A method for polymerizing vinyl fluoride

By using a combination of a ternary pentablock copolymer of ethylene oxide-propylene oxide-tetrahydrofuran, an organic solvent, and a halide salt, the problems of high reaction pressure and low conversion rate in vinyl fluoride emulsion polymerization are solved, achieving a more efficient By polymerizing vinyl fluoride, regular particle morphology and good molecular weight distribution were obtained.

CN118562034BActive Publication Date: 2024-10-18HUANGSHAN YINENG TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411062777.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-18
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

During the emulsion polymerization of vinyl fluoride, the reaction pressure is high, the monomer conversion rate is low, and the molecular weight and distribution are difficult to control.

Method used

A ternary five-block copolymer of ethylene oxide-propylene oxide-tetrahydrofuran is used as the surfactant, combined with an organic solvent and a halide salt, emulsified by stirring and heated, and then vinyl fluoride is introduced to control the polymerization pressure and initiator concentration. Adjust the micelle particle size and dispersion to increase the concentration and conversion rate of vinyl fluoride.

Benefits of technology

The polymerization reaction pressure is reduced, the conversion rate and molecular weight distribution of vinyl fluoride are improved, and a more regular particle morphology and better polymerization effect are obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118562034B_ABST
    Figure CN118562034B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of polymer preparation, and specifically discloses a vinyl fluoride polymerization method. In the process of vinyl fluoride emulsion polymerization, a multi-block copolymer is used as a surfactant, tetrahydrofuran is used as an intermediate segment, and segments of propylene oxide polymerization are linked at both ends. The triblock has moderate hydrophobic properties, and ethylene oxide segments are further connected at both ends. The ethylene oxide segments have good hydrophilic properties. Under the action of the surfactant, halogen salts and mixed solvents are added at the same time, which can not only control the size and stability of micelles in the emulsion, but also regulate the diffusion and dissolution of vinyl fluoride from the gas phase to the water phase and micelles. The present invention adopts the above-mentioned vinyl fluoride polymerization method to reduce the polymerization pressure of vinyl fluoride, regulate the molecular weight and distribution of the polymer, and obtain high-performance polyvinyl fluoride while greatly reducing the polymerization pressure, which is suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer preparation, in particular to a vinyl fluoride polymerization method. Background Art

[0002] Polyvinyl fluoride (PVF) is a thermoplastic fluororesin with the lowest fluorine content. It has outstanding weather resistance, wear resistance, barrier properties, dimensional stability, chemical stability, dielectric properties, and resistance to moisture and heat, salt spray, and mildew. With the high-quality development of a low-carbon, green, and intelligent society, PVF resin has extremely wide applications in artificial intelligence, 5G communications, battery capacitors, photovoltaic power generation, power storage, aerospace, life medicine, chemistry and chemical engineering, and other fields. PVF can be obtained from vinyl fluoride monomers by solution polymerization, suspension polymerization, or emulsion polymerization. Since the monomer vinyl fluoride (VF) is in a gaseous state and has low solubility in solvents, in order to obtain a suitable molecular weight and its distribution, it is usually preferred to use emulsion polymerization to synthesize PVF. Despite this, there are still problems in VF emulsion polymerization, such as high polymerization pressure, low VF conversion rate, and difficult control of molecular weight and its distribution, which results in extremely high pressure requirements for industrial polymerization reactors and great difficulty in implementation.

[0003] Most of the patents for the preparation of polyvinyl fluoride use initiators to initiate the polymerization of vinyl fluoride monomers, and the polymerization rate, molecular weight and its distribution are controlled by controlling the reaction temperature and pressure, thereby regulating the performance of polyvinyl fluoride. U.S. Patent US2419010A discloses a method for preparing polyvinyl fluoride, using organic peroxide as an initiator, and emulsion polymerization is carried out in medium water. The film made of the resin has advantages in flexibility, but the polymerization conditions are harsh, the polymerization temperature is 50℃~200℃, and the polymerization pressure is 15MPa~200MPa. The high pressure makes industrial implementation very difficult and also brings great disadvantages to operational safety. Patent CN1834124A discloses a method for preparing polyvinyl fluoride in the presence of a water-soluble free radical initiator and an auxiliary agent. The auxiliary agent can be a neutral inorganic salt compound, a base or alkaline compound, an acid or an acidic compound, the reaction temperature is 50℃~150℃, the pressure is 5MPa~50MPa, and the time is 1h~10h. Adding a small amount of auxiliary agent without changing the reaction temperature and pressure can achieve the purpose of controlling the reaction rate and viscosity of the polymer. Patent CN112979847A discloses a method for preparing polyvinyl fluoride resin. In a reaction medium containing fluorine and chlorine saturated alkanes, under the action of azo compounds or perfluoroperoxide compounds as free radical initiators, vinyl fluoride undergoes polymerization reaction at -20°C to 100°C and 1MPa to 20MPa to obtain polyvinyl fluoride resin with a crystallinity of 13% to 24% and a haze of 1.3% to 2.0%, which is suitable for photovoltaic, decoration and other fields.

[0004] The prior art has not reported on how to reduce the reaction pressure, increase the monomer conversion rate, and regulate the polymer molecular weight and its distribution. In view of the shortcomings of the prior art, the present invention proposes a new process for vinyl fluoride polymerization, aiming to solve the problems of high reaction pressure, low monomer conversion rate, and difficult control of molecular weight and its distribution in the vinyl fluoride emulsion polymerization process. Summary of the invention

[0005] The purpose of the present invention is to provide a vinyl fluoride polymerization method, which solves the problems of high reaction pressure, low monomer conversion rate and difficult control of molecular weight and its distribution in the vinyl fluoride emulsion polymerization process.

