A deformable biodegradable material, its preparation method and products

By performing tensile treatment on PLA/PPC composite materials, the problem of insufficient material toughness was solved, resulting in a biodegradable material with high toughness and deformability, thus expanding its application range.

CN118560015BActive Publication Date: 2026-11-17ZHEJIANG HONOR BIOMATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410642379.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2026-11-17
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

The low notched impact strength and poor toughness of PLA/PPC composites limit their application range, especially in the development of three-dimensional materials.

Method used

By stretching PLA/PPC composites at 0-30℃ and controlling the stretching ratio to not exceed their maximum stretching ratio, deformable and biodegradable materials were prepared, and the ratio of PLA to PPC and the stretching parameters were optimized.

Benefits of technology

It significantly improves the notched impact strength and toughness of the material, enabling it to deform multiple times under external force, thus broadening its application areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118560015B_ABST
    Figure CN118560015B_ABST
Patent Text Reader

Abstract

This application relates to a method for preparing a deformable and biodegradable material, comprising the following steps: providing a PLA / PPC composite material, wherein the PLA / PPC composite material comprises, by weight, 20-75 parts of polylactic acid and 25-80 parts of polypropylene carbonate; stretching the PLA / PPC composite material at a temperature of 0-30°C to obtain a deformable and biodegradable material, wherein the stretching ratio does not exceed the maximum stretching ratio of the PLA / PPC composite material. The preparation method of this invention is simple and convenient, with low equipment requirements. The deformable and biodegradable material prepared by the method of this invention not only has the advantages of being green and environmentally friendly, but also possesses excellent mechanical properties and can undergo multiple deformations in any direction under external force, thus broadening the application fields of the PLA / PPC composite system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biodegradable polymer materials technology, specifically relating to a deformable biodegradable material, its preparation method, and its products. Background Technology

[0002] Polylactic acid (PLA) is a commercially available biodegradable material derived from plant matter. It has advantages such as high strength, good processability, and excellent biocompatibility, but it has high rigidity and poor toughness.

[0003] Polypropylene carbonate (PPC) is a biodegradable material made from CO2. It is an amorphous polymer with flexible molecular chains. PPC has a low glass transition temperature, high elongation at break, good barrier properties, and good biocompatibility. However, it is prone to shrinkage and adhesion, making it difficult to use alone.

[0004] Both PLA and PPC are environmentally friendly materials. They have certain complementary properties and good compatibility. Combining the two materials can produce materials with better performance, which is conducive to opening up new application fields, promoting the development of biodegradable materials, and conforming to the carbon neutrality development policy.

[0005] Currently, the main research focus of PLA / PPC composite systems is on the preparation of high-barrier packaging materials, especially two-dimensional planar materials such as films, with few reports on three-dimensional materials. This may be because while blending PLA with PPC can improve the elongation at break, the notched impact strength of the composite system remains low, and the improvement in toughness is not significant.

[0006] CN117209982A discloses a method for preparing PLA / PPC composite materials with improved toughness and optical properties. PLA, end-capped PPC, compatibilizer, initiator, and antioxidant are mixed uniformly in a specified mass ratio and then added to a twin-screw extruder to obtain the PLA / PPC composite material. This method improves the overall toughness of the material while maintaining excellent optical properties, and increases the notched impact strength by 2.2 times. Summary of the Invention

[0007] Currently, PLA / PPC materials still have shortcomings such as low notched impact strength and poor toughness, which limits their application areas. For example, PLA / PPC materials are usually only used to prepare two-dimensional planar products (such as film products).

[0008] To overcome the shortcomings of the prior art, this application provides a preparation method for preparing a deformable and degradable material, comprising the following steps: providing a PLA / PPC composite material, wherein the PLA / PPC composite material comprises, by weight, 20-75 parts of polylactic acid and 25-80 parts of polypropylene carbonate; stretching the PLA / PPC composite material at a temperature of 0-30°C to obtain the deformable and degradable material, wherein the stretching ratio does not exceed the maximum stretching ratio of the PLA / PPC composite material.

[0009] On the other hand, this application provides a deformable biodegradable material, which is prepared by the method of this application.

[0010] In another aspect, this application provides a deformable biodegradable article comprising the deformable biodegradable material of this application. Attached Figure Description

[0011] Figure 1 The stress-displacement curves of PLA / PPC composite samples with different PPC contents are shown at 18℃ and a tensile rate of 5 mm / min.

[0012] Figure 2 The stress-displacement curves of PLA / PPC composite samples with a PPC content of 40 parts by weight are shown at 18°C ​​and different tensile rates.

