A method for preparing powder high-temperature alloy parts by low-stress isothermal forging and its application

Through low-stress isothermal forging method and combined with thermal isostatic pressure treatment, the abnormal grain growth and mold deformation problems caused by insufficient deformation of fine powder particles are solved, and high-density and low-cost powder high-temperature alloy parts are achieved, which significantly Improves mechanical properties and mold service life.

CN118559026BActive Publication Date: 2024-11-26SINO EURO MATERIALS TECH OF XIAN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411046210.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-26
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

During the existing forging process, abnormal grain growth and abnormal flaw detection signals are caused by insufficient deformation of the fine powder particles. The yield strength of the mold is reduced during high-temperature isothermal forging, resulting in mold deformation and cracking, increasing production costs.

Method used

Using low-stress isothermal forging method, by mixing fine powder (15μm~75μm) and coarse powder (106μm~150μm), thermal isostatic pressure treatment under vacuum conditions, followed by low-stress isothermal forging to reduce initial stress and load, and improve For the density and utilization of the powder, low-cost molds are selected for forging.

Benefits of technology

It effectively solves the problem of abnormal grain growth caused by insufficient deformation of fine powder particles, reduces the maximum load value in the early stage of forging, extends the mold life, improves the density and mechanical properties of powdered high-temperature alloy parts, and reduces production costs. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118559026B_ABST
    Figure CN118559026B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of powder metallurgy, and specifically discloses a method and application of preparing powder high-temperature alloy parts by low-stress isothermal forging. The method first mixes coarse and fine powders according to a set weight ratio to obtain pre-alloyed high-temperature alloy powder; then the pre-alloyed high-temperature alloy powder is loaded into a prefabricated sheath under vacuum conditions and degassed and sealed; then the sheath is subjected to hot isostatic pressing at high temperature and low pressure, and then the sheath is subjected to low-stress isothermal forging as a whole; finally, the sheath is removed, and heat treatment is performed according to a standard heat treatment system to obtain a powder high-temperature alloy part. The present invention not only optimizes the application range of the powder and improves the utilization efficiency of the powder, but also prolongs the service life of the mold and reduces the production cost by adopting a low-stress isothermal forging method; at the same time, the powder high-temperature alloy turbine disk manufactured based on this method fully meets the requirements of new aircraft engines for high thrust and long life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy, and in particular relates to a method for preparing a powder high-temperature alloy part by low-stress isothermal forging and an application thereof. Background Art

[0002] As we all know, turbine disks, as one of the important core hot end components of aircraft engines, have extremely harsh working conditions and usually need to operate in harsh environments of high temperature, high speed, high load, and complex oxidation corrosion. Therefore, in order to ensure the stability and reliability of the turbine disk, high-temperature alloy materials are usually used for manufacturing. The reason is that high-temperature alloy materials have excellent oxidation resistance and corrosion resistance, excellent performance in tensile, durability, and fatigue performance, and have long-term organizational stability, thus providing a strong guarantee for the safety and reliability of aviation flight.

[0003] However, in recent years, with the continuous increase in the thrust-to-weight ratio of advanced aircraft engines, more stringent requirements have been placed on the performance of hot-end components such as turbine discs. The powder discs produced by the conventional direct hot isostatic pressing process have been unable to meet the long-life requirements of new aircraft engines due to problems such as poor density and excessive inclusion size. The hot isostatic pressing + isothermal forging process route and the hot isostatic pressing + hot extrusion + isothermal forging process route have gradually become the mainstream process routes for powder discs. The powder discs produced by them have the advantages of uniform grain size, finer inclusion size, and high density. They can also obtain dual-performance discs through special heat treatment systems, meeting the high standards of new aircraft engines for high thrust and full life.

[0004] However, whether it is the hot isostatic pressing + isothermal forging process route or the hot isostatic pressing + hot extrusion + isothermal forging process route, the required materials must have superplasticity, and the powder used is usually 15μm ~ 75μm or 15μm ~ 53μm fine powder. The powders above 75μm and 53μm produced in the powder making process become residual waste. At the same time, during the forging process, due to the limitation of the fine powder PPB (primitive particle boundary), some powder particles have small strain during deformation. This part of the powder is prone to abnormal grain growth during the subsequent heat treatment process, resulting in a single abnormal signal during flaw detection. In addition, when isothermal forging is performed above 1000℃, the temperature of the mold itself also reaches above 1000℃. At this temperature, the yield strength of the mold is significantly reduced. It is known in the industry that isothermal forging molds above 1000℃ can only be made of N3 or Ni3Al-based high-temperature alloy materials, and the mold manufacturing cost is expensive. In the initial stage of isothermal forging, the stress will rise sharply due to work hardening, and will gradually stabilize until the recovery softening and work hardening reach a balance. During the initial forging stress stage when stress rises sharply, frequent local stress concentration will cause deformation or even cracking of the die, seriously affecting the service life of the die. At the same time, the maximum stress value in the initial stage will also limit the selection of isothermal forging equipment and die materials.

