A compatibilizer for low-smoke halogen-free cable material and its preparation process
The preparation of high-density polyethylene using titanium-based catalyst suspensions solves the problem of insufficient compatibilizer adhesion in high-density polyethylene, achieving efficient compatibilizer preparation and improving the physical and mechanical properties of cable materials.
Patent Information
- Application Number
- CN202410925536.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-11
AI Technical Summary
Existing high-density polyethylene compatibilizers have insufficient bonding ability in cable materials, resulting in poor compatibility and failing to effectively improve the physical and mechanical properties of the materials.
High-density polyethylene was prepared using a titanium-based catalyst suspension, and a compatibilizer for low-smoke halogen-free cable materials was prepared by melt extrusion using a twin-screw extruder. The high catalytic activity of the titanium-based catalyst and the suspension form improved the contact between the catalyst and the reactant gas, affecting the stereoregularity of the polymer chain and enhancing the stability and adhesive properties of the high-density polyethylene.
It improves the stability and physical strength of high-density polyethylene, enhances the adhesive properties of the compatibilizer, reduces stress concentration, and improves the physical and mechanical properties of the composite material.
Smart Images

Figure CN118562061B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a compatibilizer for low-smoke halogen-free cable materials and a preparation process thereof. Background Art
[0002] Compatibilizer, also known as a compatibilizer or synergist, is an additive added during the processing of multi-component materials. Its main function is to improve the compatibility between different polymer materials, so that materials that are originally difficult to mix or prone to phase separation can be better combined to form a uniform and stable blending system. Since cable materials need to have the ability of aging resistance and electrical resistance, it is necessary to add materials with different functions to the cable materials and use compatibilizers to mix different materials together.
[0003] Existing cable material compatibilizers are mostly composed of high-density polyethylene as the main body, grafted with different functional monomers. However, the viscosity of existing high-density polyethylene is average. In addition, solid catalysts are used in the preparation of high-density polyethylene, and the amount of catalyst added is relatively large, so some catalysts will remain. As a result, the adhesion ability of high-density polyethylene to functional monomers is average, and the adhesion ability to compatibilizers is not significantly improved.
[0004] Therefore, the present application provides a compatibilizer for low-smoke halogen-free cable materials and a preparation process thereof to meet the needs. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a compatibilizer for low-smoke halogen-free cable materials and a preparation process thereof to solve the existing problems.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A preparation process of a compatibilizer for low-smoke halogen-free cable materials comprises the following steps:
[0008] S1: Preparation of catalyst suspension
[0009] Dissolving tetrabutyl titanate and ethylene glycol in anhydrous ethanol, heating, condensing and refluxing to obtain a viscous liquid product, then dissolving the viscous liquid product and (2-carboxyethyl)phenylphosphonic acid in anhydrous ethanol to obtain a viscous solution and a (2-carboxyethyl)phenylphosphonic acid solution, respectively, slowly dropping the (2-carboxyethyl)phenylphosphonic acid solution into the viscous solution for reaction, then centrifuging using a high-speed refrigerated centrifuge, drying and grinding to obtain a titanium-based catalyst powder, then dissolving the titanium-based catalyst powder in deionized water to obtain a catalyst suspension;
[0010] S2: Preparation of high-density polyethylene
[0011] n-hexane is introduced into the reactor, and the reactor is degassed using a vacuum pump, the temperature of the reactor is increased, and hydrogen and ethylene are used to pressurize the reactor, and then triethylaluminum solution is injected into the reactor using an injection device, and then the catalyst suspension is injected into the reactor and polymerization is started, the ethylene absorption rate is monitored using a mass flow controller, and the consumed ethylene is recovered by injecting new ethylene gas into the reactor to keep the total pressure of the reactor unchanged, the gas is discharged and the reactor is cooled to 70-80° C., and then, a gas mixture of hydrogen and ethylene is injected into the reactor, and the second stage polymerization is started at this time, the gas is discharged to stabilize the reactor at 70-78° C., and ethylene gas and titanium catalyst powder are continuously added to fully react, and finally, the gas in the reactor is discharged, and the polymer powder in the reactor is collected and dried overnight to obtain high-density polyethylene;
[0012] S3: Preparation of compatibilizer using high-density polyethylene as the main component
[0013] First, MAH and BIBP are weighed and dissolved in acetone to prepare a mixed liquid, and the mixed liquid is added to a mixer, and then high-density polyethylene is added to the mixer as a grafting body to obtain a mixture, and the mixture is poured into a hopper of a twin-screw extruder, and melt-extruded using the twin-screw extruder to obtain a compatibilizer for low-smoke halogen-free cable materials.
