher sphericity.
[0013] In one embodiment, the protective gas is introduced into the container through a porous graphite heat dissipation device. The porous graphite heat dissipation device includes a porous graphite rod, and the porous graphite rod is extended into the melt, and the protective gas is introduced into the melt through the porous graphite rod to achieve cooling of the melt. The porous graphite rod can disperse the protective gas so that the protective gas is dispersed to form a plurality of bubbles, and each bubble can collide with the solidified crystal nucleus respectively to provide shear force to the crystal nucleus of the semi-solid slurry, which is conducive to forming a crystal nucleus that is close to a spherical shape.
[0014] In one embodiment, in the step of cooling the melt to the semi-solid temperature range by bubbling or stirring to obtain a semi-solid slurry, the cooling rate is 1-5°C / s. Too low a cooling rate is not conducive to forming a large number of crystal nuclei to obtain refined crystal nuclei, while too high a cooling rate will cause the crystal nuclei to grow coarsened. A cooling rate within a preferred range is conducive to forming refined solid phase particles, so that the semi-solid slurry is kept within a preferred viscosity range.
[0015] In one of the embodiments, the semi-solid magnesium alloy billet to be formed is heated to 10-30°C above the liquidus to obtain the melt. If the temperature is too high, additional energy will be consumed, while if the temperature is too low, it will be difficult to control the temperature of each part of the melt to be uniform, which may easily cause part of the melt to fall into the semi-solid temperature range and form irregularly shaped crystal nuclei in advance, which is not conducive to the subsequent cooling step to form spherical crystal nuclei.
[0016] In one of the embodiments, the inner wall of the container is a circular surface. The inner wall being a circular surface helps the semi-solid slurry to flow more smoothly along the inner wall during the rotation of the container, making the laminar flow of the semi-solid slurry more stable.
[0017] In one of the embodiments, the adjustment range of the tilt rate of the container is 1~9° / s. Specifically, a horizontal line drawn at the midpoint of the bottom of the container is the reference line, the line connecting the position of the opening of the container to pour the semi-solid slurry and the midpoint of the bottom of the container is the tilt line, and the angle change of the tilt line compared to the reference line is the tilt rate. The tilt rate of the container is adjusted within this range so that the thickest part H of the fan-shaped annular section is ≤5mm. If the thickest part of the fan-shaped annular section is too large, it means that the layers of the semi-solid slurry are not fully stratified, and the escape distance of the bubbles is large, which is not conducive to the escape of bubbles. Among them, for the thickest part of the fan-shaped annular section, the tilt rate has a greater impact than the rotation line speed. In the actual production process, the rotation line speed is generally controlled to be relatively stable, and the tilt rate of the container is adjusted within the range of 1~9° / s so that the thickest part of the fan-shaped annular section H≤5mm, so that the semi-solid slurry forms a laminar flow, and a better effect of separating bubbles is obtained, thereby avoiding the formation of pores in the semi-solid magnesium alloy, and thus making the semi-solid magnesium alloy have better mechanical properties. In one embodiment, during the transfer of the same batch of semi-solid slurry, the tilting rate of the container is controlled to maintain the thickest part of the fan-shaped annular cross section fluctuating between 20% and 20% of a specific value, so that the pouring process of the semi-solid slurry is more stable. For example, the tilting rate of the container is controlled to maintain the thickest part of the fan-shaped annular cross section at 3 mm ± 0.6 mm.
[0018] In one of the embodiments, the surface roughness Ra of the inner wall of the container satisfies: 3μm≤Ra≤6μm. When the surface roughness is too small, the container cannot drive the semi-solid slurry to be stratified, and excessive surface roughness will cause the semi-solid slurry near the inner wall of the container to adhere to the inner wall, resulting in waste of the semi-solid slurry.
[0019] In one embodiment, the semi-solid magnesium alloy billet to be formed comprises the following components in weight percentage: Al 8.5-9.5%; Zn 0.45-0.9%; Mn 0.17-0.4%; Si≤0.05%; Cu≤0.025%; Ni≤0.001%, Fe≤0.004%, and the balance is Mg. Specifically, the above components are used to prepare AZ91D magnesium alloy, which can be used in conjunction with the preparation method of the present application to obtain a semi-solid magnesium alloy with low porosity.
[0020] In a second aspect, a low-porosity semi-solid magnesium alloy is provided, which is prepared by the preparation method described in any of the above embodiments. The semi-solid magnesium alloy is prepared by the above preparation method without changing the slurry making process. By making full use of the high viscosity of the semi-solid slurry, the bubbles can be separated synchronously during the transfer of the semi-solid slurry to the mold, so that the low-porosity semi-solid magnesium alloy has better mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1The present invention is a schematic flow chart of a method for preparing a semi-solid magnesium alloy with low porosity according to an embodiment of the present application.