[0005] In view of this, this invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method and application of preparing powder high-temperature alloy parts by low-stress isothermal forging. The present invention focuses on solving the problem of abnormal grain growth and abnormal single display signal in the subsequent heat treatment due to the insufficient deformation of some fine powder particles in the existing forging process. At the same time, it can optimize the forging process, slow down the rising trend of equipment load in the initial stage of isothermal forging, and reduce the maximum load value in the initial stage of forging, effectively avoiding the problem of mold cracking and damage caused by sudden increase in load in the initial stage of forging, so low-cost molds such as K3 can be selected for isothermal forging to reduce costs. In addition, the powder particle size is optimized, which significantly improves the utilization rate of the powder.

[0007] The purpose of the present invention is to be solved by the following technical solutions:

[0008] On the one hand, the present invention provides a method for preparing a powder high-temperature alloy part by low-stress isothermal forging, firstly, two groups of high-temperature alloy powders with different particle size ranges are mixed according to a set weight ratio to obtain a pre-alloyed high-temperature alloy powder; then, the pre-alloyed high-temperature alloy powder is loaded into a prefabricated sheath under vacuum conditions and subjected to a degassing and sealing treatment; then, the entire sheath is subjected to a hot isostatic pressing treatment at a high temperature and low pressure, and then the entire sheath is isothermally forged using a low-stress isothermal forging method; finally, the sheath is removed to obtain a powder high-temperature alloy intermediate, and the intermediate is heat treated according to a standard heat treatment system to obtain a powder high-temperature alloy part.

[0009] Furthermore, the method specifically includes the following steps:

[0010] Step 1, preparing high temperature alloy powder raw material;

[0011] Step 2: Screening the high-temperature alloy powder raw material prepared in step 1 into a first group of high-temperature alloy powder and a second group of high-temperature alloy powder according to the particle size, and then mixing the screened first group of high-temperature alloy powder and the second group of high-temperature alloy powder according to a set weight ratio to obtain pre-alloyed high-temperature alloy powder;

[0012] Step 3, placing the pre-alloyed high-temperature alloy powder obtained in step 2 into a prefabricated package under vacuum conditions and performing a degassing and sealing welding process;

[0013] Step 4, subjecting the entire package after the degassing and sealing treatment in step 3 to hot isostatic pressing at high temperature and low pressure;

[0014] Step 5, performing low stress isothermal forging on the entire can after hot isostatic pressing in step 4;

[0015] Step 6: remove the jacket to obtain a powder high-temperature alloy intermediate, and perform heat treatment on the powder high-temperature alloy intermediate according to a standard heat treatment system to obtain a powder high-temperature alloy product.

[0016] Furthermore, in step 1, the high temperature alloy powder raw material is prepared by a plasma rotating electrode method or an argon atomization method.

[0017] Furthermore, in step 2, the particle size range of the first group of high-temperature alloy powders is 15μm to 75μm, the particle size range of the second group of high-temperature alloy powders is 106μm to 150μm, and the weight ratio of the first group of high-temperature alloy powders to the second group of high-temperature alloy powders is 1:1 to 3:1.

[0018] Furthermore, in step 3, the pre-alloyed high temperature alloy powder is heated to a temperature of ≤1×10 -2 Pa under the conditions of put into the prefabricated package.

[0019] Furthermore, in step 4, the parameters of the hot isostatic pressing treatment are set as follows: temperature is 1170° C. to 1240° C., pressure is 90 MPa to 110 MPa, and time is 2 h to 4 h.

[0020] Furthermore, in step 4, a powder high-temperature alloy intermediate having a density of 95% to 99% is formed in the sheath after the hot isostatic pressing treatment.

[0021] Furthermore, in step 5, the parameters of the low stress isothermal forging are set as follows: the preheating temperature is 1050° C. to 1100° C., and the strain rate is 0.004 / s to 0.006 / s.