[0006] To achieve the above object, the present invention provides a method for polymerizing vinyl fluoride, comprising the following steps:

[0007] S1 adds a surfactant and a mixed organic solvent to a reactor filled with pure water, starts stirring, emulsifies, obtains an emulsion, adds a halide salt under stirring, dissolves, and simultaneously introduces N2 to remove the air in the reactor to obtain a uniform and stable emulsion;

[0008] S2: heating the emulsion obtained in step S1, raising the temperature, introducing vinyl fluoride into the reactor, pumping in part of the initiator solution through a high-pressure pump, stirring and dissolving while initiating polymerization of vinyl fluoride, with the progress of polymerization, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride, after the reaction, pumping in the remaining initiator, adding vinyl fluoride, continuing polymerization, controlling the polymerization conversion rate of vinyl fluoride, and terminating the reaction to obtain a polyvinyl fluoride emulsion;

[0009] S3 cools the reactor to room temperature through jacket cooling water, slowly releases the reactor pressure to normal pressure, introduces N2, stirs, and removes residual vinyl fluoride monomer;

[0010] S4: filtering, washing and drying the solid-liquid mixture obtained in step S3 to obtain a polyvinyl fluoride powdered resin product;

[0011] In step S1, the surfactant is a ternary pentablock copolymer of ethylene oxide-propylene oxide-tetrahydrofuran, and the structure is (ethylene oxide) nE -(Propylene oxide) nP -(Tetrahydrofuran) nT -(Propylene oxide) nP -(ethylene oxide) nE , nE=25~100, nP=15~45, nT=8~15;

[0012] In step S1, the halide salt is one of ammonium fluoride, sodium fluoride, potassium fluoride, ammonium chloride, sodium chloride, and potassium chloride, and the concentration of the halide salt aqueous solution is 0.5wt%~10wt%.

[0013] Preferably, in step S1, the middle segment of the surfactant is a tetrahydrofuran polymer segment, which is connected to propylene oxide polymer segments at both ends, the tetrahydrofuran and propylene oxide polymer segments constitute a triblock polymer, which is further connected to ethylene oxide polymer segments at both ends, and the surfactant concentration is 0.1wt%~5.0wt%.

[0014] Preferably, in step S1, the organic solvent is a mixture of one of N,N-dimethylformamide and N,N-dimethylacetamide and one of acetone and diethyl ether, the volume ratio of the two is 0.5-2, the concentration is 0.25wt%-7.5wt%; the stirring speed is 300rpm-1000rpm.

[0015] Preferably, in step S1, the space velocity of introducing N2 is 5h -1 ~500h -1 The introduction time is 15min~60min, eliminating oxygen in the system and controlling the oxygen content below 8ppm.

[0016] Preferably, in step S2, the temperature of the emulsion is 60° C. to 90° C., and the pressure of the fluoroethylene introduced is 4.0 MPa to 15.0 MPa.

[0017] Preferably, in step S2, the initiator is an ammonium persulfate solution or a potassium persulfate solution, the amount of the initiator pumped in for the first time accounts for 30% to 60% of the total amount, the concentration of the initiator aqueous solution is 10.0wt%, and it is pumped into the reactor emulsion to make the initiator concentration in the emulsion 0.25wt% to 1.5wt%.

[0018] Preferably, in step S2, the polymerization time after the first addition of the initiator is 1 h to 4 h, and the polymerization time after the remaining initiator is added is 2 h to 5 h.

[0019] Preferably, in step S3, the space velocity of introducing N2 is 5h -1 ~500h -1 The introduction time is 15min~30min, and the content of vinyl fluoride in the control system is controlled to be lower than 15ppm.

[0020] The advantages and beneficial effects of the present invention using the above-mentioned vinyl fluoride polymerization method are:

[0021] (1) In the polyvinyl fluoride emulsion polymerization process provided by the present invention, tetrahydrofuran is used as the intermediate chain segment, which has strong lipophilicity and extends into the micelle, which is beneficial for the diffusion and dissolution of polyvinyl fluoride dissolved in water into the micelle, thereby increasing the concentration of polyvinyl fluoride in the micelle, reducing the polymerization pressure, increasing the polymerization reaction rate, and regulating the molecular weight and distribution of polyvinyl fluoride.

[0022] (2) The two ends of the tetrahydrofuran polymer chain segment are connected to the propylene oxide polymer chain segment, which has a weak lipophilicity and is beneficial to adjusting the lipophilic-hydrophilic balance value of the surfactant. The three blocks synergistically adjust the surfactant to have moderate lipophilicity, so as to stabilize the micelles and adjust the particle size and distribution of the micelles.

[0023] (3) Further connecting ethylene oxide polymer segments to both ends of the triblock polymer of (2); the ethylene oxide polymer segments have good hydrophilicity and extend into the water, thereby further adjusting the dispersion stability of the micelles and adjusting the particle size and distribution of the micelles.