[0022] Figure 2 This is a schematic diagram of the melt in a container according to one embodiment of the present application.
[0023] Figure 3 This is a schematic diagram of a porous graphite rod extending into a melt according to an embodiment of the present application.
[0024] Figure 4 This is a schematic diagram of pouring semi-solid slurry into a container according to one embodiment of the present application.
[0025] Figure 5 for Figure 4 Schematic diagram of the cross-sectional structure at AA of the middle container.
[0026] Figure 6 Another schematic diagram of a container according to an embodiment of the present application when pouring semi-solid slurry.
[0027] Figure 7 This is a metallographic diagram of the low-porosity semi-solid magnesium alloy of Example 12 of the present application.
[0028] Figure 8 This is a metallographic diagram of the semi-solid magnesium alloy with low porosity according to Comparative Example 1 of the present application.
[0029] Reference numerals: 100, container; 101, opening; 200, melt; 300, argon gas; 400, porous graphite rod; 500, semi-solid slurry; 600, mold; 800, fan-shaped annular section; L, rotation center line. DETAILED DESCRIPTION
[0030] For ease of understanding of the application, the application will be described more fully below. The application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.
[0031] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0033] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0034] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0035] The percentage contents involved in this application, unless otherwise specified, refer to mass percentage for solid-liquid mixing and solid-solid mixing, and refer to volume percentage for liquid-liquid mixing.
[0036] The percentage concentrations mentioned in this application, unless otherwise specified, refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.
[0037] The temperature parameters in this application, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range of instrument control.
[0038] The "particles" mentioned in this application, or materials with a defined particle size distribution, are not necessarily spherical in shape, but may be irregular, primary particles or secondary particles. The particle size of irregular particles is the average of their maximum diameter and minimum diameter.
[0039] like Figure 1 As shown, in one embodiment, a method for preparing a semi-solid magnesium alloy with low porosity is provided, comprising the following steps:
[0040] S1, heating the semi-solid magnesium alloy billet to be formed to a temperature above the liquidus to obtain a melt, and placing the melt in a container; combining Figure 2 , the container 100 contains a melt 200 .
[0041] S2, cooling the melt to a temperature range of the semi-solid temperature by bubbling or stirring to obtain a semi-solid slurry; Figure 2 and Figure 3 The porous graphite rod 400 of the porous graphite heat dissipation device extends into the melt 200, and argon gas 300 is introduced through the porous graphite rod 400 to achieve bubbling, and the melt 200 is cooled by bubbling, and shear force is provided to the crystal nucleus, so that the crystal nucleus tends to grow in a spherical shape better.
[0042] S3, rotating the container and gradually tilting it, so that the rotational linear speed of the lowest point of the opening of the container is 0.1-1 m / s, the semi-solid slurry flows along the circumferential laminar flow of the container, and the semi-solid slurry is poured from the opening of the container into the mold for casting as the container gradually tilts, so as to obtain the low-porosity semi-solid magnesium alloy. Figure 4 , the container 100 rotates in the counterclockwise direction (observed from the container opening direction) as shown in the figure, and the rotation linear speed is v, that is, 0.1-1 m / s. In this embodiment, the semi-solid slurry 500 flows along the circumferential laminar flow of the container 100, and as the container 100 gradually tilts, it is poured from the opening 101 of the container 100 into the mold 600 for casting.
[0043] Figure 5 for Figure 4 The top view of the cross-sectional view of the middle container 100 at AA shows that the semi-solid slurry 500 flows out toward the opening 101 and spreads out in the circumferential direction of the container. Figure 4 and Figure 6 , taking a plane perpendicular to the rotation center line L of the container 100 and passing through the lowest point of the opening as a cross section, the cross section of the semi-solid slurry 500 on the plane is a fan-shaped ring cross section 800, and the maximum thickness of the fan-shaped ring cross section 800 is ≤5 mm.