[0014] Optionally, step S1 of preparing a catalyst suspension comprises the following steps:
[0015] S1.1: Dissolve 6-8 parts by mass of tetrabutyl titanate and 1-2 parts by mass of ethylene glycol in 50-60 parts by volume of anhydrous ethanol, heat and condense under reflux for 260-280 min, and rotary evaporate at 60-70° C. for 50-60 min to obtain a viscous liquid product;
[0016] S1.2: The viscous liquid product and 1-1.5 parts by mass of (2-carboxyethyl)phenylphosphonic acid are respectively dissolved in 25 parts by volume of anhydrous ethanol to obtain a viscous solution and a (2-carboxyethyl)phenylphosphonic acid solution, and the (2-carboxyethyl)phenylphosphonic acid solution is slowly added dropwise to the viscous solution, and the reaction is carried out at 80-85°C for 40-45 minutes;
[0017] S1.3: The mixture is then centrifuged twice using a high-speed refrigerated centrifuge, dried and ground to obtain a titanium-based catalyst powder. The titanium-based catalyst powder is then dissolved in deionized water at a solid-to-liquid ratio of 1:(15-30), and stirred at high speed to obtain a catalyst suspension.
[0018] Optionally, step S2 prepares high-density polyethylene, comprising the following steps:
[0019] S2.1: 600-700 parts by volume of n-hexane are introduced into the reactor, and the reactor is degassed using a vacuum pump;
[0020] S2.2: Raise the reactor temperature to 80-100°C and then pressurize it to 2-4 MPa with hydrogen and ethylene;
[0021] S2.3: Then, the triethylaluminum solution is injected into the reactor using an injection device, reacted for 5-10 minutes, and the catalyst suspension is injected into the reactor to start polymerization;
[0022] S2.4: monitor the ethylene absorption rate using a mass flow controller and recover the consumed ethylene by injecting new ethylene gas into the reactor to maintain the total pressure of the reactor constant;
[0023] S2.5: After 10-20 min, the gas is discharged and the reactor is cooled to 70-80°C, then a gas mixture of hydrogen and ethylene is injected into the reactor, and the second stage polymerization is started at this time;
[0024] S2.6: After another 8-15 minutes, exhaust the gas to stabilize the reactor at 70-78°C, continue to add ethylene gas and titanium catalyst powder, and wait for 10-20 minutes for the reaction to be fully completed;
[0025] S2.7: Finally, the gas in the reactor is discharged, and the polymer powder in the reactor is collected and dried in an oven at 80-100°C overnight to obtain high-density polyethylene.
[0026] Optionally, step S3 uses high-density polyethylene as a main component to prepare a compatibilizer, comprising the following steps:
[0027] S3.1: First, weigh MAH and BIBP, dissolve them in acetone, stir until completely dissolved, prepare a mixed liquid, and add the mixed liquid into a mixer;
[0028] S3.2: Then, 50-75% of the total mass of high-density polyethylene is added to the mixer as the grafting body, and the mixture is taken out after mixing for 5-8 minutes to obtain a mixture;
[0029] S3.3: Pour the mixed material into the hopper of a twin-screw extruder, and use the twin-screw extruder to melt and extrude the mixed material at a melting temperature of 140-180° C. to obtain a compatibilizer for low-smoke halogen-free cable materials.
[0030] Optionally, the volume ratio of hydrogen to ethylene in step S2.2 is (3.5-7):1.
[0031] Optionally, in step S2.3, the amount of triethylaluminum solution added is 10-50 mg / L, and the amount of catalyst suspension added is 5-8 mg / L.
[0032] Optionally, the volume ratio of hydrogen to ethylene in the gas mixture of hydrogen and ethylene in step S2.5 is 1.5:1.