[0024] (4) Under the action of the ternary pentablock surfactant, a mixed solvent and a halide salt are added. The halide salt is conducive to promoting the rapid diffusion of vinyl fluoride dissolved in water into the micelles, and at the same time, the solubility of the mixed solvent in water is adjusted so that the solvent mainly exists in the micelles. The solvent in the micelles dissolves the vinyl fluoride entering the micelles, increases the concentration of vinyl fluoride in the micelles, and then reduces the polymerization reaction pressure, increases the polymerization reaction speed, and increases the conversion rate of vinyl fluoride. At the same time, the mixed solvent in the micelles can also dissolve the generated polyvinyl fluoride, avoid the precipitation of polyvinyl fluoride in the micelles, increase the kinetic chain length of polyvinyl fluoride, and effectively regulate the molecular weight and distribution of polyvinyl fluoride.

[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a particle morphology diagram of polyvinyl fluoride synthesized in Example 1 of a vinyl fluoride polymerization method of the present invention;

[0027] Figure 2 is a particle size distribution diagram of Example 7 in a method for polymerizing vinyl fluoride of the present invention;

[0028] Figure 3 It is a particle size distribution diagram of comparative example 1 in a fluoroethylene polymerization method of the present invention. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0030] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0031] A method for polymerizing vinyl fluoride comprises the following steps:

[0032] S1 adds a surfactant and a mixed organic solvent to a reactor filled with pure water, starts stirring, emulsifies, obtains an emulsion, adds a halide salt under stirring, dissolves, and simultaneously introduces N2 to remove the air in the reactor to obtain a uniform and stable emulsion;

[0033] S2 heats the emulsion obtained in step S1 to a certain temperature, introduces vinyl fluoride into the reactor to a certain pressure, the temperature of the emulsion is 60°C~90°C, the pressure of the vinyl fluoride introduced is 4.0MPa~15.0MPa, pumps in part of the initiator solution through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After a certain reaction time, pump in the remaining initiator, and add Fill with fluoroethylene, continue polymerization for a certain period of time, control the polymerization conversion rate of fluoroethylene, terminate the reaction, and obtain polyfluoroethylene emulsion; the initiator is an aqueous solution of ammonium persulfate and potassium persulfate, the amount of initiator pumped in for the first time accounts for 30% to 60% of the total amount, the concentration of the initiator aqueous solution is 10.0wt%, and it is pumped into the reactor emulsion to make the initiator concentration in the emulsion 0.25wt% to 1.5wt%; the polymerization time after the first addition of the initiator is 1h to 4h, and the polymerization time after the addition of the remaining initiator is 2h to 5h;

[0034] S3 is cooled to room temperature through the jacket cooling water, the reactor pressure is slowly released to normal pressure, N2 is introduced, stirred, and residual vinyl fluoride monomer is removed. The space velocity of N2 introduction is 5h -1 ~500h -1 , the introduction time is 15min~30min, and the content of vinyl fluoride in the control system is controlled to be less than 15ppm;

[0035] S4: filtering, washing and drying the solid-liquid mixture obtained in step S3 to obtain a polyvinyl fluoride powdered resin product;

[0036] In step S1, the surfactant is a ternary five-block copolymer of ethylene oxide-propylene oxide-tetrahydrofuran, the middle segment is a tetrahydrofuran polymer segment, which has strong lipophilicity, and the two ends are connected with propylene oxide polymer segments, which have weak lipophilicity. The tetrahydrofuran and propylene oxide polymer segments constitute a triblock polymer, which has moderate lipophilicity, and the two ends are connected with ethylene oxide polymer segments, which have strong hydrophilicity. The ternary five-block copolymer composed of tetrahydrofuran, propylene oxide and ethylene oxide has lipophilicity in the middle three blocks and hydrophilicity in the ethylene oxide segments at both ends, and the concentration is 0.1wt%~5.0wt%; the typical structure is (EO) nE -(PO) nP -(THF) nT -(PO) nP -(EO) nE, nE=25~100, nP=15~45, nT=8~15. After the micelles are formed, the tetrahydrofuran polymer chain segments extend into the micelles, the ethylene oxide polymer chain segments extend into the water, and the propylene oxide serves as the lipophilic-hydrophilic intermediate transition layer on the micelle surface, synergistically stabilizing the micelles with the tetrahydrofuran lipophilic segment and the ethylene oxide hydrophilic segment, adjusting the micelle particle size and distribution, and adjusting the diffusion rate of fluoroethylene into the micelles.

[0037] In step S1, the organic solvent is a mixture of one of N,N-dimethylformamide and N,N-dimethylacetamide and one of acetone and diethyl ether, the volume ratio of the two is 0.5-2, and the concentration is 0.25wt%-7.5wt%; the stirring speed is 300rpm-1000rpm.

[0038] After the emulsion is formed, the halide salt dissolves in the water phase and pushes the solvent into the micelles. When vinyl fluoride enters the micelles, it quickly dissolves in the solvent, increasing the concentration of vinyl fluoride in the micelles and reducing the polymerization pressure. As the concentration of vinyl fluoride increases, the reaction rate increases, and the molecular weight of the polymer also increases. The solvent also dissolves polyvinyl fluoride, maintaining the activity of the growing chain without termination, thereby increasing the molecular weight of polyvinyl fluoride.

[0039] In step S1, the halide salt is one of ammonium fluoride, sodium fluoride, potassium fluoride, ammonium chloride, sodium chloride and potassium chloride, the concentration of the halide salt aqueous solution is 0.5wt%~10wt%, and the space velocity of introducing N2 is 5h -1 ~500h -1 The introduction time is 15min~60min, eliminating oxygen in the system and controlling the oxygen content below 8ppm.

[0040] After the halide salt is dissolved in water, the solubility of vinyl fluoride in water is moderately reduced. When vinyl fluoride diffuses from the gas phase into the water phase, it is pushed into the micelle due to the presence of the halide salt.