[0022] Furthermore, the powder high-temperature alloy product obtained by the method has a density of ≥99.9%, a tensile strength of >1500MPa, a yield strength of >1100MPa, an elongation of >15%, and a cross-sectional shrinkage of >15%.

[0023] On the other hand, the present invention provides a powder high-temperature alloy turbine disk for an aircraft engine, which is prepared based on the above-mentioned method for preparing powder high-temperature alloy parts by low-stress isothermal forging.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The method provided by the present invention firstly mixes fine powder (15μm-75μm) and coarse powder (106μm-150μm) in a specific weight ratio to prepare pre-alloyed high-temperature alloy powder; then, the powder is subjected to hot isostatic pressing at high temperature and low pressure; and then, the entire package is isothermally forged by a low-stress isothermal forging method. The method provided by the present invention can effectively solve the problem of abnormal grain growth and abnormal single display signal in the subsequent heat treatment caused by insufficient deformation of some fine powder particles in the existing forging process. At the same time, through the combination strategy of coarse and fine powders, the available range of powder particle size is significantly expanded, and the utilization rate of powder is greatly improved. In addition, by adopting a low-stress (conventional forging force is about 8000t, and the present invention is about 5000t) isothermal forging method, the rising trend of equipment load and the maximum load value in the initial stage of forging are successfully reduced, and the cracking and damage of the mold caused by the sharp increase in load in the initial stage of forging are effectively avoided, thereby significantly improving the service life of the mold and greatly reducing the production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0028] Figure 1 This is a flow chart of the method for preparing powder high-temperature alloy parts by low-stress isothermal forging of the present invention;

[0029] Figure 2 This is a microstructure morphology diagram of a powder high-temperature alloy intermediate after hot isostatic pressing in Example 1 of the present invention;

[0030] Figure 3 This is a microstructure morphology diagram of a workpiece after isothermal forging according to Example 1 of the present invention;

[0031] Figure 4 It is a schematic diagram of the change of forging force during isothermal forging in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples consistent with some aspects of the present invention as detailed in the appended claims.

[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0034] See also Figure 1 The present invention provides a method for preparing a powder high-temperature alloy part by low-stress isothermal forging, which specifically comprises the following steps:

[0035] Step 1, preparing high temperature alloy powder raw material;

[0036] Step 2: Screening the high-temperature alloy powder raw material prepared in step 1 into a first group of high-temperature alloy powder and a second group of high-temperature alloy powder according to the particle size, and then mixing the screened first group of high-temperature alloy powder and the second group of high-temperature alloy powder according to a set weight ratio to obtain pre-alloyed high-temperature alloy powder;

[0037] Step 3, placing the pre-alloyed high-temperature alloy powder obtained in step 2 into a prefabricated package under vacuum conditions and performing a degassing and sealing welding process;

[0038] Step 4, subjecting the entire package after the degassing and sealing treatment in step 3 to hot isostatic pressing at high temperature and low pressure;

[0039] Step 5, performing low stress isothermal forging on the entire can after hot isostatic pressing in step 4;

[0040] Step 6: remove the sheath to obtain a powder high-temperature alloy intermediate, and perform heat treatment on the powder high-temperature alloy intermediate according to a standard heat treatment system to obtain a powder high-temperature alloy product.

[0041] Specifically, in step 1, the high-temperature alloy powder raw material is prepared by a plasma rotating electrode method or an argon atomization method.

[0042] In step 2, the particle size range of the first group of high temperature alloy powders is 15μm to 75μm, the particle size range of the second group of high temperature alloy powders is 106μm to 150μm, and the weight ratio of the first group of high temperature alloy powders to the second group of high temperature alloy powders is 1:1 to 3:1.

[0043] In step 3, the pre-alloyed high temperature alloy powder is placed in a vacuum of ≤1×10 -2 Pa under the conditions of put into the prefabricated package.

[0044] In step 4, the parameters of the hot isostatic pressing treatment are set as follows: temperature is 1170°C to 1240°C, pressure is 90MPa to 110MPa, and time is 2h to 4h; after the hot isostatic pressing treatment, a powder high-temperature alloy intermediate with a density of 95% to 99% is formed in the sheath.

[0045] In step 5, the parameters during low stress isothermal forging are set as follows: preheating temperature is 1050° C. to 1100° C., and strain rate is 0.004 / s to 0.006 / s.

