A polyester film with excellent optical and mechanical properties and its preparation process

By using a slit coating head and a coating solution of PS/SiO2 microspheres rich in H+ on the surface before longitudinal stretching of the PET film for online coating, the problems of easy cracking and uneven thickness of the coating are solved, and the efficiency is improved. Optical and mechanical properties of polyester films.

CN118562180BActive Publication Date: 2024-10-25JIANGSU KANGHUI NEW MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411060290.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-25
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

In the existing technology, it is difficult to perform online coating before longitudinal stretching during the biaxial stretching process of PET film, which results in the coating being prone to cracking and uneven thickness, affecting the optical and mechanical properties of the polyester film.

Method used

Using a slit coating head and a coating liquid of PS/SiO2 microspheres rich in H+ on the surface, online coating is performed before longitudinal stretching. The bonding fastness of the coating is improved through the chemical bond reaction of the curing agent, and the high H+ content is used. Combined fastness and even density distribution ensure uniform coating thickness.

Benefits of technology

The optical and mechanical properties of the polyester film have been improved. The coating does not crack during the biaxial stretching process, has a uniform thickness, increases the tensile strength and transmittance, and reduces haze.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118562180B_ABST
    Figure CN118562180B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of polymer materials, and relates to a polyester film with excellent optical and mechanical properties and a preparation process thereof. Preparation process: After coating the surface of a thick polyester sheet with a coating liquid, biaxial stretching and heat setting are performed in sequence to obtain a polyester film with excellent optical and mechanical properties; a slit coating head is used for coating; the coating liquid is composed of a water-based polyester, a surface rich in H + The invention comprises PS / SiO2 microspheres, a curing agent, a wetting agent and water; the curing agent reacts during the heat setting process; the obtained polyester film with excellent optical and mechanical properties comprises a polyester base film and a coating on its surface. The invention applies the coating liquid online before the polyester thick sheet is longitudinally stretched, and the obtained polyester film has excellent optical and mechanical properties, which solves the problem of easy cracking and uneven thickness of the coating caused by applying the coating liquid before longitudinal stretching in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a polyester film with excellent optical and mechanical properties and a preparation process thereof. Background Art

[0002] PET is a saturated linear macromolecular material with a symmetrical structure and no branches on the main chain. This property makes PET easy to orient and crystallize, giving it the characteristics of high melting point and high strength. In the manufacturing process of PET film, PET is stretched in both the longitudinal and transverse directions in the appropriate temperature range above the glass transition temperature and below the melting point, so that the molecular chains are highly ordered in the plane of the film, thereby significantly improving the tensile strength and elastic modulus of the film.

[0003] However, in practical applications, the winding performance of PET film is limited by the large friction coefficient of its surface. In order to improve the winding performance, the traditional practice is to add an opening agent to the surface of the film. Although this practice performs well in terms of cost-effectiveness and stability, it often causes other properties of the film, such as transparency and scratch resistance, to be affected to a certain extent, and the operation process may be more cumbersome, affecting production efficiency. For this reason, the prior art attempts to add an opening agent to the coating liquid, and apply the coating liquid containing the opening agent to the film by online coating. This can not only reduce the friction coefficient of the film surface to a certain extent and improve the winding performance, but also avoid a greater impact on other properties of the film, while also improving production efficiency.

[0004] In the processing of the film, the prior art often performs online coating after longitudinal stretching and before transverse stretching. For example, patent application CN112844944A discloses a method for preparing a low-color hardened pre-coated base film, which performs online coating after longitudinal stretching and before transverse stretching. In the prior art, online coating is rarely performed before longitudinal stretching, because the stretching ratio of the film during biaxial stretching is very large, which will not only cause cracking of the coating, but also make it difficult to obtain a product with uniform coating thickness.

[0005] However, during the stretching process of the film, the earlier the coating liquid contacts the film, the easier it is to penetrate into the microstructure of the film, thereby forming a strong and uniform coating. Therefore, it is necessary to achieve online coating before longitudinal stretching while avoiding cracking of the coating and ensuring uniform coating thickness. Summary of the invention

[0006] The purpose of the present invention is to solve the problems existing in the prior art and to provide a polyester film having excellent optical and mechanical properties and a preparation process thereof.