[0041] Example 1

[0042] A method for polymerizing vinyl fluoride comprises the following steps:

[0043] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 90 -(PO) 15 -(THF) 10 -(PO) 15 -(EO) 90, concentration is 0.5wt%, add a mixed solvent of N,N-dimethylformamide and acetone (DMF-Ace solvent), the volume ratio of the two is 0.5, the concentration is 0.6wt%, start stirring to emulsify it, set the stirring speed to 400rpm, and then add ammonium fluoride to it and dissolve it to obtain an emulsion containing an aqueous solution of ammonium fluoride with a concentration of 4.0wt%. At the same time, introduce N2 at a space velocity of 100h -1 The introduction time was 20 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 6.0 ppm, and a uniform emulsion was obtained.

[0044] S2 starts heating, raises the temperature of the emulsion to 60°C, introduces vinyl fluoride into the reactor to 5.0MPa, pumps in an initiator accounting for 50% of the total amount of initiator, i.e., a 10.0wt% ammonium persulfate solution, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 2h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.5wt%, add vinyl fluoride, continue polymerization for 3h, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0045] S3 is cooled to room temperature through jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 500h -1 The introduction time is 19 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 3.5ppm.

[0046] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0047] Example 2

[0048] A method for polymerizing vinyl fluoride comprises the following steps:

[0049] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 25 -(PO) 20 -(THF)8-(PO) 20 -(EO) 25 , concentration is 1.0wt%, add a mixed solvent of N,N-dimethylacetamide and acetone (DMAC-Ace solvent), the volume ratio of the two is 0.8, the concentration is 1.5wt%, start stirring to emulsify it, set the stirring speed to 700rpm, and then add potassium fluoride to it and dissolve it to obtain an emulsion containing potassium fluoride aqueous solution with a concentration of 10.0wt%, and at the same time, introduce N2 at a space velocity of 200h-1 The introduction time was 25 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 5.5 ppm, and a uniform emulsion was obtained.

[0050] S2 starts heating, raises the temperature of the emulsion to 85°C, introduces vinyl fluoride into the reactor to 8.0MPa, pumps in an initiator accounting for 30% of the total amount of initiator, i.e., a potassium persulfate solution with a concentration of 10.0wt%, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 1h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.8wt%, add vinyl fluoride, continue polymerization for 2.5h, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0051] S3 is cooled to room temperature through jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 450 h -1 The introduction time is 25 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 11.5ppm.

[0052] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0053] Example 3

[0054] A method for polymerizing vinyl fluoride comprises the following steps:

[0055] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 30 -(PO) 40 -(THF) 12 -(PO) 40 -(EO) 30 , concentration is 4.0wt%, add a mixed solvent of N,N-dimethylacetamide and diethyl ether (DMAC-EtO solvent), the volume ratio of the two is 1.8, the concentration is 6.2wt%, start stirring to emulsify it, set the stirring speed to 300rpm, then add sodium fluoride to it and dissolve it to obtain an emulsion containing sodium fluoride aqueous solution, the concentration is 5.5wt%, and at the same time, introduce N2, the air velocity is 5h -1 The introduction time was 55 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 7.5 ppm, and a uniform emulsion was obtained.

[0056] S2 starts heating, raises the temperature of the emulsion to 75°C, introduces vinyl fluoride into the reactor to 12.0MPa, pumps in 40% of the total initiator, i.e., a 10.0wt% potassium persulfate solution, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 3.5 hours, pump in the remaining initiator to make the initiator concentration in the emulsion 1.0wt%, add vinyl fluoride, continue polymerization for 5 hours, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0057] S3 is cooled to room temperature through jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 250h -1 The introduction time is 30 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 4.0ppm.

[0058] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0059] Example 4

[0060] A method for polymerizing vinyl fluoride comprises the following steps:

[0061] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 65 -(PO) 45 -(THF) 13 -(PO) 45 -(EO) 65 , concentration is 2.5wt%, add a mixed solvent of N,N-dimethylformamide and acetone (DMF-Ace solvent), the volume ratio of the two is 1.5, the concentration is 0.25wt%, start stirring to emulsify it, set the stirring speed to 600rpm, and then add ammonium chloride to it and dissolve it to obtain an emulsion containing an aqueous solution of ammonium chloride with a concentration of 2.0wt%. At the same time, introduce N2 at a space velocity of 50h -1 The introduction time was 15 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 7.0 ppm, and a uniform emulsion was obtained.

[0062] S2 starts heating, raises the temperature of the emulsion to 60°C, introduces vinyl fluoride into the reactor to 6.0MPa, pumps in an initiator accounting for 35% of the total amount of initiator, i.e., a 10.0wt% ammonium persulfate solution, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 3 hours, pump in the remaining initiator to make the initiator concentration in the emulsion 0.4wt%, add vinyl fluoride, continue polymerization for 3 hours, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0063] S3 is cooled to room temperature through jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 200h -1 The introduction time is 21 minutes, stirring is continued to remove the residual vinyl fluoride monomer, and the vinyl fluoride content of the system is controlled to be 8.8ppm.

[0064] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0065] Example 5

[0066] A method for polymerizing vinyl fluoride comprises the following steps:

[0067] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 80 -(PO) 30 -(THF)8-(PO) 30 -(EO) 80 , concentration is 4.5wt%, add a mixed solvent of N,N-dimethylformamide and ether (DMF-EtO solvent), the volume ratio of the two is 2.0, the concentration is 3.4wt%, start stirring to emulsify it, set the stirring speed to 800rpm, and then add potassium fluoride to it and dissolve it to obtain an emulsion containing potassium fluoride aqueous solution with a concentration of 7.0wt%, and at the same time, introduce N2 with a space velocity of 350h -1 The introduction time was 30 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 4.2 ppm, and a uniform emulsion was obtained.