[0033] Optionally, the amount of titanium-based catalyst powder added in step S2.6 is 0.5% of the total mass of the system.
[0034] Optionally, the volume ratio of MAH and BIBP in step S3.1 is 1:(0.5-2).
[0035] A compatibilizer for low-smoke halogen-free cable materials is prepared by the preparation process of the above-mentioned compatibilizer for low-smoke halogen-free cable materials.
[0036] Compared with the prior art, the present invention has at least the following beneficial effects:
[0037] In the above scheme, titanium-based catalyst powder is prepared and the powder is prepared into a catalyst suspension. The titanium-based catalyst has good catalytic activity and can achieve efficient polymerization reaction at the temperature and pressure required. The amount added during the process is less, which saves costs. Moreover, adding the catalyst to the reaction in the form of a suspension can make the catalyst fully contact with the reaction gas, further improving the catalytic efficiency of the catalyst.
[0038] By using titanium-based catalysts to prepare high-density polyethylene, titanium-based catalysts can affect the stereoregularity of polymer chains, causing the polymer to change from a random polymer to a highly oriented isotactic polymer, thereby making the resulting high-density polyethylene more stable and physically strong.
[0039] By using high-density polyethylene as the grafting body, the high-density polyethylene has a stable morphology, a high density, and a strong binding force to the functional monomer, so that the prepared compatibilizer has good adhesion properties, which can make the two-phase materials closely combined, reduce stress concentration, and thus improve the physical and mechanical properties of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, further serve to explain the principles of the invention and to enable those skilled in the relevant art to make and use the invention.
[0041] Figure 1 The present invention is a flow chart of the preparation process of a compatibilizer for low-smoke halogen-free cable materials used in an embodiment of the present invention. DETAILED DESCRIPTION
[0042] The following is a detailed description of the preparation process of a low-smoke halogen-free cable material compatibilizer provided by the present invention in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternative methods to implement some known technologies; and the accompanying drawings are only for a more specific description of the embodiments, and are not intended to specifically limit the present invention.
[0043] Embodiment 1:
[0044] A preparation process of a compatibilizer for low-smoke halogen-free cable materials, such as Figure 1 As shown, the following steps are included:
[0045] S1: Preparation of catalyst suspension
[0046] S1.1: Dissolve 6 parts by mass of tetrabutyl titanate and 1 part by mass of ethylene glycol in 60 parts by volume of anhydrous ethanol, heat and condense under reflux for 260 min, and rotary evaporate at 70°C for 60 min to obtain a viscous liquid product;
[0047] S1.2: The viscous liquid product and 1.5 parts by mass of (2-carboxyethyl)phenylphosphonic acid are dissolved in 25 parts by volume of anhydrous ethanol to obtain a viscous solution and a (2-carboxyethyl)phenylphosphonic acid solution, respectively. The (2-carboxyethyl)phenylphosphonic acid solution is slowly added dropwise to the viscous solution and reacted at 80°C for 40 minutes.
[0048] S1.3: The mixture was then centrifuged twice using a high-speed refrigerated centrifuge, dried and ground to obtain a titanium-based catalyst powder. The titanium-based catalyst powder was then dissolved in deionized water at a solid-liquid ratio of 1:15, and stirred at a high speed to obtain a catalyst suspension.
[0049] S2: Preparation of high-density polyethylene
[0050] S2.1: 600 parts by volume of n-hexane is introduced into the reactor, and the reactor is degassed using a vacuum pump;
[0051] S2.2: The reactor temperature was raised to 90°C, and then pressurized to 4 MPa with hydrogen and ethylene, with a volume ratio of hydrogen to ethylene of 3.5:1;
[0052] S2.3: Then, the triethylaluminum solution was injected into the reactor using an injection device, and the reaction was carried out for 10 minutes. The catalyst suspension was injected into the reactor and polymerization was started. The amount of the triethylaluminum solution added was 10 mg / L, and the amount of the catalyst suspension added was 5 mg / L.
