A kind of high efficiency corrosion and scale inhibitor and preparation method thereof

The high-efficiency corrosion inhibitor is prepared by emulsifying cross-linking method of modified chitosan porous microspheres and thiolated benzimidazole, which solves the scale and metal corrosion problems in the circulating cooling water system, and achieves excellent scale and corrosion inhibition and corrosion inhibition performance , improve industrial production efficiency and resource utilization.

CN118561436BActive Publication Date: 2024-11-19BEIJING PENGFA ENVIRONMENTAL PROTECTION GRP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410832585.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-19
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

The scale formation and metal corrosion problems caused by the increase in the concentration of anion and cations in the circulating cooling water system affect equipment operation and resource utilization efficiency.

Method used

The highly effective corrosion inhibitor is prepared by emulsifying cross-linking method by modifying chitosan porous microspheres and thiolated benzimidazole. The metal cations are chelated by amide groups and carboxylic acid groups, and the metal surface is formed by sulfhydryl groups. Position bonds form a dense adsorption film to protect the metal surface.

Benefits of technology

It significantly improves scale resistance and corrosion inhibition performance, extends the service life of the equipment, reduces water quality deterioration and resource waste, and improves industrial production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

The invention discloses a high-efficiency corrosion and scale inhibitor and a preparation method thereof, and relates to the technical field of scale inhibitors. When preparing the high-efficiency corrosion and scale inhibitor, the present invention reacts 2-aminobenzimidazole and 3-chloro-1-propanethiol to obtain mercaptobenzimidazole; chitosan and methyl acrylate are reacted to obtain pre-modified chitosan; the pre-modified chitosan is prepared into an emulsion, tris(2-aminoethyl)amine is used as a cross-linking agent, and chitosan porous microspheres are prepared by an emulsification cross-linking method; chitosan porous microspheres and maleic anhydride are reacted to obtain modified chitosan porous microspheres; modified chitosan porous microspheres and mercaptobenzimidazole are reacted to obtain a high-efficiency corrosion and scale inhibitor. The high-efficiency corrosion and scale inhibitor prepared by the present invention has excellent corrosion inhibition and scale inhibition performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of scale inhibitors, in particular to a high-efficiency corrosion and scale inhibitor and a preparation method thereof. Background Art

[0002] The circulating cooling water system plays a vital role in industrial production. The demand for water resources in industries such as petroleum, chemical, and electric power is very large. The circulating cooling system is mainly composed of heat exchange equipment, cooling equipment, water pumps, pipes and other equipment. The circulating cooling system in industrial production can effectively save water resources by increasing the concentration multiple. Circulating cooling water usually contains a large number of incompatible anions and cations. With the increase of concentration multiples, water temperature, leakage of process media and other comprehensive factors, the concentration of various anions and cations in the cooling water will increase exponentially. These anions and cations are easy to form inorganic salt scale and adhere to the pipe wall of the circulating cooling water system. The scale attached to the pipe wall will affect the heat transfer efficiency of the heat exchanger and cause the blockage of the pipeline. The long-term existence of the scale is a consumption of the equipment, and it also affects the normal operation of the circulating cooling water system. At the same time, the dissolved oxygen in the water can corrode the metal in the system. Since the circulating cooling water system is generally a relatively closed system, the long-term operation of the system causes the scale to accumulate and the metal to corrode, causing the water quality to gradually deteriorate. Based on the above problems, an efficient corrosion and scale inhibitor is invented to save resources, save industrial production costs and greatly improve industrial production efficiency. Summary of the invention

[0003] The purpose of the present invention is to provide a high-efficiency corrosion and scale inhibitor and a preparation method thereof, so as to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] A highly efficient corrosion and scale inhibitor, wherein the highly efficient corrosion and scale inhibitor is prepared by reacting chitosan porous microspheres with maleic anhydride to obtain modified chitosan porous microspheres; and reacting the modified chitosan porous microspheres with mercaptolated benzimidazole to obtain the highly efficient corrosion and scale inhibitor;

[0006] The chitosan porous microspheres are prepared by preparing pre-modified chitosan into an emulsion, using tri(2-aminoethyl)amine as a cross-linking agent, and adopting an emulsification cross-linking method.