[0044] The above-mentioned method for preparing a semi-solid magnesium alloy with low porosity is that the semi-solid slurry with certain viscosity and fluidity flows laminarly along the circumference of the container under the action of gravity by rotating and tilting the container. The semi-solid slurry near the inner wall of the container has a relatively low flow rate due to friction, while the semi-solid slurry far from the inner wall has a relatively higher flow rate, so that the semi-solid slurry flows in layers during the flow process, so as to spread out. The relative movement of the solid phase particles in each layer of the semi-solid slurry makes it easier for bubbles to leave the semi-solid slurry, and at the same time, the path for deep bubbles to leave the semi-solid slurry can be shortened. The weak shear force generated by the rotation of the above-mentioned linear speed will not have a negative impact on the growth of the crystal nucleus in the semi-solid slurry, but will be conducive to the formation of a better crystal nucleus morphology. At the same time, the slurry is not easy to be involved in gas during the laminar flow process. The semi-solid magnesium alloy is prepared by the above-mentioned preparation method without changing the pulping process. By making full use of the characteristics of the large viscosity of the semi-solid slurry, and by rotating the container to make the semi-solid slurry undergo laminar motion and spread out, the semi-solid slurry can simultaneously complete the separation of bubbles during the transfer process to the mold, and finally a semi-solid magnesium alloy with low porosity is obtained.
[0045] The following are some specific embodiments:
[0046] The experiment was conducted using AZ91D magnesium alloy, wherein the components of AZ91D, by weight percentage, include: Al 8.92%, Zn 0.617%, Mn 0.208%, Si 0.023%, Cu 0.001%, Ni 0.001%, Fe 0.002%, and the balance is Mg.
[0047] Example 1: The AZ91D magnesium alloy billet to be formed is heated to 20°C above the liquidus line in a resistance furnace to obtain a melt, and the melt is transferred to a container, wherein the interior of the container is a cylindrical cavity, the inner wall is a circular surface, and the surface roughness Ra of the inner wall of the container is 6μm.
[0048] A porous graphite rod was placed in the melt, 10 mm from the bottom of the container. Argon was used as a protective gas, and argon was passed into the melt through the porous graphite rod to cool the melt in a bubbling manner, with a cooling rate of 5°C / s, to obtain a semi-solid slurry with a solid content of 15%.
[0049] The mold is preheated to 350°C before casting, and the container is rotated and gradually tilted so that the rotational linear speed of the lowest point of the opening of the container is 1 m / s, so that the semi-solid slurry flows in a circumferential laminar flow along the container. During rotation, a plane perpendicular to the rotation center line of the container and passing through the lowest point of the opening is used as a cross section, and the cross section of the semi-solid slurry on the plane is a fan-shaped cross section. The tilting rate of the container is controlled within the range of 1 to 9° / s so that the thickest part H of the fan-shaped cross section is 5 mm, and the semi-solid slurry is poured from the opening of the container into the mold for casting to obtain the low-porosity semi-solid magnesium alloy.
[0050] Example 2: The difference from Example 1 is that the surface roughness Ra of the inner wall of the container is 3 μm.
[0051] Example 3: The difference from Example 1 is that the surface roughness Ra of the inner wall of the container is 4.5 μm.
[0052] Embodiment 4: The difference from Embodiment 1 is that the cooling rate is 1°C / s.
[0053] Example 5: The difference from Example 1 is that the cooling rate is 2°C / s.
[0054] Example 6: The difference from Example 1 is that argon gas is introduced into the melt through a porous graphite rod and the temperature is reduced by bubbling to obtain a semi-solid slurry with a solid content of 10%.
[0055] Example 7: The difference from Example 1 is that argon gas is introduced into the melt through a porous graphite rod and the temperature is reduced by bubbling to obtain a semi-solid slurry with a solid content of 12%.
[0056] Embodiment 8: The difference from Embodiment 1 is that the thickest part H of the fan-shaped annular section is 1 mm.
[0057] Embodiment 9: The difference from Embodiment 1 is that the thickest part H of the fan-shaped annular section is 3 mm.
[0058] Embodiment 10: The difference from Embodiment 1 is that the rotational linear velocity at the lowest point of the opening of the container is 0.1 m / s.
[0059] Embodiment 11: The difference from Embodiment 1 is that the rotational linear velocity at the lowest point of the opening of the container is 0.3 m / s.
[0060] Example 12: The difference from Example 1 is that the surface roughness Ra of the inner wall of the container is 4.5 μm. The cooling rate is 2°C / s. Argon gas is introduced into the melt through a porous graphite rod and the melt is cooled by bubbling to obtain a semi-solid slurry with a solid content of 12%. The thickest part H of the fan-shaped annular section is 3 mm. The rotational linear speed of the lowest point at the opening of the container is 0.3 m / s.
[0061] Example 13: The difference from Example 1 is that neon gas is used as the protective gas, the neon gas is introduced into the melt through a porous graphite rod, and the melt is cooled by bubbling to obtain a semi-solid slurry with a solid content of 15%.