[0053] S2.4: monitor the ethylene absorption rate using a mass flow controller and recover the consumed ethylene by injecting new ethylene gas into the reactor to maintain the total pressure of the reactor constant;
[0054] S2.5: After 20 minutes, the gas is discharged and the reactor is cooled to 80°C, then a gas mixture of hydrogen and ethylene is injected into the reactor, wherein the volume ratio of hydrogen to ethylene in the gas mixture of hydrogen and ethylene is 1.5:1, and the second stage polymerization is started at this time;
[0055] S2.6: After another 8 minutes, exhaust the remaining gas and stabilize the reactor at 78°C, continue to add ethylene gas and titanium catalyst powder, the amount of titanium catalyst powder added is 0.5% of the total mass of the system, and wait until the reaction is sufficient;
[0056] S2.7: Finally, the gas in the reactor is discharged, and the polymer powder in the reactor is collected and dried in an oven at 100°C overnight to obtain high-density polyethylene.
[0057] S3: Preparation of compatibilizer using high-density polyethylene as the main component
[0058] S3.1: First, weigh MAH and BIBP, dissolve them in acetone, and stir until completely dissolved to prepare a mixed liquid, wherein the volume ratio of MAH to BIBP is 1:0.5;
[0059] S3.2: Then, 75% of the total mass of high-density polyethylene is added to the mixer as the grafting body, and the mixture is taken out after mixing for 8 minutes to obtain a mixture;
[0060] S3.3: Pour the mixed material into the hopper of a twin-screw extruder, and use the twin-screw extruder to melt and extrude the mixed material at a melting temperature of 160° C. to obtain a compatibilizer for low-smoke halogen-free cable materials.
[0061] Embodiment 2:
[0062] A preparation process of a compatibilizer for low-smoke halogen-free cable materials, such as Figure 1 As shown, the following steps are included:
[0063] S1: Preparation of catalyst suspension
[0064] S1.1: 8 parts by mass of tetrabutyl titanate and 2 parts by mass of ethylene glycol were dissolved in 50 parts by volume of anhydrous ethanol, heated to condense and reflux for 260 min, and rotary evaporated at 70°C for 60 min to obtain a viscous liquid product;
[0065] S1.2: The viscous liquid product and 1 part by mass of (2-carboxyethyl)phenylphosphonic acid are dissolved in 25 parts by volume of anhydrous ethanol to obtain a viscous solution and a (2-carboxyethyl)phenylphosphonic acid solution, respectively. The (2-carboxyethyl)phenylphosphonic acid solution is slowly added dropwise to the viscous solution and reacted at 80°C for 40 minutes.
[0066] S1.3: The mixture is then centrifuged twice using a high-speed refrigerated centrifuge, dried and ground to obtain a titanium-based catalyst powder. The titanium-based catalyst powder is then dissolved in deionized water at a solid-liquid ratio of 1:30, and stirred at a high speed to obtain a catalyst suspension.
[0067] S2: Preparation of high-density polyethylene
[0068] S2.1: 700 parts by volume of n-hexane is introduced into the reactor, and the reactor is degassed using a vacuum pump;
[0069] S2.2: The reactor temperature was raised to 90°C, and then pressurized to 4 MPa with hydrogen and ethylene, with a volume ratio of hydrogen to ethylene of 7:1;
[0070] S2.3: Then, the triethylaluminum solution was injected into the reactor using an injection device, and the reaction was carried out for 10 minutes. The catalyst suspension was injected into the reactor and polymerization was started. The amount of the triethylaluminum solution added was 10 mg / L, and the amount of the catalyst suspension added was 8 mg / L.
[0071] S2.4: monitor the ethylene absorption rate using a mass flow controller and recover the consumed ethylene by injecting new ethylene gas into the reactor to maintain the total pressure of the reactor constant;
[0072] S2.5: After 20 minutes, the gas is discharged and the reactor is cooled to 80°C, then a gas mixture of hydrogen and ethylene is injected into the reactor, wherein the volume ratio of hydrogen to ethylene in the gas mixture of hydrogen and ethylene is 1.5:1, and the second stage polymerization is started at this time;
[0073] S2.6: After another 8 minutes, exhaust the remaining gas and stabilize the reactor at 78°C, continue to add ethylene gas and titanium catalyst powder, the amount of titanium catalyst powder added is 0.5% of the total mass of the system, and wait until the reaction is sufficient;
[0074] S2.7: Finally, the gas in the reactor is discharged, the polymer powder in the reactor is collected and dried in an oven at 100°C overnight to obtain high-density polyethylene.