[0013] Figure 3 The appearance of the stretched material strips of Embodiment 2, Embodiments 6-9 of the present invention and the material strip of Comparative Example 2 are shown.

[0014] Figure 4 The force-displacement curves of the stretched material specimens of Embodiments 2, 6-8 and Comparative Example 2 are shown at 23°C and a compression rate of 2 mm / min.

[0015] Figure 5 This illustrates the deformation capability of the stretched material spline of Embodiment 9 of the present invention in different spatial directions. Detailed Implementation

[0016] General definitions and terms

[0017] Unless otherwise stated, all publications, patent applications, patents and other references mentioned herein are incorporated herein in their entirety by way of citation.

[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of any conflict, the definitions provided herein shall prevail.

[0019] Unless otherwise stated, all percentages, parts, proportions, etc. are by weight.

[0020] When a quantity, concentration, or other value or parameter is given as a range, preferred range, or preferred upper and lower limits, or a specific value, it should be understood as specifically disclosing all ranges formed by pairs of values ​​from any upper or preferred range and any lower or preferred range, regardless of whether the range is disclosed individually. Unless otherwise stated, when a numerical range is referred to herein, the range means including its endpoints and all integers and fractions within that range. The scope of this invention is not limited to the specific numerical value referenced when defining a range. For example, "1-8" encompasses 1, 2, 3, 4, 5, 6, 7, 8, and any subrange consisting of any two of these values, such as 2-6, 3-5.

[0021] When used with a numerical variable, the terms "about" or "approximately" usually mean that the value of the variable and all values ​​of the variable are within the experimental error (e.g., within a 95% confidence interval for the mean) or within ±10% of the specified value, or a wider range.

[0022] The terms “comprising,” “including,” “having,” “containing,” or “involving,” and their other variations herein, are inclusive or open-ended and do not exclude other unlisted elements or method steps. Those skilled in the art will understand that the foregoing terms such as “comprising” encompass the meaning of “consisting of.” The expression “consisting of” excludes any unspecified elements, steps, or ingredients. The expression “substantially constitutes” limits the scope to the specified elements, steps, or ingredients, plus optional elements, steps, or ingredients that do not materially affect the essential and novel features of the claimed subject matter. It should be understood that the expression “comprising” encompasses both the expressions “substantially constitutes” and “consisting of.”

[0023] The term “selected from…” means one or more elements from the groups listed below, selected independently, and may include combinations of two or more elements.

[0024] When describing numerical or range endpoints in this document, it should be understood that the disclosure includes the specific values ​​or endpoints referenced.

[0025] As used herein, the terms “one or more” or “at least one” refer to one, two, three, four, five, six, seven, eight, nine or more.

[0026] Unless otherwise stated, the terms "combination thereof" and "mixture thereof" refer to a multi-component mixture of the elements, such as two, three, four, and up to the maximum possible multi-component mixture.

[0027] Furthermore, if the number of components or parts of the present invention is not previously specified, it indicates that there is no limitation on the number of times a component or part may appear (or be present). Therefore, it should be interpreted as including one or at least one, and the singular form of a component or part also includes the plural, unless the value clearly indicates a singular number.

[0028] As used herein, the terms “optional” or “optionally” mean that the event or situation subsequently described may or may not occur, including both the occurrence and non-occurrence of the event or situation.

[0029] When the lower and upper limits of a numerical range are disclosed, any numerical value falling within that range and any included range are specifically disclosed. In particular, each range of values ​​disclosed herein (in the form of “about a to b”, or equivalently, “approximately a to b”, or equivalently, “about ab”) should be understood to represent each numerical value and range encompassed within a wider range.

[0030] As used herein, the term “room temperature” (RT) refers to about 20 to 35°C, preferably about 25°C.

[0031] The term "neck" as used in this article refers to the phenomenon where a material becomes locally thinner after being subjected to stress and yielding.

[0032] The term “tensile displacement” as used in this article refers to the difference between the size of the material after stretching and the initial size of the material (i.e., the size of the material before stretching).

[0033] The term “maximum stretchable dimension” as used in this article refers to the maximum dimension to which a material can be stretched without defects (such as cracks, necking, fractures, etc.).

[0034] The term “maximum stretchable displacement” as used in this article refers to the difference between the maximum stretchable dimension of the material and the initial material dimension (i.e., the unstretched material dimension).

[0035] As used herein, the term "stretch ratio" refers to the ratio of the material's stretched dimensions to its initial dimensions (i.e., the dimensions of the material before stretching). Unless otherwise stated, the stretched dimensions refer to the dimensions to which the material is stretched under the presence of external forces.