[0068] S2 starts heating, raises the temperature of the emulsion to 70°C, introduces vinyl fluoride into the reactor to 4.0MPa, pumps in an initiator accounting for 60% of the total amount of initiator, i.e., a 10.0wt% ammonium persulfate solution, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 4 hours, pump in the remaining initiator to make the initiator concentration in the emulsion 0.25wt%, add vinyl fluoride, continue polymerization for 4 hours, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0069] S3 is cooled to room temperature through the jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 50h -1 The introduction time is 27 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 11.9ppm.

[0070] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0071] Example 6

[0072] A method for polymerizing vinyl fluoride comprises the following steps:

[0073] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 50 -(PO) 20 -(THF) 14 -(PO) 20 -(EO) 50 , concentration is 2.0wt%, add a mixed solvent of N,N-dimethylacetamide and diethyl ether (DMAC-EtO solvent), the volume ratio of the two is 0.6, the concentration is 7.5wt%, start stirring to emulsify it, set the stirring speed to 500rpm, and then add potassium fluoride to it and dissolve it to obtain an emulsion containing potassium fluoride aqueous solution with a concentration of 1.5wt%, and at the same time, introduce N2 at a space velocity of 500h -1 The introduction time was 45 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 2.5 ppm, and a uniform emulsion was obtained.

[0074] S2 starts heating, raises the temperature of the emulsion to 85°C, introduces vinyl fluoride into the reactor to 14.0MPa, pumps in an initiator accounting for 55% of the total amount of initiator, i.e., a potassium persulfate solution with a concentration of 10.0wt%, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 1h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.7wt%, add vinyl fluoride, continue polymerization for 3.5h, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0075] S3 is cooled to room temperature through jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 320h -1 The introduction time is 17 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 8.0ppm.

[0076] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0077] Example 7

[0078] A method for polymerizing vinyl fluoride comprises the following steps:

[0079] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 100 -(PO) 25 -(THF) 11 -(PO) 25 -(EO) 100 , concentration is 0.1wt%, add a mixed solvent of N,N-dimethylformamide and ether (DMF-EtO solvent), the volume ratio of the two is 1.3, the concentration is 1.9wt%, start stirring to emulsify it, set the stirring speed to 350rpm, and then add ammonium fluoride to it and dissolve it to obtain an emulsion containing an aqueous solution of ammonium fluoride with a concentration of 6.0wt%. At the same time, N2 is introduced with a space velocity of 80h -1 The introduction time was 15 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 6.8 ppm, and a uniform emulsion was obtained.

[0080] S2 starts heating, raises the temperature of the emulsion to 80°C, introduces vinyl fluoride into the reactor to 9.0MPa, pumps in an initiator accounting for 38% of the total amount of initiator, i.e., a 10.0wt% ammonium persulfate solution, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 3 hours, pump in the remaining initiator to make the initiator concentration in the emulsion 1.2wt%, add vinyl fluoride, continue polymerization for 2 hours, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0081] S3 is cooled to room temperature through jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 300h -1 The introduction time is 16 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 8.0 ppm.

[0082] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0083] Example 8

[0084] A method for polymerizing vinyl fluoride comprises the following steps:

[0085] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 55 -(PO) 45 -(THF) 15 -(PO) 45 -(EO) 55 , concentration is 3.5wt%, add a mixed solvent of N,N-dimethylformamide and acetone (DMF-Ace solvent), the volume ratio of the two is 1.1, the concentration is 2.6wt%, start stirring to emulsify it, set the stirring speed to 900rpm, and then add potassium chloride to it and dissolve it to obtain an emulsion containing potassium chloride aqueous solution with a concentration of 8.5wt%. At the same time, introduce N2 at a space velocity of 250h -1 The introduction time was 40 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 4.5 ppm, and a uniform emulsion was obtained.

[0086] S2 starts heating, raises the temperature of the emulsion to 72°C, introduces vinyl fluoride into the reactor to 15.0MPa, pumps in an initiator accounting for 60% of the total amount of initiator, i.e., a potassium persulfate solution with a concentration of 10.0wt%, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 2.5h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.6wt%, add vinyl fluoride, continue polymerization for 5h, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0087] S3 is cooled to room temperature through the jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 5h -1 The introduction time is 23 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 14.0ppm.

[0088] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0089] Example 9

[0090] A method for polymerizing vinyl fluoride comprises the following steps:

[0091] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 75 -(PO) 15 -(THF) 10 -(PO) 15 -(EO) 75 , concentration is 5.0wt%, add a mixed solvent of N,N-dimethylacetamide and diethyl ether (DMAC-EtO solvent), the volume ratio of the two is 0.7, the concentration is 5.0wt%, start stirring to emulsify it, set the stirring speed to 650rpm, and then add ammonium fluoride to it and dissolve it to obtain an emulsion containing an ammonium fluoride aqueous solution with a concentration of 0.5wt%, and at the same time, introduce N2 at a space velocity of 300h −1 The introduction time was 50 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 3.2 ppm, and a uniform emulsion was obtained.