[0075] S3: Preparation of compatibilizer using high-density polyethylene as the main component
[0076] S3.1: First, weigh MAH and BIBP, dissolve them in acetone, and stir until completely dissolved to prepare a mixed liquid, wherein the volume ratio of MAH to BIBP is 1:0.5;
[0077] S3.2: Then, 60% of the total mass of high-density polyethylene is added to the mixer as the grafting body, and the mixture is taken out after mixing for 8 minutes to obtain a mixture;
[0078] S3.3: Pour the mixed material into the hopper of a twin-screw extruder, and use the twin-screw extruder to melt and extrude the mixed material at a melting temperature of 160° C. to obtain a compatibilizer for low-smoke halogen-free cable materials.
[0079] Embodiment 3:
[0080] A preparation process of a compatibilizer for low-smoke halogen-free cable materials, such as Figure 1 As shown, the following steps are included:
[0081] S1: Preparation of catalyst suspension
[0082] S1.1: Dissolve 6 parts by mass of tetrabutyl titanate and 1 part by mass of ethylene glycol in 60 parts by volume of anhydrous ethanol, heat and condense under reflux for 280 min, and rotary evaporate at 60°C for 50 min to obtain a viscous liquid product;
[0083] S1.2: The viscous liquid product and 1.5 parts by mass of (2-carboxyethyl)phenylphosphonic acid are dissolved in 25 parts by volume of anhydrous ethanol to obtain a viscous solution and a (2-carboxyethyl)phenylphosphonic acid solution, respectively. The (2-carboxyethyl)phenylphosphonic acid solution is slowly added dropwise to the viscous solution and reacted at 85°C for 45 minutes.
[0084] S1.3: The mixture was then centrifuged twice using a high-speed refrigerated centrifuge, dried and ground to obtain a titanium-based catalyst powder. The titanium-based catalyst powder was then dissolved in deionized water at a solid-liquid ratio of 1:15, and stirred at a high speed to obtain a catalyst suspension.
[0085] S2: Preparation of high-density polyethylene
[0086] S2.1: 600 parts by volume of n-hexane is introduced into the reactor, and the reactor is degassed using a vacuum pump;
[0087] S2.2: The reactor temperature was raised to 80°C, and then pressurized to 2 MPa with hydrogen and ethylene, with a volume ratio of hydrogen to ethylene of 3.5:1;
[0088] S2.3: Then, the triethylaluminum solution was injected into the reactor using an injection device, and the reaction was continued for 5 minutes. The catalyst suspension was injected into the reactor and polymerization was started. The amount of the triethylaluminum solution added was 10 mg / L, and the amount of the catalyst suspension added was 5 mg / L.
[0089] S2.4: monitor the ethylene absorption rate using a mass flow controller and recover the consumed ethylene by injecting new ethylene gas into the reactor to maintain the total pressure of the reactor constant;
[0090] S2.5: After 20 minutes, the gas is discharged and the reactor is cooled to 75°C, then a gas mixture of hydrogen and ethylene is injected into the reactor, wherein the volume ratio of hydrogen to ethylene in the gas mixture of hydrogen and ethylene is 1.5:1, and the second stage polymerization is started at this time;
[0091] S2.6: After another 8-15 minutes, exhaust the remaining gas and stabilize the reactor at 70°C, continue to add ethylene gas and titanium catalyst powder, the amount of titanium catalyst powder added is 0.5% of the total mass of the system, and wait until the reaction is sufficient;
[0092] S2.7: Finally, the gas in the reactor is discharged, and the polymer powder in the reactor is collected and dried in an oven at 80°C overnight to obtain high-density polyethylene.
[0093] S3: Preparation of compatibilizer using high-density polyethylene as the main component
[0094] S3.1: First, weigh MAH and BIBP, dissolve them in acetone, and stir until completely dissolved to prepare a mixed liquid, wherein the volume ratio of MAH to BIBP is 1:0.5;
[0095] S3.2: Then, 75% of the total mass of high-density polyethylene is added to the mixer as the grafting body, and the mixture is taken out after mixing for 8 minutes to obtain a mixture;
[0096] S3.3: Pour the mixed material into the hopper of a twin-screw extruder, and use the twin-screw extruder to melt and extrude the mixed material at a melting temperature of 180° C. to obtain a compatibilizer for low-smoke halogen-free cable materials.