[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A process for preparing a polyester film with excellent optical and mechanical properties, wherein a coating liquid is coated on the surface of a thick polyester sheet, and then biaxial stretching and heat setting are performed in sequence to obtain a polyester film with excellent optical and mechanical properties;

[0009] The coating adopts a slit coating head;

[0010] The coating liquid is composed of water-based polyester, surface rich in H + PS / SiO2 microspheres, curing agent, wetting agent and water; the surface is rich in H + The density of PS / SiO2 microspheres is 1-1.05g / m 3 ;

[0011] The surface is rich in H + The preparation process of PS / SiO2 microspheres is as follows: first, hydrated silica is coated on the surface of PS microspheres (i.e., polystyrene microspheres) by the sol-gel method to obtain a surface rich in NH4 + PS / SiO2 microspheres, and then the surface is rich in NH4 + PS / SiO2 microspheres were treated with acid to remove NH4 + Replace with H + , the surface is rich in H + PS / SiO2 microspheres;

[0012] The curing agent reacts during the heat setting process.

[0013] The surface of the polyester thick sheet of the present invention is coated with a coating liquid, so that during the biaxial stretching process, the coating liquid can fill the micro cracks left during the stretching process of the polyester thick sheet; during the heat setting process, the curing agent reacts to connect the water-based polyester with active groups such as carbonyl and ester groups in the polyester film through chemical bonds, thereby improving the bonding strength of the coating and the polyester film.

[0014] It is difficult to apply the coating liquid online before longitudinal stretching in the prior art, because the stretching ratio of the film during the biaxial stretching process is very large, which will cause the coating to crack; the present invention selects water-based polyester of the same material as PET as the base material of the coating to ensure that the coating does not crack during the biaxial stretching process.

[0015] In the prior art, it is difficult to obtain a product with uniform coating thickness by applying the coating liquid online before longitudinal stretching. The present invention can obtain a product with uniform coating thickness by applying the coating liquid online before longitudinal stretching. The main reasons are as follows:

[0016] (1) The present invention adopts a slit coating head to ensure uniformity of coating weight;

[0017] (2) The present invention uses a surface rich in H + PS / SiO2 microspheres, H +The bonding strength with PS / SiO2 microspheres is high. + It is not easy to leave the PS / SiO2 microspheres and enter the coating liquid. The low ion concentration of the coating liquid can be maintained for a long time, which can ensure that the PS / SiO2 microspheres can still generate a sufficiently strong repulsive force at low concentrations. This repulsive force is sufficient to maintain the orderly arrangement between them, thereby forming an orderly crystal structure, thereby ensuring that the PS / SiO2 microspheres can be evenly distributed during the coating process without local aggregation or sparseness. Through this orderly arrangement and uniform distribution, a coating with uniform thickness and stable performance can be finally obtained;

[0018] If the surface is enriched with NH4 + PS / SiO2 microspheres, NH4 + The bonding strength with PS / SiO2 microspheres is low, NH4 + It is easy to leave the PS / SiO2 microspheres and enter the coating solution, which leads to an increase in the ion concentration of the coating solution, and produces a serious shielding effect on the electrostatic repulsion between the PS / SiO2 microspheres, making it difficult for the PS / SiO2 microspheres to generate a strong enough repulsive force to maintain an orderly crystal structure at low concentrations, and then the PS / SiO2 microspheres are disordered during the coating process, forming an irregular aggregation state, and finally leading to uneven coating thickness, affecting the performance and quality of the coating;

[0019] (3) Surface rich in H + The density of PS / SiO2 microspheres is close to that of water and water-based polyester, and no sedimentation will occur after dispersion;

[0020] (4) The coating liquid does not contain emulsifier. If emulsifier is present, bubbles will be generated very easily, which will greatly affect the coating uniformity and surface appearance quality.

[0021] As the preferred technical solution:

[0022] The above-mentioned process for preparing a polyester film having excellent optical and mechanical properties comprises the following components in the coating solution: 15-20 parts of water-based polyester, a surface rich in H + 3-5 parts of PS / SiO2 microspheres, 0.5-1 parts of curing agent, 0.02-0.04 parts of wetting agent, and 130-150 parts of water.

[0023] As described above, a polyester film having excellent optical and mechanical properties has a surface rich in H + In the PS / SiO2 microspheres, the diameter of the PS microspheres is 50-60nm, and the thickness of the shell is 20-30nm, so that the surface is rich in H +The refractive index of PS / SiO2 microspheres is not less than 1.55%, which is close to the refractive index of PET 1.6%, which is beneficial to reduce the haze of the product.