[0046] The present invention is conceived as follows: the method of the present invention can solve the problem of abnormal grain growth and abnormal single display signal in the subsequent heat treatment caused by insufficient deformation of some fine powder particles in the existing forging process. The principle is: during conventional isothermal forging, deformation behavior will occur at the original grain boundary of the powder alloy, resulting in excessive distortion inside the material, multiple slip systems will be generated, a large number of dislocations will be eliminated by large-angle migration, the number of small-angle grain boundaries will continue to decrease, and recrystallization will gradually develop towards the inside of the original grains, and finally gradually transform into a completely recrystallized equiaxed structure. However, the fine powder will form an original particle boundary due to the adsorption of oxidant points on the surface, which will hinder the deformation of the powder particles and reduce the offset of the large-angle grain boundaries, so that a large number of dislocations will accumulate inside the powder, and abnormal grain growth will occur during the subsequent heat treatment process. During the isothermal forging process, the deformation of the upper and lower end faces is often not very large, and the deformation of the two side areas is second, and the deformation is often concentrated in the middle area. At the same time, compared with large-size particles, small-size particles are more difficult to deform, and the abnormal grain growth caused by insufficient strain is more obvious. The present invention uses a mixed powder of fine powder + coarse powder, and uses a high temperature and low pressure hot isostatic pressing process to stably batch prepare a powder high temperature alloy intermediate with a density of 95% to 99%. The powder high temperature alloy intermediate has pores in a vacuum state. During the deformation process, the powder particles will displace each other, and this displacement is mostly started from small-sized particles. On the one hand, it will destroy the original particle boundary generated on the powder surface, and on the other hand, it will also help to increase the deformation of small-sized particles, and finally form a completely recrystallized structure, so that parts with a density of ≥99.9% can be prepared. At the same time, when the powder particles fill the pores, the initial maximum load required for deformation will be reduced. After the dynamic recrystallization is started, the required load will be further reduced, which is beneficial to the selection of equipment and the improvement of mold life.

[0047] In order to further verify the efficacy of the present invention, the following experiments were conducted: Example 1

[0048] The preparation of X-type powder high-temperature alloy turbine disk for an aircraft engine includes the following processes:

[0049] 1) Preparation of high temperature alloy powder by plasma rotating electrode method;

[0050] 2) Screening the high-temperature alloy powder prepared in step 1) into a first group of high-temperature alloy powder and a second group of high-temperature alloy powder according to the particle size, and then mixing the screened first group of high-temperature alloy powder and the second group of high-temperature alloy powder at a set weight ratio of 3:1 to obtain pre-alloyed high-temperature alloy powder;

[0051] The particle size of the first group of high temperature alloy powders ranges from 15 μm to 75 μm, and the particle size of the second group of high temperature alloy powders ranges from 106 μm to 150 μm;

[0052] 3) The pre-alloyed high temperature alloy powder obtained in step 2) is placed in a vacuum of ≤1×10 -2 Pa, and then put it into a prefabricated package and perform degassing and sealing treatment;

[0053] 4) The entire package after the degassing and sealing treatment in step 3) is subjected to hot isostatic pressing at high temperature and low pressure. The microstructure of the powder high-temperature alloy intermediate formed in the package after the hot isostatic pressing treatment is as follows: Figure 2 As shown, the density of the powder high-temperature alloy intermediate was measured to be 95%;

[0054] The parameters of hot isostatic pressing treatment were set as follows: temperature was 1170°C, pressure was 90 MPa, and time was 4 h;

[0055] 5) performing low stress isothermal forging on the entire can after hot isostatic pressing in step 4);

[0056] Among them, the parameters during isothermal forging are set as follows: preheating temperature is 1050°C, strain rate is 0.004 / s, and forging force is 4500t;

[0057] 6) Finally, the jacket is removed and heat treated according to the standard heat treatment system to obtain an X-type powder high-temperature alloy turbine disk. The microstructure of the X-type powder high-temperature alloy turbine disk is as follows: Figure 3 As shown, the density of the X-type powder high-temperature alloy turbine disk was measured to be 99.92%.