[0097] Comparative Example 1:
[0098] Compared with Example 1, Comparative Example 1 is a commercially available compatibilizer.
[0099] Comparative Example 2:
[0100] Compared with Example 1, Comparative Example 2 is commercially available high-density polyethylene.
[0101] Comparative Example 3:
[0102] Compared with Example 1, the difference of Comparative Example 3 is that, in step S2, a catalyst suspension is not used, but a titanium catalyst powder is used, specifically: “S2.1: 600 parts by volume of n-hexane is introduced into the reactor, and the reactor is degassed using a vacuum pump;
[0103] S2.2: The reactor temperature was raised to 90°C, and then pressurized to 4 MPa with hydrogen and ethylene, with a volume ratio of hydrogen to ethylene of 3.5:1;
[0104] S2.3: Then, the triethylaluminum solution was injected into the reactor using an injection device, and the reaction was carried out for 10 minutes. The titanium catalyst powder was injected into the reactor and polymerization was started. The amount of triethylaluminum solution added was 10 mg / L, and the amount of titanium catalyst powder added was 0.5% of the total mass of the system.
[0105] S2.4: monitor the ethylene absorption rate using a mass flow controller and recover the consumed ethylene by injecting new ethylene gas into the reactor to maintain the total pressure of the reactor constant;
[0106] S2.5: After 20 minutes, the gas is discharged and the reactor is cooled to 80°C, then a gas mixture of hydrogen and ethylene is injected into the reactor, wherein the volume ratio of hydrogen to ethylene in the gas mixture of hydrogen and ethylene is 1.5:1, and the second stage polymerization is started at this time;
[0107] S2.6: After another 8 minutes, exhaust the remaining gas and stabilize the reactor at 78°C, continue to add ethylene gas and titanium catalyst powder, the amount of titanium catalyst powder added is 0.5% of the total mass of the system, and wait until the reaction is sufficient;
[0108] S2.7: Finally, the gas in the reactor was discharged, and the polymer powder in the reactor was collected and dried in an oven at 100° C. overnight to obtain a high-density polyethylene. The prepared high-density polyethylene was recorded as Comparative Example 3.
[0109] Comparative Example 4:
[0110] Compared with Example 1, the difference of Comparative Example 4 is that the high-density polyethylene used in step S3 is commercially available high-density polyethylene, specifically: “S3.1: First, weigh MAH and BIBP, and dissolve them in acetone, stirring until completely dissolved to prepare a mixed liquid, wherein the volume ratio of MAH to BIBP is 1:0.5;
[0111] S3.2: Then, 75% of the total mass of the system of commercially available high-density polyethylene as the grafting body is added to the mixer, and the mixture is taken out after mixing for 8 minutes to obtain a mixture;
[0112] S3.3: Pour the mixed material into the hopper of a twin-screw extruder, and use the twin-screw extruder to melt and extrude the mixed material at a melting temperature of 160° C. to obtain a compatibilizer for low-smoke halogen-free cable materials, which is recorded as Comparative Example 4.
[0113] Intrinsic viscosity test
[0114] 125 mg of the high-density polyethylene prepared in Examples 1-3 and Comparative Examples 2 and 3 were respectively dissolved in phenol / tetrachloroethane (the mass ratio of phenol to tetrachloroethane was 1:1) to prepare a solution with a mass concentration of 5 mg / mL. The flow time of the sample solution was tested using an Ubbelohde viscometer, and the intrinsic viscosity of the sample was calculated as η = (√(1+1.4(t1-t0) / t0)-1) / 0.7c.
[0115] Wherein, η is the intrinsic viscosity, c is the concentration of the sample in the phenol / tetrachloroethane solution, t0 is the flow time of the solvent, and t1 is the flow time of the sample solution, as shown in Table 1.