[0092] S2 starts heating, raises the temperature of the emulsion to 90°C, introduces vinyl fluoride into the reactor to 10.0MPa, pumps in an initiator accounting for 30% of the total amount of initiator, i.e., a potassium persulfate solution with a concentration of 10.0wt%, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 4 hours, pump in the remaining initiator to make the initiator concentration in the emulsion 1.4wt%, add vinyl fluoride, continue polymerization for 4.5 hours, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0093] S3 is cooled to room temperature by cooling water through the jacket, and the reactor pressure is slowly released to normal pressure. N2 is introduced at a space velocity of 400 h -1 The introduction time is 15 minutes, stirring is continued to remove the residual vinyl fluoride monomer, and the vinyl fluoride content of the system is controlled to be 6.2ppm.

[0094] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0095] Example 10

[0096] A method for polymerizing vinyl fluoride comprises the following steps:

[0097] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 40 -(PO) 35 -(THF)9-(PO) 35 -(EO) 40 , concentration is 3.0wt%, a mixed solvent of N,N-dimethylacetamide and acetone (DMAC-Ace solvent) is added, the volume ratio of the two is 1.6, the concentration is 4.7wt%, stirring is turned on to emulsify it, the stirring speed is set to 1000rpm, and then sodium chloride is added thereto to dissolve, and an emulsion containing sodium chloride aqueous solution is obtained, the concentration is 3.0wt%, and N2 is introduced at a space velocity of 400h -1 The introduction time was 60 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 2.0 ppm, and a uniform emulsion was obtained.

[0098] S2 starts heating and heats the emulsion to 65°C. Vinyl fluoride is introduced into the reactor to 7.0MPa, and an initiator accounting for 40% of the total amount of initiator, i.e., a 10wt% ammonium persulfate solution, is pumped in through a high-pressure pump. While stirring and dissolving, vinyl fluoride polymerization is initiated. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 1.5h, the remaining initiator is pumped in to make the initiator concentration in the emulsion 1.5wt%, and vinyl fluoride is added. The polymerization continues for 2h, and the polymerization conversion rate of vinyl fluoride is controlled. The reaction is terminated to obtain a polyvinyl fluoride emulsion.

[0099] S3 is cooled to room temperature through the jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 100h -1 The introduction time is 29 minutes, stirring is continued to remove the residual vinyl fluoride monomer, and the vinyl fluoride content of the system is controlled to be 10.0ppm.

[0100] S4: filtering, washing and drying the obtained solid-liquid mixture to obtain a polyvinyl fluoride powdered resin product.

[0101] The average particle size of the polyvinyl fluoride prepared in Examples 1-10 ranges from tens of nanometers to hundreds of nanometers, and the particle size of most particles is concentrated between 50nm and 450nm. Figure 1 As shown, the polyvinyl fluoride particles prepared by the polymerization method of Example 1 of the present invention have a relatively regular morphology and are spherical with a rough surface. Clusters of various shapes are formed between the particles, and there are large differences in the number of particles in the clusters.

[0102] Comparative Example 1

[0103] A method for polymerizing vinyl fluoride comprises the following steps:

[0104] S1 Add the surfactant sodium dodecyl sulfate to the reactor filled with pure water at a concentration of 4.0wt%, add a mixed solvent of N,N-dimethylacetamide and diethyl ether (DMAC-EtO solvent) at a volume ratio of 1.8 and a concentration of 6.2wt%, start stirring to emulsify it, set the stirring speed to 300rpm, then add sodium fluoride to dissolve it to obtain an emulsion containing sodium fluoride aqueous solution at a concentration of 5.5wt%, and introduce N2 at a space velocity of 5h -1 The introduction time was 55 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 7.5 ppm, and a uniform emulsion was obtained.

[0105] S2 starts heating, raises the temperature of the emulsion to 75°C, introduces vinyl fluoride into the reactor to 12.0MPa, pumps in 40% of the total initiator, i.e., a 10.0wt% potassium persulfate solution, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 3.5 hours, pump in the remaining initiator to make the initiator concentration in the emulsion 1.0wt%, add vinyl fluoride, continue polymerization for 5 hours, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride 2 emulsion.

[0106] S3 is cooled to room temperature through jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 250h -1 The introduction time is 30 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 4.0ppm.

[0107] S4 filters, washes and dries the obtained solid-liquid mixture to obtain a PVF powdered resin product. It has been determined that the average particle size of polyvinyl fluoride prepared by using a general surfactant sodium dodecyl sulfate and a ternary five-block copolymer without adding a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) is between 1000nm and 3000nm. The particle morphology is irregular, and the polymerization effect is not as good as that of the ternary five-block copolymer with the addition of a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF).

[0108] Comparative Example 2

[0109] A method for polymerizing vinyl fluoride comprises the following steps:

[0110] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) ternary five-block copolymer into a reactor filled with pure water, the structure of which is (EO) 25 -(PO) 20 -(THF)8-(PO) 20 -(EO) 25 The concentration was 1.0 wt %. Stirring was started to emulsify the mixture. The stirring speed was set to 700 rpm. Potassium fluoride was added thereto and dissolved to obtain an emulsion containing an aqueous solution of potassium fluoride with a concentration of 10.0 wt %. N2 was introduced at a space velocity of 200 h -1 The introduction time was 25 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 5.5 ppm, and a uniform emulsion was obtained.