[0058] In order to further verify the effect of the present invention, the inventors conducted relevant measurements on the forging load data during the isothermal forging process of the present invention and the traditional process, such as Figure 4 As shown in the figure, the solid line is the forging force curve of the fully dense part made by the traditional process. The forging force has a slow rising trend in the initial stage, and the maximum forging force reaches 8000t. The dotted line is the forging force curve of the X-type powder high-temperature alloy turbine disk with the same size prepared according to the present invention. The rising trend of the forging force in the initial forging stage is slowed down. With the progress of forging and the further improvement of density, the forging force increases. The maximum forging force in the initial stage is 4500t, and the forging force is reduced by 43.5%, which has less impact on the mold and is more conducive to the protection of the mold.

[0059] In addition, the inventors compared the tensile properties of the X-type powder high-temperature alloy turbine disk finally prepared by the present invention and the fully dense product (with the same specifications as the X-type powder high-temperature alloy turbine disk) finally prepared by the traditional process at 400°C, as shown in Table 1 below:

[0060] Table 1 Comparison of tensile properties of the parts made by the present invention and the parts made by the traditional process at 400°C

[0061]

[0062] It can be seen from the test results in Table 1 that the mechanical properties of the X-type powder high-temperature alloy turbine disk obtained by the present invention are significantly better than those of the fully dense parts obtained by the traditional process. Specifically, the X-type powder high-temperature alloy turbine disk obtained by the present invention has an average tensile strength of 1561.5 MPa, an average yield strength of 1151 MPa, an average elongation of 21.7%, and an average cross-sectional shrinkage of 30.05%, while the fully dense parts obtained by the traditional process have an average tensile strength of only 1520.5 MPa, an average yield strength of 1100.5 MPa, an average elongation of 18.7%, and an average cross-sectional shrinkage of 23.4%. Example 2

[0063] The preparation of a Y-shaped powder high-temperature alloy turbine disk for an aircraft engine includes the following processes:

[0064] 1) Preparation of high temperature alloy powder by argon atomization method;

[0065] 2) Screening the high-temperature alloy powder prepared in step 1) into a first group of high-temperature alloy powder and a second group of high-temperature alloy powder according to the particle size, and then mixing the screened first group of high-temperature alloy powder and the second group of high-temperature alloy powder at a set weight ratio of 2:1 to obtain pre-alloyed high-temperature alloy powder;

[0066] The particle size of the first group of high temperature alloy powders ranges from 20 μm to 50 μm, and the particle size of the second group of high temperature alloy powders ranges from 110 μm to 140 μm;

[0067] 3) The pre-alloyed high temperature alloy powder obtained in step 2) is placed in a vacuum of ≤1×10 -2 Pa, and then put it into a prefabricated package and perform degassing and sealing treatment;

[0068] 4) The entire package after the degassing and sealing treatment in step 3) is subjected to hot isostatic pressing at high temperature and low pressure. The powder high-temperature alloy intermediate formed in the package after the hot isostatic pressing treatment is measured to have a density of 99%;

[0069] The parameters of hot isostatic pressing treatment were set as follows: temperature was 1200 °C, pressure was 100 MPa, and time was 3 h;

[0070] 5) performing low stress isothermal forging on the entire can after hot isostatic pressing in step 4);

[0071] Among them, the parameters during isothermal forging are set as follows: preheating temperature is 1050°C, strain rate is 0.005 / s, and forging force is 5000t;

[0072] 6) Finally, the jacket is removed and heat treatment is performed according to a standard heat treatment system to obtain a Y-type powder high-temperature alloy turbine disk. The density of the Y-type powder high-temperature alloy turbine disk is measured to be 99.5%. Example 3

[0073] The preparation of Z-type powder high-temperature alloy turbine disk for an aircraft engine includes the following processes:

[0074] 1) Preparation of high temperature alloy powder by plasma rotating electrode method;

[0075] 2) Screening the high-temperature alloy powder prepared in step 1) into a first group of high-temperature alloy powder and a second group of high-temperature alloy powder according to the particle size, and then mixing the screened first group of high-temperature alloy powder and the second group of high-temperature alloy powder at a set weight ratio of 1:1 to obtain pre-alloyed high-temperature alloy powder;

[0076] The particle size of the first group of high temperature alloy powders ranges from 15 μm to 35 μm, and the particle size of the second group of high temperature alloy powders ranges from 120 μm to 140 μm;

[0077] 3) The pre-alloyed high temperature alloy powder obtained in step 2) is placed in a vacuum of ≤1×10 -2 Pa, and then put it into a prefabricated package and perform degassing and sealing treatment;