[0007] The pre-modified chitosan is prepared by reacting chitosan and methyl acrylate;

[0008] The thiolated benzimidazole is prepared by reacting 2-aminobenzimidazole and 3-chloro-1-propanethiol.

[0009] A method for preparing a high-efficiency corrosion and scale inhibitor comprises the following preparation steps:

[0010] (1) Add 2-aminobenzimidazole and 3-chloro-1-propanethiol in a molar ratio of 1:1 to toluene with a mass of 10 to 12 times that of 2-aminobenzimidazole, add an acid-binding agent with a mass of 0.03 to 0.05 times that of 2-aminobenzimidazole, stir at 55 to 65°C and 300 to 500 r / min for 2 to 3 hours under nitrogen protection, and dry at 50 to 60°C for 7 to 8 hours under vacuum conditions to obtain thiolated benzimidazole;

[0011] (2) Pre-modified chitosan and 3-5% acetic acid aqueous solution were mixed in a mass ratio of 1:(26-30) to prepare a dispersed phase; at 10-30°C and 300-500 r / min stirring conditions, 0.6-0.8 times the mass of the dispersed phase was uniformly added to the continuous phase within 30 minutes, and then 0.3-0.5 times the mass of the dispersed phase was added. The reaction was continued with stirring for 4-5 hours, centrifuged, washed with acetone and anhydrous ethanol for 3-5 times each, and dried at 50-60°C under vacuum conditions for 7-8 hours to obtain chitosan porous microspheres;

[0012] (3) Chitosan porous microspheres, maleic anhydride, 1,4-benzoquinone, and N,N-dimethylformamide were mixed uniformly in a mass ratio of 1:1.1-1.3:0.02-0.04:8-10, stirred at 50-60°C and 300-500 r / min for 10-12 h, filtered, washed with anhydrous ethanol 3-5 times, and dried at 50-60°C under vacuum for 7-8 h to obtain modified chitosan. Porous microspheres; the modified chitosan porous microspheres, thiolated benzimidazole, azobisisobutyronitrile and toluene are mixed evenly in a mass ratio of 1:1.1~1.3:0.03~0.05:8~10, stirred at 70~80℃ and 300~500r / min for 3~4h, filtered, washed with anhydrous ethanol for 3~5 times, dried at 50~60℃ under vacuum conditions for 7~8h, to obtain a high-efficiency corrosion and scale inhibitor.

[0013] As an optimization, the acid binding agent in step (1) is triethylamine.

[0014] As an optimization, the reaction process of the thiolated benzimidazole in step (1) is:

[0015] .

[0016] As an optimization, the pre-modified chitosan in step (2) is prepared by uniformly mixing chitosan and methanol in a mass ratio of 1:(10-12), adding methyl acrylate in an amount of 1.1-1.3 times the mass of chitosan at a uniform rate within 2 hours at 0-2°C and 300-500 r / min stirring under nitrogen protection, heating to 28-32°C, continuing to stir and react for 20-24 hours, and drying at 50-60°C for 7-8 hours under vacuum conditions;

[0017] The reaction process is:

[0018] .

[0019] As an optimization, the deacetylation degree of the chitosan is 80-86%.

[0020] As an optimization, the continuous phase in step (2) is prepared by uniformly mixing Span 80, sorbitan monooleate polyoxyethylene ether, and petroleum ether in a mass ratio of 1:1:(40-50).

[0021] As an optimization, the cross-linking agent in step (2) is tris(2-aminoethyl)amine.

[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0023] When preparing the high-efficiency corrosion and scale inhibitor, the present invention comprises the following steps: 2-aminobenzimidazole and 3-chloro-1-propanethiol are reacted to obtain mercaptobenzimidazole; chitosan and methyl acrylate are reacted to obtain pre-modified chitosan; the pre-modified chitosan is prepared into an emulsion, tri(2-aminoethyl)amine is used as a cross-linking agent, and an emulsification cross-linking method is adopted to obtain chitosan porous microspheres; the chitosan porous microspheres and maleic anhydride are reacted to obtain modified chitosan porous microspheres; and the modified chitosan porous microspheres and mercaptobenzimidazole are reacted to obtain the high-efficiency corrosion and scale inhibitor.