[0111] S2 starts heating, raises the temperature of the emulsion to 85°C, introduces vinyl fluoride into the reactor to 8.0MPa, pumps in an initiator accounting for 30% of the total amount of initiator, i.e., a potassium persulfate solution with a concentration of 10.0wt%, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving. As the polymerization proceeds, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride. After reacting for 1h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.8wt%, add vinyl fluoride, continue polymerization for 2.5h, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0112] S3 is cooled to room temperature through jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 450 h -1 The introduction time is 25 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 11.5ppm.

[0113] S4 filters, washes and dries the obtained solid-liquid mixture to obtain a polyvinyl fluoride powder resin product. It has been determined that the average particle size of the polyvinyl fluoride prepared without adding a solvent ranges from 800 nm to 1500 nm. The particle morphology is irregular, and the polymerization effect is not as good as that of adding a mixed solvent.

[0114] Comparative Example 3

[0115] A method for polymerizing vinyl fluoride comprises the following steps:

[0116] S1 Add a surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) pentablock copolymer into a reactor filled with pure water, the structure of which is (EO) 90 -(PO) 15 -(THF) 10 -(PO) 15 -(EO) 90 , concentration is 0.5wt%, add a mixed solvent of N,N-dimethylformamide and acetone (DMF-Ace solvent), the volume ratio of the two is 0.5, the concentration is 0.6wt%, start stirring to emulsify it, set the stirring speed to 400rpm, and introduce N2 at the same time, the air velocity is 100h -1 The introduction time was 20 min, the air in the reactor was excluded, the oxygen content of the system was controlled to be 6.0 ppm, and a uniform emulsion was obtained.

[0117] S2 starts heating, raises the temperature of the emulsion to 60°C, introduces vinyl fluoride into the reactor to 5.0MPa, pumps in an initiator accounting for 50% of the total amount of the initiator, i.e., a 10.0wt% ammonium persulfate solution, through a high-pressure pump, and initiates the polymerization of vinyl fluoride while stirring and dissolving to obtain an emulsion containing polyvinyl fluoride. After reacting for 2h, pump in the remaining initiator to make the initiator concentration in the emulsion 0.5wt%, continue the polymerization for 3h, control the polymerization conversion rate of vinyl fluoride, terminate the reaction, and obtain a polyvinyl fluoride emulsion.

[0118] S3 is cooled to room temperature through jacket cooling water, the reactor pressure is slowly released to normal pressure, and N2 is introduced at a space velocity of 500h -1 The introduction time is 19 minutes, stirring is continued, residual vinyl fluoride monomer is removed, and the vinyl fluoride content of the system is controlled to be 3.5ppm.

[0119] S4 filters, washes and dries the obtained solid-liquid mixture to obtain a polyvinyl fluoride powder resin product. It has been determined that the average particle size of polyvinyl fluoride prepared without adding halogen salts ranges from 50nm to 1000nm, the particle morphology is relatively regular, and the polymerization effect is not as good as that of adding halogen salts.

[0120] The particle size distribution data of the polyvinyl fluoride prepared in Examples 1-10 and Comparative Examples 1-3 were measured, and the results are shown in Table 1. The particle size distributions of Example 7 and Comparative Example 1 are shown in Table 1. Figure 2 and Figure 3 shown.

[0121] Table 1 Reaction pressure, vinyl fluoride conversion rate and average particle size of polyvinyl fluoride in the examples and comparative examples

[0122] ;

[0123] As shown in Table 1, compared with Examples 1-10, Comparative Example 1 does not add the surfactant ternary five-block copolymer of ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF), but uses the general surfactant sodium dodecyl sulfate. The average particle size of the prepared polyvinyl fluoride is larger than that of Examples 1-10, the conversion rate is low, and the dispersion is large. Compared with Examples 1-10, Comparative Example 2 does not add an organic solvent. The average particle size of the prepared polyvinyl fluoride is larger than that of Examples 1-10, the conversion rate is low, and the dispersion is large. Compared with Examples 1-10, Comparative Example 3 does not add halogen. The average particle size of the prepared polyvinyl fluoride is larger than that of Examples 1-10, the conversion rate is low, and the dispersion is large. This shows that the simultaneous addition of the ternary five-block copolymer of ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF), the organic solvent, and the halogen in the present invention has the effect of reducing the average particle size of the polymer, improving the conversion rate, and improving the polymerization effect. Under the action of the ternary five-block surfactant, a mixed solvent and a halide salt are added. The halide salt is conducive to promoting the rapid diffusion of vinyl fluoride dissolved in water into the micelles, and at the same time, the solubility of the mixed solvent in water is adjusted so that the solvent mainly exists in the micelles. The solvent in the micelles plays a role in dissolving the vinyl fluoride entering the micelles, increasing the concentration of vinyl fluoride in the micelles, and then playing an effect of reducing the polymerization reaction pressure, increasing the polymerization reaction speed, and increasing the conversion rate of vinyl fluoride. At the same time, the mixed solvent in the micelles can dissolve the generated polyvinyl fluoride, avoid the precipitation of polyvinyl fluoride in the micelles, increase the kinetic chain length of polyvinyl fluoride, and effectively regulate the molecular weight and distribution of polyvinyl fluoride.

[0124] from Figure 1 It can be seen that the minimum particle size of the polyvinyl fluoride obtained in Example 1 is about 50 nm, the maximum particle size is about 500 nm, and the average particle size is about 275.1 nm.

[0125] from Figure 2 It can be seen that the average particle size of the polyvinyl fluoride prepared in Example 7 is 313.9 nm, particles in the particle size range of 0-100 nm account for 7.36% of the total number of particles, particles in the particle size range of 200-300 nm account for 26.38% of the total number of particles, and particles in the particle size range of 700-800 nm account for 2.45% of the total number of particles.