[0062] Example 14: The difference from Example 1 is that the melt is cooled by stirring (1000 rpm / min) to obtain a semi-solid slurry with a solid content of 15%.
[0063] Comparative Example 1: The difference from Example 1 is that the container does not rotate when tilted.
[0064] Comparative Example 2: The difference from Example 1 is that the linear speed of rotation at the lowest point of the opening of the container is 0.05 m / s.
[0065] Comparative Example 3: The difference from Example 1 is that the linear speed of rotation at the lowest point of the opening of the container is 3 m / s.
[0066] Test: The semi-solid magnesium alloys of the above embodiments and comparative examples were die-cast to obtain castings, with a filling speed of 100 mm / s, a holding pressure of 120 MPa, a holding time of 420 s, and a mold temperature of 320°C. The yield strength and elongation of the castings were tested in accordance with the standard of "GB / T228.1-2021 Tensile Test of Metallic Materials Part 1: Room Temperature Test Method", and the specific results are shown in Table 1.
[0067] Table 1
[0068] Conclusion: By comparing the embodiments and comparative examples 1-3, it can be seen that the semi-solid magnesium alloys of the embodiments have better yield strength and elongation. This is because the semi-solid slurry flows in layers during the flow process through the preparation method of the present application. The relative movement of the particles of each layer of the semi-solid slurry makes it easier for bubbles to leave the melt, and at the same time, the path for deep bubbles to leave the melt can be shortened. The weak shear force generated by the above rotation will not have a negative impact on the growth of the crystal nucleus in the melt, but will be conducive to the formation of a better crystal nucleus morphology. At the same time, the semi-solid slurry is not easy to be involved in the gas during the laminar flow process, which ultimately makes the bubble content of the semi-solid magnesium alloy less, and thus makes the semi-solid magnesium alloy of each embodiment have better mechanical properties. The container of comparative example 1 is not rotated, and the bubbles are not easy to escape from the inside of the semi-solid slurry. Comparative example 2 uses a too low rotation line speed, and the layers of the semi-solid slurry are difficult to spread out in layers, and the bubbles are difficult to remove. Comparative example 3 uses a too high rotation line speed, and the semi-solid slurry is easy to entrain gas, resulting in an increase in pores and further reduction in performance.
[0069] By comparing Examples 1 to 3, it can be seen that the surface roughness of the inner wall of the container within a certain range can enable the semi-solid slurry to form a better stratification, thereby separating the bubbles, and ultimately making the semi-solid magnesium alloy have better mechanical properties. Among them, the surface roughness of Example 3 is at a better value, which enables the semi-solid slurry to better form laminar flow to separate bubbles, so that Example 3 has better mechanical properties.
[0070] By comparing Example 1, Example 4 and Example 5, it can be seen that the cooling rate within a certain range can make the semi-solid magnesium alloy have better mechanical properties, and at the optimal value of Example 5, the mechanical properties are better. This is because a moderate cooling rate helps to make the crystal nucleus of the semi-solid slurry more spherical and the size is within an optimal range, so that the semi-solid slurry has an optimal viscosity, which is convenient for forming laminar flow and separating bubbles.
[0071] By comparing Example 1, Example 6 and Example 7, it can be seen that when the semi-solid slurry is cooled to a solid content within a specific range in each example, the semi-solid magnesium alloy can have good mechanical properties, among which Example 7 has better mechanical properties. This is because the solid content of the semi-solid slurry is at an optimal value, and the ratio of the solid phase to the liquid phase is better, so that the semi-solid slurry is at an optimal viscosity. At this time, each layer of the semi-solid slurry has a better relative flow velocity, and the relative movement between the solid phase particles can promote the escape of bubbles, and the rotation promotes the uniform growth of the semi-solid slurry, which can ultimately make the semi-solid magnesium alloy have better mechanical properties.
[0072] By comparing Example 1, Example 8 and Example 9, it can be seen that the thickest value of the fan-shaped ring section formed by the semi-solid slurry at the opening is within a certain range, which can reduce the bubble content of the semi-solid slurry, so that the semi-solid magnesium alloy has better mechanical properties. Among them, the thickest value of the fan-shaped ring section of Example 9 is at a better value, which is conducive to the escape of bubbles, so that the semi-solid magnesium alloy has better mechanical properties.