[0024] First, chitosan and methyl acrylate are reacted to prepare pre-modified chitosan, and the amino groups on the chitosan react with the carbon-carbon double bonds on the methyl acrylate to undergo Michael addition reaction, thereby introducing ester bonds on the chitosan; the pre-modified chitosan is prepared into an emulsion, tri(2-aminoethyl)amine is used as a cross-linking agent, and chitosan porous microspheres are prepared by an emulsion cross-linking method, and the ester bonds on the pre-modified chitosan react with the amino groups on the tri(2-aminoethyl)amine to cross-link the chitosan and simultaneously introduce A large number of amide groups are stable in nature and can chelate metal cations in the solution, giving the high-efficiency corrosion and scale inhibitor excellent scale inhibition performance; chitosan porous microspheres are reacted with maleic anhydride to obtain modified chitosan porous microspheres; the anhydride on the maleic anhydride reacts with the hydroxyl group on the chitosan to form an ester bond, and carboxyl groups and carbon-carbon double bonds are introduced into the modified chitosan porous microspheres; the carboxylic acid group also has the performance of chelating metal cations in the solution, further improving the scale inhibition performance of the high-efficiency corrosion and scale inhibitor.

[0025] Secondly, 2-aminobenzimidazole and 3-chloro-1-propanethiol are reacted to obtain thiolated benzimidazole, and the modified chitosan porous microspheres and thiolated benzimidazole are reacted to obtain a high-efficiency corrosion and scale inhibitor; the thiol group on the thiolated benzimidazole reacts with the carbon-carbon double bond on the modified chitosan porous microspheres to introduce a benzimidazole structure on the modified chitosan porous microspheres; the two nitrogen atoms in the benzimidazole molecular structure contain lone pairs of electrons, which are easy to form coordination bonds with empty d orbitals of metal atoms such as Fe and Cu, and are adsorbed on the metal surface to form a dense adsorption film, thereby achieving the effect of protecting the metal surface and giving the high-efficiency corrosion and scale inhibitor excellent corrosion inhibition performance. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] Example 1: A method for preparing a highly efficient corrosion and scale inhibitor, the method for preparing a highly efficient corrosion and scale inhibitor comprising the following preparation steps:

[0028] (1) 2-aminobenzimidazole and 3-chloro-1-propanethiol were added in a molar ratio of 1:1 to toluene (10 times the mass of 2-aminobenzimidazole), and triethylamine (0.03 times the mass of 2-aminobenzimidazole) was added. The mixture was stirred at 55°C and 300 r / min for 3 h under nitrogen protection, and dried at 50°C for 8 h under vacuum to obtain thiolated benzimidazole.

[0029] (2) Chitosan and methanol were mixed at a mass ratio of 1:10, and methyl acrylate (1.1 times the mass of chitosan) was added dropwise at a uniform rate within 2 hours at 0°C and 300 r / min under nitrogen protection. The temperature was raised to 28°C, and the reaction was continued with stirring for 24 hours. The pre-modified chitosan was obtained by drying at 50°C under vacuum for 8 hours. The pre-modified chitosan and 3% acetic acid aqueous solution were mixed at a mass ratio of 1:26 to prepare a dispersed phase. Span 80 and dehydrated sorbitan were added. Sorbitol monooleate polyoxyethylene ether and petroleum ether were mixed uniformly at a mass ratio of 1:1:40 to prepare a continuous phase; under the stirring conditions of 10°C and 300r / min, a dispersed phase with a mass of 0.6 times the mass of the continuous phase was uniformly added dropwise to the continuous phase within 30 minutes, and then tri(2-aminoethyl)amine with a mass of 0.3 times the mass of the dispersed phase was added, and the reaction was continued with stirring for 5 hours, centrifuged, washed with acetone and anhydrous ethanol for 3 times each, and dried at 50°C for 8 hours under vacuum conditions to obtain chitosan porous microspheres;

[0030] (3) Chitosan porous microspheres, maleic anhydride, 1,4-benzoquinone, and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:1.1:0.02:8, stirred at 50°C and 300 r / min for 12 h, filtered, washed with anhydrous ethanol three times, and dried at 50°C under vacuum conditions for 8 h to obtain modified chitosan porous microspheres; modified chitosan porous microspheres, thiolated benzimidazole, azobisisobutyronitrile, and toluene were mixed evenly in a mass ratio of 1:1.1:0.03:8, stirred at 70°C and 300 r / min for 4 h, filtered, washed with anhydrous ethanol three times, and dried at 50°C under vacuum conditions for 8 h to obtain a high-efficiency corrosion and scale inhibitor.