[0126] from Figure 3It can be seen that the average particle size of the polyvinyl fluoride prepared in Comparative Example 1 is 1836.9 nm, the particles in the particle size range of 900-1100 nm account for 5.36% of the total number of particles, the particles in the particle size range of 1500-1700 nm account for 17.86% of the total number of particles, and the particles in the particle size range of 2900-3100 nm account for 2.98% of the total number of particles. Comparative Example 1 does not add the surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) block copolymer, but uses a general surfactant to prepare sodium dodecyl sulfate. The average particle size of the polyvinyl fluoride prepared ranges from 1000 to 3000. The particle morphology is irregular, and the polymerization effect is not as good as the effect of adding the surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) block copolymer. It shows that adding surfactant ethylene oxide (EO)-propylene oxide (PO)-tetrahydrofuran (THF) block copolymer can reduce the particle size of polyvinyl fluoride, and the particle morphology is regular and the polymerization effect is good.

[0127] Therefore, the present invention adopts the above-mentioned vinyl fluoride polymerization method to solve the problems of high reaction pressure, low monomer conversion rate and difficult control of molecular weight and its distribution in the vinyl fluoride emulsion polymerization process.

[0128] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for polymerizing vinyl fluoride, characterized in that: The steps include: S1 adds a surfactant and a mixed organic solvent to a reactor filled with pure water, starts stirring, emulsifies, obtains an emulsion, adds a halide salt under stirring, dissolves, and simultaneously introduces N2 to remove the air in the reactor to obtain a uniform and stable emulsion; S2: heating the emulsion obtained in step S1, raising the temperature, introducing vinyl fluoride into the reactor, pumping in part of the initiator solution through a high-pressure pump, stirring and dissolving while initiating polymerization of vinyl fluoride, with the progress of polymerization, the pressure decreases, and vinyl fluoride is added to the polymerization kettle through a booster pump to maintain the pressure in the polymerization kettle to obtain an emulsion containing polyvinyl fluoride, after the reaction, pumping in the remaining initiator, adding vinyl fluoride, continuing polymerization, controlling the polymerization conversion rate of vinyl fluoride, and terminating the reaction to obtain a polyvinyl fluoride emulsion; S3 cools the reactor to room temperature through jacket cooling water, slowly releases the reactor pressure to normal pressure, introduces N2, stirs, and removes residual vinyl fluoride monomer; S4: filtering, washing and drying the solid-liquid mixture obtained in step S3 to obtain a polyvinyl fluoride powdered resin product; In step S1, the surfactant is a ternary pentablock copolymer of ethylene oxide-propylene oxide-tetrahydrofuran, and the structure is (ethylene oxide) nE -(Propylene oxide) nP -(Tetrahydrofuran) nT -(Propylene oxide) nP -(ethylene oxide) nE , nE=25~100, nP=15~45, nT=8~15; In step S1, the halide salt is one of ammonium fluoride, sodium fluoride, potassium fluoride, ammonium chloride, sodium chloride, and potassium chloride, and the concentration of the halide salt aqueous solution is 0.5wt%~10wt%; the organic solvent is a mixture of one of N,N-dimethylformamide and N,N-dimethylacetamide and one of acetone and ether, the volume ratio of the two is 0.5~2, the concentration is 0.25wt%~7.5wt%, and the stirring speed is 300rpm~1000rpm.

2. A method for polymerizing vinyl fluoride according to claim 1, characterized in that: In step S1, the middle segment of the surfactant is a tetrahydrofuran polymer segment, which is connected to propylene oxide polymer segments at both ends. The tetrahydrofuran and propylene oxide polymer segments constitute a triblock polymer, which is further connected to ethylene oxide polymer segments at both ends. The surfactant concentration is 0.1wt%~5.0wt%.

3. A method for polymerizing vinyl fluoride according to claim 1, characterized in that: In step S1, the space velocity of N2 is 5h -1 ~500h -1 The introduction time is 15min~60min, eliminating oxygen in the system and controlling the oxygen content below 8ppm.

4. A method for polymerizing vinyl fluoride according to claim 1, characterized in that: In step S2, the temperature of the emulsion is 60°C to 90°C, and the pressure of the introduced vinyl fluoride is 4.0 MPa to 15.0 MPa.

5. A method for polymerizing vinyl fluoride according to claim 1, characterized in that: In step S2, the initiator is an ammonium persulfate solution or a potassium persulfate solution. The amount of the initiator pumped in for the first time accounts for 30% to 60% of the total amount. The concentration of the initiator aqueous solution is 10.0 wt %, which is pumped into the reactor emulsion to make the initiator concentration in the emulsion 0.25 wt % to 1.5 wt %.

6. A method for polymerizing vinyl fluoride according to claim 1, characterized in that: In step S2, the polymerization time after the first addition of the initiator is 1 h to 4 h, and the polymerization time after the remaining initiator is added is 2 h to 5 h.

7. A method for polymerizing vinyl fluoride according to claim 1, characterized in that: In step S3, the space velocity of N2 is 5h -1 ~500h -1 The introduction time is 15min~30min, and the content of vinyl fluoride in the control system is controlled to be lower than 15ppm.

Citation Information

Patent Citations

  • Preparation method of polyvinyl fluoride resin

    CN112979847A

  • Prepn. of PVF

    CN1834124A

  • Polyvinyl fluoride

    US2419010A

  • Preparation method of polyether amine

    CN102604072A