[0078] 4) The entire package after the degassing and sealing treatment in step 3) is subjected to hot isostatic pressing at high temperature and low pressure. The powder high-temperature alloy intermediate formed in the package after the hot isostatic pressing treatment is measured to have a density of 97%;

[0079] The parameters of hot isostatic pressing treatment were set as follows: temperature 1240 °C, pressure 110 MPa, and time 2 h;

[0080] 5) performing low stress isothermal forging on the entire can after hot isostatic pressing in step 4);

[0081] Among them, the parameters during isothermal forging were set as follows: preheating temperature was 1050 °C, strain rate was 0.006 / s, and forging force was 5500t;

[0082] 6) Finally, the jacket is removed and heat treatment is performed according to a standard heat treatment system to obtain a Z-type powder high-temperature alloy turbine disk. The density of the Z-type powder high-temperature alloy turbine disk is measured to be 99.3%.

[0083] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0084] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for preparing powder high temperature alloy parts by low stress isothermal forging, It is characterized in that First, two groups of high-temperature alloy powders with different particle size ranges are mixed according to a set weight ratio to obtain pre-alloyed high-temperature alloy powder; then the pre-alloyed high-temperature alloy powder is loaded into a prefabricated sheath under vacuum conditions and subjected to degassing and sealing treatment; then the entire sheath is subjected to hot isostatic pressing treatment at high temperature and low pressure, and then the entire sheath is isothermally forged using a low-stress isothermal forging method; finally, the sheath is removed to obtain a powder high-temperature alloy intermediate, and the intermediate is heat treated according to a standard heat treatment system to obtain a powder high-temperature alloy product; The specific steps include: Step 1, preparing high temperature alloy powder raw material; Step 2: Screening the high-temperature alloy powder raw material prepared in step 1 into a first group of high-temperature alloy powder and a second group of high-temperature alloy powder according to the particle size, and then mixing the screened first group of high-temperature alloy powder and the second group of high-temperature alloy powder according to a set weight ratio to obtain pre-alloyed high-temperature alloy powder; Step 3, placing the pre-alloyed high-temperature alloy powder obtained in step 2 into a prefabricated package under vacuum conditions and performing a degassing and sealing welding process; Step 4, subjecting the entire package after the degassing and sealing treatment in step 3 to hot isostatic pressing at high temperature and low pressure; Step 5, performing low stress isothermal forging on the entire can after hot isostatic pressing in step 4; Step 6: removing the jacket to obtain a powder high-temperature alloy intermediate, and heat treating the powder high-temperature alloy intermediate according to a standard heat treatment system to obtain a powder high-temperature alloy product; Wherein, in step 2, the particle size range of the first group of high temperature alloy powders is 15 μm to 75 μm, the particle size range of the second group of high temperature alloy powders is 106 μm to 150 μm, and the weight ratio of the first group of high temperature alloy powders to the second group of high temperature alloy powders is 1:1 to 3:1; In step 4, the parameters of the hot isostatic pressing treatment are set as follows: temperature is 1170° C. to 1240° C., pressure is 90 MPa to 110 MPa, and time is 2 h to 4 h; after the hot isostatic pressing treatment, a powder high-temperature alloy intermediate with a density of 95% to 99% is formed in the sheath; In step 5, the parameters of the low stress isothermal forging are set as follows: the preheating temperature is 1050° C. to 1100° C., and the strain rate is 0.004 / s to 0.006 / s.

2. The method for preparing a powder high-temperature alloy part by low-stress isothermal forging according to claim 1, It is characterized in that In step 1, the high temperature alloy powder raw material is prepared by a plasma rotating electrode method or an argon atomization method.

3. The method for preparing a powder high temperature alloy part by low stress isothermal forging according to claim 1, It is characterized in that In step 3, the pre-alloyed high temperature alloy powder is placed in a vacuum of ≤1×10 -2 Pa under the conditions of put into the prefabricated package.

4. The method for preparing a powder high temperature alloy part by low stress isothermal forging according to claim 1, It is characterized in that The powder high-temperature alloy product obtained by the method has a density of ≥99.9%, a tensile strength of >1500MPa, a yield strength of >1100MPa, an elongation of >15%, and a cross-sectional shrinkage of >15%.

5. A powder high temperature alloy turbine disk for aircraft engines, It is characterized in that The powder high-temperature alloy turbine disk is prepared based on the method for preparing powder high-temperature alloy parts by low-stress isothermal forging as described in any one of claims 1 to 4.