[0036] In this article, "deformable" means that a material can deform under the action of external force, and after the external force is removed, the deformation of the material will be fixed or basically maintained, and will not spontaneously rebound.

[0037] Unless otherwise stated, in this article, “deformation” or “shape change” has the same meaning as “shape change”, referring to a change in shape that can be fixed or substantially maintained after the removal of external force.

[0038] As used in this article, the term "maximum stretchable ratio" refers to the ratio of the maximum stretchable dimension of a material to its initial dimension (i.e., the dimension of the material before stretching).

[0039] In this article, "PHB" refers to poly-β-hydroxybutyrate.

[0040] Preparation methods of deformable and biodegradable materials

[0041] This invention relates to a method for preparing a deformable and biodegradable material, comprising the following steps:

[0042] PLA / PPC composite materials are provided, which, by weight, contain 20-75 parts of polylactic acid and 25-80 parts of polypropylene carbonate.

[0043] PLA / PPC composites are stretched at 0-30℃ to obtain deformable and degradable materials, wherein the stretching ratio does not exceed the maximum stretching ratio of the PLA / PPC composite.

[0044] The preparation method of this application will be described below with specific steps.

[0045] Provide PLA / PPC composite materials

[0046] In this article, "PLA / PPC composite material" refers to a blend of polylactic acid and polypropylene carbonate, wherein the polylactic acid and polypropylene carbonate form a homogeneous or near-homogeneous system, that is, the material of PLA / PPC composite material is uniform in physical and chemical properties and has no obvious boundaries or macroscopic limits.

[0047] The PLA / PPC composite material can be used to prepare the deformable and biodegradable material of this application through subsequent stretching treatment. There are no particular limitations on the manner in which the PLA / PPC composite material is provided; it can be provided by any method in the art. Polylactic acid and polypropylene carbonate can be melt-blended, granulated to form a blend masterbatch, and then the blend masterbatch can be used to produce the PLA / PPC composite material.

[0048] Melt blending and granulation can be performed using equipment commonly used in the art, such as a twin-screw extruder. In one embodiment, PLA and PPC chips are mixed in a certain proportion and then fed into a twin-screw extruder. After melt mixing in the twin-screw extruder, the mixture is extruded and granulated to obtain PLA / PPC blend masterbatch.

[0049] The melt blending temperature should allow PLA and PPC to fully melt without decomposition. The melt blending process of PLA and PPC can be achieved by setting the parameters of a screw extruder. In one embodiment, the screw temperature of the twin-screw extruder can be 150-180°C, the rotation speed can be 200-300 rpm, and the throughput time of PLA and PPC within the twin-screw extruder can be 0.5-2 minutes. After melt blending, the PLA and PPC are extruded through the screw extruder and then granulated to obtain PLA / PPC blend masterbatch. During granulation, air cooling can be used as the cooling method for the masterbatch, which helps to avoid introducing unwanted moisture into the material.

[0050] PLA / PPC composite materials can be produced from blended masterbatches using methods commonly used in the art, such as injection molding and extrusion molding. In one embodiment, injection molding is used to produce PLA / PPC composite materials from blended masterbatches. The advantages of injection molding are: by adjusting the mold shape, PLA / PPC composite materials with desired shapes can be flexibly prepared; and by controlling the parameters of the injection molding process, the properties of the obtained PLA / PPC composite materials can be improved to a certain extent. In one embodiment, the injection molding process is carried out according to the national standard GB / T 1040.2-2006, with a screw temperature of 160 / 180 / 170℃; an injection pressure of 35-40 bar; a holding time of 50 s; and a mold temperature of 20℃.

[0051] A drying step may also be included before melt blending PLA and PPC and / or before forming PLA / PPC composite materials from the blend masterbatch using an injection molding process to remove unwanted moisture from the materials. Drying can be performed using any drying method or equipment available in the art, such as infrared drying, oven drying, etc. In one embodiment, PLA and PPC chips are placed in an oven at 60°C and dried with air dried at 160°C for 10 hours. In another embodiment, the PLA / PPC blend masterbatch is placed in an oven at 60°C and dried with air dried at 160°C for 10 hours.

[0052] The ratio of PLA and PPC chips corresponds to the respective weight percentages of PLA and PPC in the PLA / PPC composite material and deformable biodegradable material. Appropriate PLA and PPC ratios contribute to the good mechanical properties and deformability of the deformable biodegradable material. With appropriate PLA and PPC ratios, the PPC segments within the deformable biodegradable material will orient themselves during gradual stretching, causing the material to turn white. Thanks to the good compatibility of PLA and PPC, the movement of PPC segments will uniformly disrupt the PLA segments, and due to the shape-preserving properties of PLA, the stretched material will not exhibit defects (such as necking).