[0024] As described above, a polyester film having excellent optical and mechanical properties has a surface rich in H + The preparation steps of PS / SiO2 microspheres are as follows:

[0025] (1) Add dispersant (NaPO3)6 to a mixed solution of deionized water and isopropanol, stir at a speed of 500-800 rpm for 10-15 minutes, add PS microspheres, stir at a speed of 8000-1000 rpm for 20-25 minutes to prepare a slurry, and pass the slurry through a sand mill 3-5 times to ensure that the PS microspheres are evenly dispersed;

[0026] (2) Stirring the slurry at 60±0.5°C and 200-250 rpm for 25-30 min, during which time 10-35% ammonia water was added dropwise to adjust the pH value to 9-10;

[0027] (3) stirring the slurry at 60±0.5°C and 200-250 rpm for 55-60 min, during which tetraethyl orthosilicate (TEOS) was added dropwise;

[0028] In steps (1) to (3), isopropanol, deionized water, PS microspheres, (NaPO3) 6、 The mass ratio of ethyl orthosilicate is 20-30:50-60:15-20:0.5-1:4-5;

[0029] (4) Stir the slurry at 90±0.5°C and 200-250 rpm for 180-200 min, then cool, wash, filter and dry to obtain a NH4-rich + PS / SiO2 microspheres;

[0030] (5) Enrich the surface with NH4 + The PS / SiO2 microspheres were dispersed in water to obtain a dispersion with a solid content of 15-20%, and stirred at a speed of 200-250 rpm for 50-60 min. During this process, dilute hydrochloric acid with a mass concentration of 20-36% was added dropwise to adjust the pH value to 4-5, washed, filtered, and dried to obtain a dispersion rich in H + PS / SiO2 microspheres.

[0031] As described above, the preparation process of a polyester film with excellent optical and mechanical properties, the preparation process of a polyester thick sheet is as follows: first, the raw material slices are crystallized and dried at 150-180°C, and then sent to a corresponding extrusion system for melt extrusion to obtain a melt, the melt extrusion temperature is 260-285°C, and then the melt is cooled on a rotating cooling roller through a die head to obtain a polyester thick sheet.

[0032] As described above, the preparation process of a polyester film with excellent optical and mechanical properties is biaxially stretched, that is, stretched 3.5-4.5 times in the transverse direction and 3-4 times in the longitudinal direction in a drying oven at 90-180°C, and the coating liquid is leveled and dried here.

[0033] In the above-mentioned process for preparing a polyester film having excellent optical and mechanical properties, the heat setting temperature is 220-245°C.

[0034] The present invention also provides a polyester film with excellent optical and mechanical properties, which is prepared by the preparation process of a polyester film with excellent optical and mechanical properties as described in any one of the above items, and comprises a polyester base film and a coating on the surface thereof.

[0035] As the preferred technical solution:

[0036] The polyester film with excellent optical and mechanical properties as described above has coatings on both sides of the polyester base film, a single coating has a thickness of 40-60 nm, and a coating roughness Ra of 6-10 nm.

[0037] As described above, a polyester film with excellent optical and mechanical properties, the polyester base film consists of an upper surface layer, a core layer, and a lower surface layer; the raw materials of the upper surface layer and the lower surface layer are both film-grade slices; the raw material of the core layer is a mixture of high-gloss slices and PEI, wherein the mass content of PEI is 5-10%; the thickness of the upper surface layer or the lower surface layer is 0.5-0.75μm, and the thickness of the core layer is 3-4.5μm.

[0038] A polyester film having excellent optical and mechanical properties as described above, wherein the polyester film having excellent optical and mechanical properties has a longitudinal tensile strength of ≥240 MPa, a transverse tensile strength of ≥330 MPa, a longitudinal elastic modulus of ≥4.3 GPa, a transverse elastic modulus of ≥6.6 GPa, a haze of 0.5-0.8%, and a transmittance of 92-95%;

[0039] The polyester film with excellent optical and mechanical properties of the present invention has no microcracks on its surface. If there are microcracks on the surface, the material will easily deform from the cracks until it breaks during a tensile test, which will reduce the tensile strength and elastic modulus. The high tensile strength and elastic modulus of the present invention also confirm that the polyester film with excellent optical and mechanical properties of the present invention has no microcracks on its surface.