[0116] Table 1: Intrinsic viscosity test of examples and comparative examples
[0117]
[0118] It can be seen that the intrinsic viscosity of the high-density polyethylene of Example 1 is the largest among all the measured data, reaching 0.924 g / dL. The intrinsic viscosities of Examples 2 and 3 also reached 0.898 g / dL and 0.905 g / dL. A larger intrinsic viscosity means better adhesion, while the intrinsic viscosities of Comparative Examples 2 and 3 are only 0.879 g / dL and 0.653 g / dL, respectively. This proves that the high-density polyethylene prepared using the catalyst suspension has a better intrinsic viscosity. This is because the catalyst suspension can fully contact with the reaction gas to improve the catalytic effect, so that the generated high-density polyethylene has better stability and viscosity, and its intrinsic viscosity is better than that of the commercially available high-density polyethylene of Comparative Example 2, so that when the compatibilizer is subsequently prepared, it has better binding force to the functional monomer, thereby improving the adhesion performance of the compatibilizer.
[0119] Grafting rate determination
[0120] Weigh 1g of the compatibilizer of Examples 1-3 and Comparative Examples 1 and 4, add 100mL of xylene to a conical flask, put it in a 150°C constant temperature oil bath, and wait for about 1.5h until it dissolves; leave the oil bath to make the solution temperature about 100°C, pour it into a large beaker containing 200mL of acetone, until the compatibilizer precipitates, filter it, and place it in an oven at 70-100°C for 1h to obtain a purified sample. Then accurately weigh about 0.5g (accurate to 0.001g) of the purified sample, record it as M, and dissolve it in 100mL of xylene (about 1h), leave the conical flask in the oil bath, and cool it for 5-10min (about 70°C). Use a pipette to accurately measure 10 mL of potassium hydroxide-ethanol solution (with a standardized concentration), add it to a conical flask, and heat to reflux for 15 minutes. When there is no condensation or reflux, remove the conical flask; add 3 drops of phenolphthalein indicator, and back-titrate with acetic acid-xylene solution (with a standardized concentration) to change the solution color from red to white, and record the consumed acid volume V1.
[0121] Weigh the blank sample according to the same steps and titrate the acid volume V0 consumed by the blank sample.
[0122] Grafting rate G = (V0-V1) * C / M * 4.9
[0123] Wherein, C is the concentration of acetic acid-xylene solution, and M is the mass of purified sample, as shown in Table 2.
[0124] Table 2: Grafting rate of examples and comparative examples
[0125]
[0126] It can be seen that the grafting rate of Example 1 reaches 0.94%, and that of Example 2 and Example 3 are also 0.92% and 0.91%. That is to say, the grafting efficiencies of the embodiments are 94%, 92% and 91%, respectively, while the grafting rate of Comparative Example 1 of the commercially available product is not as high as that of the embodiments, being only 0.84%. It can be seen that the compatibilizer of the embodiments has a higher grafting rate, i.e., better binding force to the functional monomer.
[0127] The grafting rate of comparative example 4 is only 0.78%, which indicates that the high-density polyethylene prepared by the present invention has better adhesion and has an auxiliary effect on improving the adhesion performance of the compatibilizer prepared subsequently.