[0053] In one embodiment, the PLA / PPC composite material comprises, by weight, 20-75 parts of polylactic acid and 25-80 parts of polypropylene carbonate. In a preferred embodiment, the PLA / PPC composite material comprises, by weight, 50-70 parts of polylactic acid and 30-50 parts of polypropylene carbonate. If the proportion of PPC is too low, the PLA / PPC composite material will fracture rapidly after reaching its yield point, thus failing to achieve effective stretching. As the proportion of PPC increases, the PLA / PPC composite material can be stretched further without defects (such as cracks, necking, etc.) (i.e., the higher the maximum stretch ratio of the material), indicating better ductility of the composite material. At a given stretch ratio, the better the ductility of the PLA / PPC composite material, the higher the stretching rate it can withstand. The higher the stretch ratio of the PLA / PPC composite material during the stretching process, the softer the deformable biodegradable material obtained after stretching, with lower flexural strength, higher notched impact strength, and stronger deformation capacity. However, when the proportion of PPC is too high, the maximum stretchability of PLA / PPC composites will decrease, and the heat resistance of the deformable and degradable material obtained after stretching PLA / PPC composites will deteriorate, that is, the temperature at which the material shrinks will be lower, which is not conducive to the shape stability of the corresponding products in practical applications.

[0054] This application achieves improved material properties through stretching. Therefore, in one embodiment, the PLA / PPC composite material does not contain additives. This is beneficial for reducing costs and also improves material safety, making it suitable for applications with high safety requirements (e.g., medical devices, protective gear).

[0055] Tensile testing of PLA / PPC composite materials

[0056] The inventors of this application have discovered that by cold-drawing PLA / PPC composite materials, the toughness of the material can be significantly improved (e.g., the notched impact strength can be greatly increased) while ensuring that no defects appear in the material. Furthermore, the cold-drawn material can undergo multiple deformations in any direction under external force. "Cold-drawing" as described herein refers to stretching the material at a relatively low temperature, for example, stretching the PLA / PPC composite material at a temperature of 0-30°C. In one embodiment, the PLA / PPC composite material is stretched at a temperature of 0-30°C to obtain a deformable biodegradable material, wherein the stretching ratio does not exceed the maximum stretching ratio of the PLA / PPC composite material.

[0057] The parameter settings during the stretching process have a significant impact on material properties. The stretching process parameters in this application (such as temperature, stretching ratio, and stretching speed) enable the product to obtain different degrees of mechanical properties to meet the performance requirements of different applications. In particular, they can form a good matching effect with the PLA / PPC composite material with the specific composition of this application, so that the material undergoing stretching can obtain more suitable properties.

[0058] It should be understood that during the stretching process at a specific temperature, the material and the environment essentially reach thermal equilibrium, meaning the stretched material is at or near the same temperature as the environment. This is to obtain a deformable and biodegradable material. The temperature during the stretching process affects the material's stretchability; a suitable temperature ensures the desired stretching process for the PLA / PPC composite material is achieved. In one embodiment, the PLA / PPC composite material is stretched at a temperature of 0-30°C, preferably 10-30°C, and more preferably 15-20°C. If the stretching temperature is too high, the displacement at the point where the material necks decreases, i.e., the maximum stretchability ratio decreases; while if the temperature is too low, the stretched material may experience brittle fracture, which is also detrimental to the material's stretchability.

[0059] The maximum stretchable dimension of a PLA / PPC composite material is the largest dimension to which it can be stretched without defects (such as cracks, necking, or fracture). The presence of defects can be visually assessed. Furthermore, this application reveals that the maximum stretchable dimension of a material can be determined by stress changes within the material. When the material passes its yield point, a first stress drop occurs; subsequently, the material can be gradually stretched and elongated with almost constant stress; as the amount of tensile displacement increases, a second stress drop occurs. The inventors discovered that between the first stress drop (yield point) and the second stress drop, the material can be stretched without defects; however, after the second stress drop, continued stretching will lead to defects. Therefore, the dimension at which the second stress drop occurs can represent its maximum stretchable dimension.