[0031] Example 2: A method for preparing a highly efficient corrosion and scale inhibitor, the method for preparing a highly efficient corrosion and scale inhibitor comprising the following preparation steps:

[0032] (1) 2-aminobenzimidazole and 3-chloro-1-propanethiol were added in a molar ratio of 1:1 to toluene (11 times the mass of 2-aminobenzimidazole), and triethylamine (0.04 times the mass of 2-aminobenzimidazole) was added. The mixture was stirred at 60°C and 400 r / min for 2.5 h under nitrogen protection, and dried at 55°C for 7.5 h under vacuum conditions to obtain thiolated benzimidazole.

[0033] (2) Chitosan and methanol were mixed in a mass ratio of 1:11, and methyl acrylate (1.2 times the mass of chitosan) was added dropwise at a uniform rate within 2 hours at 1°C and 400 r / min under nitrogen protection. The temperature was raised to 29°C, and the stirring reaction was continued for 22 hours. Under vacuum conditions, it was dried at 55°C for 7.5 hours to obtain pre-modified chitosan. Pre-modified chitosan and 4% acetic acid aqueous solution were mixed in a mass ratio of 1:28 to prepare a dispersed phase. Span 80 and Sorbus anhydrous were added. Alcohol monooleate polyoxyethylene ether and petroleum ether are mixed uniformly in a mass ratio of 1:1:45 to prepare a continuous phase; under the stirring conditions of 20°C and 400r / min, a dispersed phase with a mass of 0.7 times the mass of the continuous phase is uniformly added dropwise to the continuous phase within 30 minutes, and then tri(2-aminoethyl)amine with a mass of 0.4 times the mass of the dispersed phase is added, and the stirring reaction is continued for 4.5 hours, centrifuged, washed with acetone and anhydrous ethanol for 4 times respectively, and dried at 55°C for 7.5 hours under vacuum conditions to obtain chitosan porous microspheres;

[0034] (3) Chitosan porous microspheres, maleic anhydride, 1,4-benzoquinone, and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:1.2:0.03:9, stirred at 55°C and 400 r / min for 11 h, filtered, washed with anhydrous ethanol 4 times, and dried at 55°C under vacuum for 7.5 h to obtain modified chitosan porous microspheres; modified chitosan porous microspheres, thiolated benzimidazole, azobisisobutyronitrile, and toluene were mixed evenly in a mass ratio of 1:1.2:0.04:9, stirred at 75°C and 400 r / min for 3.5 h, filtered, washed with anhydrous ethanol 4 times, and dried at 55°C under vacuum for 7.5 h to obtain a high-efficiency corrosion and scale inhibitor.

[0035] Example 3: A method for preparing a highly efficient corrosion and scale inhibitor, the method for preparing a highly efficient corrosion and scale inhibitor comprising the following preparation steps:

[0036] (1) 2-aminobenzimidazole and 3-chloro-1-propanethiol were added in a molar ratio of 1:1 to toluene (12 times the mass of 2-aminobenzimidazole), and triethylamine (0.05 times the mass of 2-aminobenzimidazole) was added. The mixture was stirred at 65°C and 500 r / min for 2 h under nitrogen protection, and dried at 60°C for 7 h under vacuum to obtain thiolated benzimidazole.