[0128] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A process for preparing a compatibilizer for low-smoke halogen-free cable materials, characterized in that: The following steps are involved: S1: Preparation of catalyst suspension Dissolving tetrabutyl titanate and ethylene glycol in anhydrous ethanol, heating, condensing and refluxing to obtain a viscous liquid product, then dissolving the viscous liquid product and (2-carboxyethyl)phenylphosphonic acid in anhydrous ethanol to obtain a viscous solution and a (2-carboxyethyl)phenylphosphonic acid solution, respectively, slowly dropping the (2-carboxyethyl)phenylphosphonic acid solution into the viscous solution for reaction, then centrifuging using a high-speed refrigerated centrifuge, drying and grinding to obtain a titanium-based catalyst powder, then dissolving the titanium-based catalyst powder in deionized water to obtain a catalyst suspension; S2: Preparation of high-density polyethylene S2.1: 600-700 parts by volume of n-hexane are introduced into the reactor, and the reactor is degassed using a vacuum pump; S2.2: Raise the reactor temperature to 80-100°C and then pressurize it to 2-4 MPa with hydrogen and ethylene; S2.3: Then, the triethylaluminum solution is injected into the reactor using an injection device, and the reaction is carried out for 5-10 minutes. The catalyst suspension is injected into the reactor and polymerization is started. The amount of the triethylaluminum solution added is 10-50 mg / L, and the amount of the catalyst suspension added is 5-8 mg / L; S2.4: monitor the ethylene absorption rate using a mass flow controller and recover the consumed ethylene by injecting new ethylene gas into the reactor to maintain the total pressure of the reactor constant; S2.5: After 10-20 min, the gas is discharged and the reactor is cooled to 70-80°C, then a gas mixture of hydrogen and ethylene is injected into the reactor, and the second stage polymerization is started at this time; S2.6: After another 8-15 minutes, exhaust the gas to stabilize the reactor at 70-78°C, continue to add ethylene gas and titanium catalyst powder, the amount of titanium catalyst powder added is 0.5% of the total mass of the system, and wait for 10-20 minutes for the reaction to be fully completed; S2.7: Finally, the gas in the reactor is discharged, the polymer powder in the reactor is collected and dried in an oven at 80-100°C overnight to obtain high-density polyethylene; S3: Preparation of compatibilizer using high-density polyethylene as the main component First, MAH and BIBP are weighed and dissolved in acetone to prepare a mixed liquid, and the mixed liquid is added to a mixer, and then high-density polyethylene is added to the mixer as a grafting body to obtain a mixture, and the mixture is poured into a hopper of a twin-screw extruder, and melt-extruded using the twin-screw extruder to obtain a compatibilizer for low-smoke halogen-free cable materials.
2. The preparation process of the compatibilizer for low-smoke halogen-free cable materials according to claim 1, characterized in that: Step S1: preparing a catalyst suspension, comprising the following steps: S1.1: Dissolve 6-8 parts by mass of tetrabutyl titanate and 1-2 parts by mass of ethylene glycol in 50-60 parts by volume of anhydrous ethanol, heat and condense under reflux for 260-280 min, and rotary evaporate at 60-70° C. for 50-60 min to obtain a viscous liquid product; S1.2: The viscous liquid product and 1-1.5 parts by mass of (2-carboxyethyl)phenylphosphonic acid are respectively dissolved in 25 parts by volume of anhydrous ethanol to obtain a viscous solution and a (2-carboxyethyl)phenylphosphonic acid solution, and the (2-carboxyethyl)phenylphosphonic acid solution is slowly added dropwise to the viscous solution, and the reaction is carried out at 80-85°C for 40-45 minutes; S1.3: The mixture is then centrifuged twice using a high-speed refrigerated centrifuge, dried and ground to obtain a titanium-based catalyst powder. The titanium-based catalyst powder is then dissolved in deionized water at a solid-to-liquid ratio of 1:(15-30), and stirred at high speed to obtain a catalyst suspension.
3. The preparation process of the compatibilizer for low-smoke halogen-free cable materials according to claim 2, characterized in that: Step S3 uses high-density polyethylene as the main component to prepare a compatibilizer, comprising the following steps: S3.1: First, weigh MAH and BIBP, dissolve them in acetone, stir until completely dissolved, prepare a mixed liquid, and add the mixed liquid into a mixer; S3.2: Then, 50-75% of the total mass of high-density polyethylene is added to the mixer as the grafting body, and the mixture is taken out after mixing for 5-8 minutes to obtain a mixture; S3.3: Pour the mixed material into the hopper of a twin-screw extruder, and use the twin-screw extruder to melt and extrude the mixed material at a melting temperature of 140-180° C. to obtain a compatibilizer for low-smoke halogen-free cable materials.
4. The preparation process of the compatibilizer for low-smoke halogen-free cable materials according to claim 3, characterized in that: The volume ratio of hydrogen to ethylene in step S2.2 is (3.5-7):
1.
5. The preparation process of the compatibilizer for low-smoke halogen-free cable materials according to claim 4, characterized in that: The volume ratio of hydrogen to ethylene in the gas mixture of hydrogen and ethylene in step S2.5 is 1.5:
1.
6. The preparation process of the compatibilizer for low-smoke halogen-free cable materials according to claim 5, characterized in that: The volume ratio of MAH and BIBP in step S3.1 is 1:(0.5-2).