[0060] A suitable stretch ratio can give the stretched material good flexibility and deformation capacity. In one embodiment, the ratio of the stretch ratio to the maximum stretch ratio of the PLA / PPC composite material is 0.1-0.9, preferably 0.6-0.8, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, etc. This preferred ratio can impart the desired properties to the stretched material, while the stretched material (i.e., deformable and degradable material) can still retain a certain stretchability during deformation, which is beneficial for shaping the stretched material (i.e., deformable and degradable material) in various ways without producing defects. In another embodiment, the stretch ratio of the PLA / PPC composite material stretching process is 1.1-2.0, preferably 1.3-1.6, for example, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, etc. If the draw ratio is too low, the material's toughness cannot be effectively improved. Increasing the draw ratio helps improve the material's flexibility and deformation capacity. Better deformation capacity allows the material to undergo more complex deformations, expanding its application scenarios. If the draw ratio is too high, the material is more likely to develop necks, and the deformation capacity of the necked portion will decrease.

[0061] The stretching rate affects the maximum stretchability of the material. A lower stretching rate results in a greater maximum stretchable displacement, which allows for good flexibility and deformation capacity even in PLA / PPC composites with a low PPC content. In one embodiment, the stretching rate during the stretching process of the PLA / PPC composite is 1-50 mm / min, preferably 2-20 mm / min, such as 1 mm / min, 2 mm / min, 3 mm / min, 4 mm / min, 5 mm / min, 6 mm / min, 8 mm / min, 10 mm / min, 15 mm / min, 18 mm / min, 20 mm / min, 25 mm / min, 30 mm / min, 35 mm / min, 40 mm / min, 45 mm / min, 50 mm / min, etc.

[0062] The tensile process can be performed using conventional equipment in the field, including but not limited to: universal testing machines.

[0063] The following illustrates a specific implementation scheme for the preparation of deformable and biodegradable materials:

[0064] Step (1) Pretreatment: Place PLA and PPC slices in an oven at 60°C and dry them for 10 hours by passing in air that has been dried at 160°C.

[0065] Step (2) Melt blending and granulation: The PLA and PPC chips from step (1) are blended in different proportions and then added to a twin-screw extruder for granulation. The screw temperature is 150-180℃, the rotation speed is 200-300rpm, and the time is 0.5-2min. The cooling method during granulation is air cooling. The PLA part is 10-80 parts and the PPC part is 20-90 parts.

[0066] Step (3) Sample preparation: After drying the blended masterbatch from step (2) under the drying conditions of step (1) for 3 hours, it is injection molded into 1A tensile test strips (i.e. PLA / PPC composite material) according to the national standard GB / T 1040.2-2006. The screw temperature is 160 / 180 / 170℃; the injection pressure is 35-40 bar; the holding time is 50s; and the mold temperature is 20℃.

[0067] Step (4) Strip stretching: The strip from step (3) is cold-stretched at a temperature of 0-30℃ on a universal testing machine at a rate of 1-50 mm / min. The actual length of the stretched portion of the strip is 80 mm, which is calculated based on a stretching ratio of 1.1-2.0, i.e., 8-80 mm. The strip is stretched until it turns white, and no cracks or necks appear. This stretched portion of the material is the deformable and biodegradable material of this application.

[0068] Deformable and biodegradable materials

[0069] On the other hand, this application also relates to deformable and biodegradable materials prepared by the above-described preparation method. The deformable and biodegradable materials of this application possess excellent toughness; they can deform multiple times in any direction under external force, and the material does not spring back after the external force is removed.

[0070] In this application, the deformable and biodegradable material is placed in an environment of 20-25℃ for a sufficient period of time until the size of the deformable and biodegradable material no longer changes, and then the material is tested for performance.

[0071] Notched impact strength: An indicator for measuring the toughness of the deformable and biodegradable material in this invention, defined as the energy absorbed per unit cross-sectional area when the specimen breaks or fractures under impact load. In this invention, the notched impact strength can be tested using a simply supported beam impact testing machine according to the national standard GB / T 1843-2008. The notched impact strength of the deformable and biodegradable material of this invention can be approximately 6.5 kJ / m. 2 The above describes the improvement in toughness of the material after stretching. In one embodiment, the notched impact strength of the deformable biodegradable material is more than five times that of the PLA / PPC composite material.

[0072] The flexural strength and flexural modulus of deformable and biodegradable materials can be used to characterize their mechanical properties. The flexural strength and flexural modulus can be determined by a three-point bending test according to national standard GB / T 9341-2008 at a test speed of 2 mm / min. In one embodiment, the flexural strength of the deformable and biodegradable material is 10-60 MPa. In another embodiment, the flexural modulus of the deformable and biodegradable material is 1000-3000 MPa. The deformable and biodegradable material of this application possesses suitable flexural strength and flexural modulus, giving it not only excellent deformation capacity but also good load-bearing capacity, which is beneficial for maintaining the shape after deformation.