[0037] (2) Chitosan and methanol were mixed in a mass ratio of 1:12, and methyl acrylate (1.3 times the mass of chitosan) was added dropwise at a uniform rate within 2 hours at 2°C and 500 r / min under nitrogen protection. The temperature was raised to 32°C, and the reaction was continued with stirring for 20 hours. The pre-modified chitosan was obtained by drying at 60°C under vacuum for 7 hours. The pre-modified chitosan and 5% acetic acid aqueous solution were mixed in a mass ratio of 1:30 to prepare a dispersed phase. Span 80 and dehydrated sorbitan were added. Sorbitol monooleate polyoxyethylene ether and petroleum ether were mixed uniformly at a mass ratio of 1:1:50 to prepare a continuous phase; under the stirring conditions of 30°C and 500r / min, a dispersed phase with a mass 0.8 times that of the continuous phase was uniformly added dropwise to the continuous phase within 30min, and then tri(2-aminoethyl)amine with a mass 0.5 times that of the dispersed phase was added, and the reaction was continued with stirring for 4h, centrifuged, washed with acetone and anhydrous ethanol for 5 times each, and dried at 60°C for 7h under vacuum conditions to obtain chitosan porous microspheres;

[0038] (3) Chitosan porous microspheres, maleic anhydride, 1,4-benzoquinone, and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:1.3:0.04:10, stirred at 60°C and 500 r / min for 10 h, filtered, washed with anhydrous ethanol 5 times, and dried at 60°C for 7 h under vacuum conditions to obtain modified chitosan porous microspheres; modified chitosan porous microspheres, thiolated benzimidazole, azobisisobutyronitrile, and toluene were mixed evenly in a mass ratio of 1:1.3:0.05:10, stirred at 80°C and 500 r / min for 3 h, filtered, washed with anhydrous ethanol 5 times, and dried at 60°C for 7 h under vacuum conditions to obtain a high-efficiency corrosion and scale inhibitor.

[0039] Comparative Example 1

[0040] The preparation method of the high-efficiency corrosion and scale inhibitor of Comparative Example 1 is different from that of Example 2 in that step (1) is not performed, and step (3) is modified as follows: chitosan porous microspheres, maleic anhydride, 1,4-benzoquinone, and N,N-dimethylformamide are uniformly mixed in a mass ratio of 1:1.2:0.03:9, stirred at 55°C and 400 r / min for 11 hours, filtered, washed with anhydrous ethanol 4 times, and dried at 55°C under vacuum for 7.5 hours to obtain a high-efficiency corrosion and scale inhibitor. The remaining steps are the same as those of Example 2.

[0041] Comparative Example 2

[0042] The preparation method of the high-efficiency corrosion and scale inhibitor of Comparative Example 2 is different from that of Example 2 in step (2). Step (2) is modified as follows: chitosan and 4% acetic acid aqueous solution are mixed uniformly at a mass ratio of 1:28 to prepare a dispersed phase; Span 80, sorbitan monooleate polyoxyethylene ether, and petroleum ether are mixed uniformly at a mass ratio of 1:1:45 to prepare a continuous phase; under stirring conditions of 20°C and 400 r / min, 0.7 times the mass of the dispersed phase is uniformly added dropwise to the continuous phase within 30 minutes, and then 0.4 times the mass of the dispersed phase 1,5-glutaraldehyde is added, the reaction is continued to stir for 4.5 hours, centrifuged, washed with acetone and anhydrous ethanol 4 times each, and dried at 55°C under vacuum conditions for 7.5 hours to prepare chitosan porous microspheres. The remaining steps are the same as those of Example 2.

[0043] Comparative Example 3

[0044] The preparation method of the high-efficiency corrosion and scale inhibitor of Comparative Example 3 is different from that of Example 2 only in step (3), and step (3) is modified as follows: chitosan porous microspheres, acrylic acid, 1,4-benzoquinone, and N,N-dimethylformamide are mixed uniformly in a mass ratio of 1:1.2:0.03:9, stirred at 55°C and 400 r / min for 11 hours, filtered, washed with anhydrous ethanol 4 times, and dried at 55°C for 7.5 hours under vacuum conditions to obtain modified chitosan porous microspheres; modified chitosan porous microspheres, thiolated benzimidazole, azobisisobutyronitrile, and toluene are mixed uniformly in a mass ratio of 1:1.2:0.04:9, stirred at 75°C and 400 r / min for 3.5 hours, filtered, washed with anhydrous ethanol 4 times, and dried at 55°C for 7.5 hours under vacuum conditions to obtain a high-efficiency corrosion and scale inhibitor. The remaining steps are the same as those of Example 2.