[0073] By comparing Example 1, Example 10 and Example 11, it can be seen that the linear speed of rotation within a certain range can eliminate bubbles, so that the mechanical properties of the semi-solid magnesium alloy are better. Among them, the linear speed of rotation in Example 11 is at a better value, which helps the semi-solid slurry to form multi-layer laminar flows with different flow rates, better separate bubbles, and thus make the semi-solid magnesium alloy have better mechanical properties.
[0074] By comparing Example 1 and Example 12, it can be seen that the mechanical properties of Example 12 are significantly improved compared with Example 1. It can be seen that when all parameters are at a good value, the mechanical properties of the semi-solid magnesium alloy after forming are improved. This is because when all parameters are at a good value, the semi-solid slurry can be better promoted to delaminate, so as to more effectively remove the bubbles in the semi-solid slurry, so that the semi-solid magnesium alloy has fewer pores inside.
[0075] By comparing Example 1, Example 13 and Example 14, it can be seen that no matter cooling is achieved by protective gases such as argon or neon, or by stirring, the preparation method can be used to reduce pores, so that the semi-solid magnesium alloy has better mechanical properties.
[0076] The semi-solid magnesium alloys of Example 12 and Comparative Example 1 were placed under a metallographic microscope to observe the microstructure. Figure 7 and Figure 8 As shown, the white part in the figure is the crystal core. Figure 7 The uniformity of the crystal nucleus of the semi-solid magnesium alloy in Figure 8 The shape of the crystal nucleus is higher and closer to a sphere. This is because during the rotation and stratification process, each crystal nucleus is subjected to a certain shear force, which makes the crystal nucleus grow in a spherical shape. In addition, during the rotation of the container, the temperature of each position of the semi-solid slurry is relatively uniform, which makes the crystal nucleus grow uniformly. The dark black dots in the figure are pores. These are bubbles retained in the semi-solid slurry and formed as the semi-solid slurry solidifies into a semi-solid magnesium alloy. It can be seen that Figure 7 Compared with Figure 8 Obviously less, this is because when the container rotates, the relative movement of the solid phase particles in each layer of the semi-solid slurry makes it easier for the bubbles to leave the semi-solid slurry, shortening the path for deep bubbles to leave the semi-solid slurry, thereby obtaining a semi-solid magnesium alloy with low porosity.
[0077] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0078] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a low-porosity semi-solid magnesium alloy, characterized in that: The steps include: Heating a semi-solid magnesium alloy billet to be formed to a temperature above the liquidus to obtain a melt, and placing the melt in a container; Cooling the melt to a semi-solid temperature range by bubbling or stirring to obtain a semi-solid slurry; The container is rotated and gradually tilted so that the rotational linear speed of the lowest point of the opening of the container is 0.1~1m / s, the semi-solid slurry flows in a circumferential laminar flow along the container, and as the container is gradually tilted, the semi-solid slurry is poured from the opening of the container into the mold for casting to obtain the low-porosity semi-solid magnesium alloy. When the container is tilted, the adjustment range of the tilt rate of the container is 1~9° / s, and the surface roughness Ra of the inner wall of the container satisfies: 3μm≤Ra≤6μm. A plane perpendicular to the rotation center line of the container and passing through the lowest point of the opening is used as a cross section. The cross section of the semi-solid slurry on the plane is a fan-shaped cross section, and the maximum thickness of the fan-shaped cross section is ≤5mm.
2. The method for preparing a low-porosity semi-solid magnesium alloy according to claim 1, characterized in that: The semi-solid magnesium alloy billet to be formed comprises the following components in percentage by mass: Al 8.5-9.5%, Zn 0.45-0.9%, Mn 0.17-0.4%, Si≤0.05%, Cu≤0.025%, Ni≤0.001%, Fe≤0.004%, and the balance is Mg.
3. The method for preparing a low-porosity semi-solid magnesium alloy according to claim 1, characterized in that: include: A protective gas is introduced into the container, and the protective gas cools the melt to within the semi-solid temperature range by bubbling, thereby obtaining a semi-solid slurry.
4. The method for preparing a semi-solid magnesium alloy with low porosity according to claim 1, characterized in that: The solid content of the semi-solid slurry is 10-15%.
5. The method for preparing a low-porosity semi-solid magnesium alloy according to claim 1, characterized in that: The linear speed of rotation of the lowest point of the opening of the container is 0.3 m / s.
6. The method for preparing a low-porosity semi-solid magnesium alloy according to any one of claims 1 to 5, characterized in that: The semi-solid magnesium alloy billet to be formed is heated to 10-30° C. above the liquidus to obtain the melt.
7. A low-porosity semi-solid magnesium alloy, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Method and device for preparing semi-solid slurry