[0073] Deformable and biodegradable products

[0074] On the other hand, this application relates to a deformable biodegradable article comprising the deformable biodegradable material of this application.

[0075] The deformable biodegradable material of this application has excellent deformability and can deform in any direction and in any manner, including but not limited to bending, twisting, and stretching. Therefore, the deformable biodegradable article of this application can have excellent shape flexibility.

[0076] The deformable and biodegradable article of this application may also include unstretched PLA / PPC composite material. The stretching process described in this application can be performed on a localized portion of the PLA / PPC composite material; therefore, the resulting article can simultaneously comprise both the deformable material and the unstretched PLA / PPC composite material. Such an article offers a simple and efficient preparation method with unexpected advantages: by stretching a localized portion of a PLA / PPC composite material with the same composition, the properties of that portion of the material can be adjusted, resulting in a monolithic article with differentiated local properties. The stretched PLA / PPC composite material (i.e., the deformable and biodegradable material of this application) possesses deformability and better toughness to meet the need for shape changes, while the unstretched PLA / PPC composite material maintains good rigidity, providing support for the article. Therefore, the article composed of stretched and unstretched PLA / PPC composite materials not only possesses the advantages of a monolithic component (e.g., good bonding strength) but also has flexibly adjustable local properties.

[0077] Beneficial effects

[0078] The method for preparing deformable and biodegradable materials of this invention is simple to operate, requires minimal equipment, and offers advantages such as low cost and high efficiency. The deformable and biodegradable materials prepared by this method do not pollute the environment and can mitigate the greenhouse effect, demonstrating green and environmentally friendly advantages. The deformable and biodegradable materials of this invention, after specific stretching treatment, do not require the introduction of additional modifying additives, and their toughness, notched impact strength, and other properties are significantly improved. Furthermore, the deformable and biodegradable materials of this invention can undergo multiple deformations in any direction under external force and possess excellent load-bearing capacity. Further, in the method of this application, by adjusting the raw material composition of the PLA / PPC composite material and the parameters during the stretching process, the mechanical properties of the product can be effectively controlled to meet the performance requirements of different applications, thus broadening the application fields of the PLA / PPC composite system.

[0079] Example

[0080] The present invention will now be described in further detail with reference to specific embodiments.

[0081] It should be noted that the following embodiments are merely examples to clearly illustrate the technical solutions of the present invention, and are not intended to limit the present invention. For those skilled in the art, other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here, and obvious variations or modifications derived therefrom are still within the protection scope of this invention. Unless otherwise specified, the instruments, equipment, and reagents used herein are commercially available.

[0082] Material

[0083] Polylactic acid (PLA): Purchased from Hisun Biomaterials Co., Ltd.; brand name: REVODE 101.

[0084] Polypropylene carbonate (PPC): Purchased from Zhejiang Huafeng Environmental Protection Materials Co., Ltd.; Grade: HF 901.

[0085] Poly(3-hydroxybutyric acid) (PHB): Purchased from Guangdong Hefeng Biotechnology Co., Ltd.; Brand: MDF1000.

[0086] Polybutylene succinate (PBS): purchased from Xinjiang Lanshan Tunhe Polyester Co., Ltd.; brand name: TH803S.

[0087] Polybutylene adipate / terephthalate (PBAT): Purchased from Xinjiang Lanshan Tunhe Polyester Co., Ltd.; Grade: TH801T.

[0088] equipment

[0089] Twin-screw extruder: Nanjing Keya Chemical Complete Equipment Co., Ltd., model HK26.

[0090] Injection molding machine: Changzhou Aobo Injection Molding Machinery Co., Ltd., model ABL200.

[0091] Universal testing machine: Shenzhen Sansi Zongheng Technology Co., Ltd., model UTM4503X.

[0092] Simply supported beam impact testing machine: Jiangsu Tianyuan Testing Equipment Co., Ltd., model TY-4020A.

[0093] Oven: Dongguan Xinyi Electric Heating Machinery Co., Ltd., Model CD-9.

[0094] Water bath: Changzhou Yuexin Instrument Manufacturing Co., Ltd., Model HH-1.

[0095] preparation

[0096] Samples for the examples and comparative examples were prepared according to the following procedures and Table 1:

[0097] Step (1) Pretreatment: Place the raw material slices in an oven at 60°C and dry them for 10 hours by passing in air that has been dried at 160°C.