[0045] Test Example 1

[0046] Test of scale inhibition performance

[0047] Test method: GB / T16632 "Calcium carbonate precipitation method" for the determination of scale inhibition performance of water treatment agents was used to determine the scale inhibition rates of the examples and comparative examples. The results are shown in Table 1.

[0048] Table 1

[0049]

[0050] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the high-efficiency corrosion and scale inhibitor prepared by the present invention has good scale inhibition performance.

[0051] By comparison, the scale inhibition rates of Examples 1 to 3 are greater than that of Comparative Example 2, indicating that pre-modified chitosan is prepared by reacting chitosan and methyl acrylate, and the amino groups on the chitosan react with the carbon-carbon double bonds on the methyl acrylate to undergo Michael addition reaction, thereby introducing ester bonds on the chitosan; the pre-modified chitosan is formulated into an emulsion, and tri(2-aminoethyl)amine is used as a cross-linking agent to prepare chitosan porous microspheres by an emulsification cross-linking method, and the ester bonds on the pre-modified chitosan react with the amino groups on the tri(2-aminoethyl)amine to cross-link the chitosan while introducing a large number of amide groups on the chitosan porous microspheres, the amide groups are stable in nature, can chelate metal cations in the solution, and give the high-efficiency corrosion and scale inhibitor excellent scale inhibition performance.

[0052] By comparison, the scale inhibition rates of Examples 1 to 3 are greater than that of Comparative Example 3, indicating that the chitosan porous microspheres and maleic anhydride are reacted to prepare modified chitosan porous microspheres; the anhydride on the maleic anhydride reacts with the hydroxyl groups on the chitosan to form ester bonds, and carboxyl groups are introduced into the modified chitosan porous microspheres; the carboxylic acid groups also have the property of chelating metal cations in the solution, further improving the scale inhibition performance of the high-efficiency corrosion and scale inhibitor.

[0053] Test Example 2

[0054] Corrosion inhibition performance test

[0055] Test method: The corrosion inhibition rates of the examples and comparative examples were measured using the "rotating coupon corrosion test method" of GB / T18175 national standard for the determination of corrosion inhibition performance of water treatment agents. The results are shown in Table 2.

[0056] Table 2

[0057]

[0058] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 2, it can be found that the high-efficiency corrosion and scale inhibitor prepared by the present invention has good corrosion inhibition performance.

[0059] By comparison, the corrosion inhibition rates of Examples 1 to 3 are greater than that of Comparative Example 1, indicating that the chitosan porous microspheres are reacted with maleic anhydride to obtain modified chitosan porous microspheres; the anhydride on the maleic anhydride reacts with the hydroxyl group on the chitosan to generate an ester bond, and a carbon-carbon double bond is introduced into the modified chitosan porous microspheres; 2-aminobenzimidazole and 3-chloro-1-propanethiol are reacted to obtain thiolated benzimidazole, and the modified chitosan porous microspheres and thiolated benzimidazole are reacted to obtain an efficient inhibition agent. Corrosion and scale inhibitor; the thiol group on the thiolated benzimidazole reacts with the carbon-carbon double bond on the modified chitosan porous microspheres to introduce the benzimidazole structure on the modified chitosan porous microspheres. The two nitrogen atoms in the benzimidazole molecular structure contain lone pairs of electrons, which are easy to form coordination bonds with the empty d orbitals of metal atoms such as Fe and Cu, and are adsorbed on the metal surface to form a dense adsorption film, thereby achieving the effect of protecting the metal surface and giving the high-efficiency corrosion and scale inhibitor excellent corrosion inhibition performance.

[0060] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A highly efficient corrosion and scale inhibitor, It is characterized in that The high-efficiency corrosion and scale inhibitor is prepared by reacting chitosan porous microspheres with maleic anhydride to obtain modified chitosan porous microspheres; and reacting modified chitosan porous microspheres with mercaptolated benzimidazole to obtain the high-efficiency corrosion and scale inhibitor. The chitosan porous microspheres are prepared by preparing pre-modified chitosan into an emulsion, using tri(2-aminoethyl)amine as a cross-linking agent, and adopting an emulsification cross-linking method; The pre-modified chitosan is prepared by reacting chitosan and methyl acrylate; The thiolated benzimidazole is prepared by reacting 2-aminobenzimidazole and 3-chloro-1-propanethiol.