[0098] Step (2) Melt blending and granulation: The raw material slices from step (1) are blended in different weight parts (see Table 1 below) and then added to a twin-screw extruder for granulation. The screw temperature is 150-180℃, the rotation speed is 200-300rpm, and the time is 0.5-2min. The cooling method during the granulation process is air cooling.

[0099] Step (3) Sample preparation: After drying the masterbatch from step (2) under the drying conditions of step (1) for 3 hours, it is injection molded into 1A material specimens to be stretched according to the national standard GB / T 1040.2-2006. The screw temperature is 160 / 180 / 170℃; the injection pressure is 35-40 bar; the holding time is 50s; and the mold temperature is 20℃.

[0100] Step (4) Strip stretching treatment: The material strip to be stretched in step (3) is stretched at a certain temperature and a certain stretching rate on a universal testing machine. A portion of 80 mm in length is selected on the material strip to be stretched as the actual stretching portion. According to a certain stretching ratio, the actual stretching portion is stretched to the corresponding size. This stretched material strip is the sample of the example and comparative example.

[0101] Table 1

[0102]

[0103]

[0104] Note: "Tension displacement*" refers to the difference between the size to which the spline is stretched when an external force is applied and the original size of the spline (i.e., 80 mm).

[0105] "Actual tensile displacement**" refers to the difference between the actual size of the specimen and the initial size (i.e., 80 mm) after the specimen has been stretched, the external force applied to it has been removed, and it has been placed in an environment of 20-25℃ for a sufficient period of time until the specimen size has stabilized.

[0106] Performance testing

[0107] Notched impact strength: Tested using a simply supported beam impact testing machine according to GB / T 1843-2008.

[0108] Bending strength and bending modulus: GB / T 9341-2008 Three-point bending test, test speed 2mm / min.

[0109] According to the above test method, the stretched material specimens of the examples and comparative examples were measured, and the data shown in Table 2 below were obtained.

[0110] Table 2

[0111]

[0112]

[0113] Figure 1 Stress-displacement curves of PPC / PLA composite specimens with different PPC contents at 18°C ​​and a tensile rate of 5 mm / min are shown. The specimen preparation process is the same as that described in the examples above. At a tensile rate of 5 mm / min, when the PPC content is low, for example, a PPC / PLA composite specimen composed of 20 parts by weight of PPC and 80 parts by weight of PLA, the specimen fractures rapidly after reaching the yield point (i.e., the first stress reduction). Figure 1 The PPC20 curve is shown. When the PPC content is high, the material can be gradually stretched after passing the yield point, and the stress will decrease again with the increase of the stretching ratio (i.e., the stress decreases for the second time). Before the stress decreases for the second time, no defects will appear in the material during stretching. When the material is stretched to the stretching displacement at which the stress decreases for the second time (i.e., the maximum stretchable displacement), and stretching continues, defects will appear in the material. For example, a PPC / PLA composite sample composed of 30 parts by weight of PPC and 70 parts by weight of PLA will fracture (e.g., Figure 1As shown in the PPC30 curve, the PPC / PLA composite sample composed of 40 parts by weight of PPC and 60 parts by weight of PLA exhibits a neck (as shown in the curve). Figure 1 As shown in the PPC40 curve, the PPC / PLA composite sample composed of 70 parts by weight of PPC and 30 parts by weight of PLA gradually tapers in width and then shows a neck (as shown in the curve). Figure 1 (As shown in the PPC70 curve).

[0114] Figure 2 Stress-displacement curves of a PLA / PPC composite specimen composed of 40 parts by weight of PPC and 60 parts by weight of PLA are shown at 18°C ​​and different tensile rates. The specimen preparation process is the same as that described in the examples above. Figure 2 As can be seen, the stretching rate significantly affects the maximum stretchable displacement of the material. The lower the stretching rate, the higher the stretchable displacement at the second stress reduction point, i.e., the higher the maximum stretchable displacement. This indicates that by reducing the stretching rate, the maximum stretchable displacement (and maximum stretch ratio) of samples with lower PPC content can be increased.

[0115] Figure 3 The images show photographs of stretched material strips from embodiments of this application, as well as comparative examples of unstretched material strips. Figure 3 As can be seen, in the embodiments, the stretched spline did not exhibit any defects, cracks, or necks. The stretched portion turned white and did not show significant thinning in the width direction. As shown in Table 2, the toughness of the stretched material in the embodiments was greatly improved, the notched impact strength was significantly increased, and the flexural modulus was significantly reduced.

[0116] The material strip stretched according to the embodiments of this application can deform multiple times in any direction under the action of external force, and does not spring back after the external force is removed. Figure 4 The force-displacement curves of the material specimens of Embodiments 2, 6-8 and Comparative Example 2 of the present invention are shown at 23°C and a compression rate of 2 mm / min. Figure 5 The material's appearance after deformation is shown, demonstrating its ability to deform in different spaces.

[0117] As can be seen from Examples 2 and 6-9, during the stretching process, the higher the stretching ratio, the better the flexibility of the stretched material. In Example 8, with a stretching ratio of 1.4, compared to the unstretched material (Comparative Example 2), its notched impact strength increased by nearly 11 times, and its flexural modulus decreased by 70%.

[0118] During stretching, the higher the stretch ratio, the stronger the material's deformation capacity. For example... Figure 4As shown, under the same bending displacement, the higher the tensile ratio of the specimen, the smaller the force required for deformation, meaning the specimen is more easily deformed under stress, and better deformation capacity enables the material to undergo more complex deformation.

[0119] As can be seen from Examples 5 and 10-11, under the same stretching ratio, the mechanical properties of the stretched material are basically the same when the stretching rate is different.

[0120] During stretching, temperature affects the maximum stretchable displacement of the material. If the temperature is too high during stretching, the displacement will be smaller when the specimen develops a neck. Figure 1 It can be seen that for the PPC60 curve with a stretching temperature of 18°C ​​(where the PPC content is 60 parts by weight and the PLA content is 40 parts by weight), the maximum stretchable displacement is approximately 70 mm; in Example 12, the stretching temperature is 24°C, and the maximum stretchable displacement is approximately 20 mm. If the stretching temperature is too low, the material will experience brittle fracture during the stretching process.

[0121] This application further verifies the dimensional stability of the stretched material in the service environment. The stretched material samples were immersed in water at different temperatures for a certain period of time, and then removed to measure the length and mechanical properties of the samples. The test data are shown in Table 3 below. According to Table 3, the samples of Example 2 did not shrink after being immersed in water at 23℃ and 36℃, and their mechanical properties were essentially maintained.

[0122] Table 3

[0123]

[0124] In summary, this application effectively regulates the mechanical properties and deformability of the material by controlling the composition of the composite material and parameters during the stretching process (such as stretching ratio, stretching rate, and temperature). The deformable and biodegradable material of this application has great application potential in fields such as medical devices, protective gear, toys, and daily necessities.

[0125] Those skilled in the art will recognize that many modifications and variations can be made to this invention without departing from its spirit and scope. The specific embodiments described herein are provided by way of example only and are not intended to limit the scope in any way. The true scope and spirit of the invention are shown in the appended claims, and the description and embodiments are merely exemplary.

Claims

1. A method for preparing a deformable and biodegradable material, comprising the following steps: A PLA / PPC composite material is provided, wherein, by weight, the PLA / PPC composite material comprises: 50-70 parts of polylactic acid and 30-50 parts of polypropylene carbonate; The PLA / PPC composite material is stretched at a temperature of 10-30°C to obtain the deformable and degradable material, wherein the stretching ratio does not exceed the maximum stretching ratio of the PLA / PPC composite material. in, The ratio of the stretching ratio to the maximum stretchable ratio of the PLA / PPC composite material is 0.6-0.8; The stretching ratio is 1.3-1.6; The stretching rate is 2-20 mm / min.

2. The method of claim 1, wherein, The stretching temperature is 15-20℃.

3. The method of claim 1, wherein, The PLA / PPC composite material is provided through the following steps: Polylactic acid and polypropylene carbonate are melt-blended and then granulated to form a blend masterbatch. The blended masterbatch is used to prepare the PLA / PPC composite material.

4. The method according to any one of claims 1-3, wherein, The PLA / PPC composite material does not contain any additives.

5. A deformable and biodegradable material, which is prepared by the method of any one of claims 1-4.

6. The deformable and biodegradable material of claim 5, wherein, The deformable and biodegradable material has a flexural strength of 10-60 MPa; and / or The deformable and biodegradable material has a flexural modulus of 1000-3000 MPa; and / or The notched impact strength of the deformable and biodegradable material is 6.5 kJ / m. 2 The above; and / or The notched impact strength of the deformable and biodegradable material is more than 5 times that of the notched impact strength of the PLA / PPC composite material.

7. A deformable and biodegradable article comprising the deformable and biodegradable material of claim 5 or 6.

Citation Information

Patent Citations

  • Reinforced and toughened polylactic acid material and preparation method thereof

    CN114350128A

  • Preparation method of PLA / PPC composite material with improved toughness and optical performance