2. A method for preparing a highly efficient corrosion and scale inhibitor, It is characterized in that The method comprises the following preparation steps: (1) Add 2-aminobenzimidazole and 3-chloro-1-propanethiol in a molar ratio of 1:1 to toluene with a mass of 10 to 12 times that of 2-aminobenzimidazole, add an acid-binding agent with a mass of 0.03 to 0.05 times that of 2-aminobenzimidazole, stir at 55 to 65°C and 300 to 500 r / min for 2 to 3 hours under nitrogen protection, and dry at 50 to 60°C for 7 to 8 hours under vacuum conditions to obtain thiolated benzimidazole; (2) Pre-modified chitosan and 3-5% acetic acid aqueous solution were mixed in a mass ratio of 1:(26-30) to prepare a dispersed phase; at 10-30°C and 300-500 r / min stirring conditions, 0.6-0.8 times the mass of the dispersed phase was uniformly added to the continuous phase within 30 minutes, and then 0.3-0.5 times the mass of the dispersed phase was added. The reaction was continued with stirring for 4-5 hours, centrifuged, washed with acetone and anhydrous ethanol for 3-5 times each, and dried at 50-60°C under vacuum conditions for 7-8 hours to obtain chitosan porous microspheres; (3) Chitosan porous microspheres, maleic anhydride, 1,4-benzoquinone, and N,N-dimethylformamide were mixed uniformly in a mass ratio of 1:1.1-1.3:0.02-0.04:8-10, stirred at 50-60°C and 300-500 r / min for 10-12 h, filtered, washed with anhydrous ethanol 3-5 times, and dried at 50-60°C under vacuum for 7-8 h to obtain modified chitosan. Porous microspheres; the modified chitosan porous microspheres, thiolated benzimidazole, azobisisobutyronitrile and toluene are mixed evenly in a mass ratio of 1:1.1~1.3:0.03~0.05:8~10, stirred at 70~80℃ and 300~500r / min for 3~4h, filtered, washed with anhydrous ethanol for 3~5 times, dried at 50~60℃ under vacuum conditions for 7~8h, to obtain a high-efficiency corrosion and scale inhibitor.

3. A method for preparing a high-efficiency corrosion and scale inhibitor according to claim 2, It is characterized in that The acid binding agent in step (1) is triethylamine.

4. The method for preparing a high-efficiency corrosion and scale inhibitor according to claim 2, It is characterized in that The reaction process of the thiolated benzimidazole in step (1) is as follows: 。 5. The method for preparing a high-efficiency corrosion and scale inhibitor according to claim 2, It is characterized in that The pre-modified chitosan in step (2) is prepared by uniformly mixing chitosan and methanol in a mass ratio of 1:(10-12), adding methyl acrylate in an amount of 1.1-1.3 times the mass of chitosan at a uniform rate within 2 hours at 0-2°C and 300-500 r / min stirring under nitrogen protection, heating to 28-32°C, continuing stirring and reacting for 20-24 hours, and drying at 50-60°C for 7-8 hours under vacuum conditions; The reaction process is: 。 6. A method for preparing a high-efficiency corrosion and scale inhibitor according to claim 5, It is characterized in that The deacetylation degree of the chitosan is 80-86%.

7. The method for preparing a high-efficiency corrosion and scale inhibitor according to claim 2, It is characterized in that The continuous phase in step (2) is prepared by uniformly mixing Span 80, sorbitan monooleate polyoxyethylene ether, and petroleum ether in a mass ratio of 1:1:(40-50).

Citation Information

Patent Citations

  • Inhibitor-supported carrier and preparation method and application thereof

    CN101914771A

  • Slow release scale inhibition agent for circulation cooling water

    CN108862641A

  • Use of water-soluble natural graft polymers as water-treatment agents

    WO1992010433A1