[0040] The coating thickness of the polyester film with excellent optical and mechanical properties of the present invention is uniform. If the coating thickness is uneven, the haze in the local area will increase and the transmittance will decrease. The lower haze and higher transmittance of the present invention also confirm that the coating thickness of the polyester film with excellent optical and mechanical properties of the present invention is uniform.

[0041] Beneficial effects:

[0042] (1) The present invention applies the coating liquid online before the polyester thick sheet is longitudinally stretched, and the obtained polyester film has excellent optical and mechanical properties, which solves the problem of easy cracking and uneven thickness of the coating caused by applying the coating liquid before longitudinal stretching in the prior art.

[0043] (2) The present invention uses water-based polyester, which is the same material as PET, as the coating substrate, ensuring that the coating does not crack during the biaxial stretching process.

[0044] (3) The coating liquid of the present invention is coated using a slit coating head, which ensures the uniformity of the coating weight.

[0045] (4) The coating solution of the present invention contains a surface rich in H + The PS / SiO2 microspheres have high bonding strength and can maintain low ion concentration in the coating solution, ensuring uniform distribution of PS / SiO2 microspheres, forming an ordered crystal structure, and ensuring uniform coating thickness; the surface is rich in H + The density of PS / SiO2 microspheres is close to that of water and water-based polyester. They do not settle after dispersion, and the coating liquid does not contain emulsifiers to avoid bubbles affecting the coating uniformity and surface appearance quality.

[0046] (5) In the heat setting process of the present invention, the curing agent reacts to connect the water-based polyester with the active groups in the polyester film through chemical bonds, thereby improving the bonding strength between the coating and the polyester film. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a schematic diagram of the structure of a polyester film having excellent optical and mechanical properties according to Example 1 of the present invention;

[0048] Among them, 1-upper coating layer, 2-upper surface layer, 3-core layer, 4-lower surface layer, 5-lower coating layer. DETAILED DESCRIPTION

[0049] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0050] The following are the test methods for the relevant performance indicators in each embodiment and comparative example:

[0051] Coating thickness: An optical thickness gauge (manufacturer: NXT GmbH, model: Metis LITE RT-VIS) was used for testing, and the film thickness accuracy mode of 40-200nm was adopted during the test.

[0052] Roughness Ra: measured using a 3D surface profiler (manufacturer: KEYENCE Corporation, model: VK-X3100) in white light interferometry mode.

[0053] Tensile strength and elastic modulus: Tested in accordance with ASTM D882-2009 standard; 5 areas were randomly selected from the polyester film, each with a size of 200×10 mm. After cutting out 5 areas to obtain 5 samples, each sample was tested. The gauge length during the test was 100 mm, the test environment was 25°C, 50% RH, the tensile rate was 100 mm / min, the preload was 0.3 N, the elastic modulus was 0.3~0.8% (non-platform area), and the average value was taken after the test.

[0054] Haze and transmittance: measured in accordance with ASTM D1003-2013 standard; 5 areas were randomly selected from the polyester film, 5 areas were cut out to obtain 5 samples, each sample was tested, and the average value was taken after the test.

[0055] Example 1

[0056] A process for preparing a polyester film having excellent optical and mechanical properties, the specific steps are as follows:

[0057] (1) Preparation of raw materials;

[0058] (NaPO3)6;

[0059] A mixed solution of deionized water and isopropyl alcohol;

[0060] PS microspheres: manufacturer is Zhongke Leiming (Beijing) Technology Co., Ltd., item number is PS000050, diameter is 50nm;

[0061] Ammonia water: mass concentration is 10%, the solvent is water;

[0062] Tetraethyl orthosilicate;

[0063] water;

[0064] Dilute hydrochloric acid: mass concentration is 20%, the solvent is water;

[0065] Water-based polyester: manufacturer is Toyobo Co., Ltd., model number is MD1200;

[0066] Curing agent: water-based closed curing agent, the manufacturer is Anhui Anda Huatai New Materials Co., Ltd., model A05;

[0067] Wetting agent: manufacturer is Evonik Industries, model is surfynol 104E;

[0068] Raw material slice a and raw material slice b: both are film-grade slices (manufacturer: Kanghui New Material Technology Co., Ltd., model: KH2650A);

[0069] Raw material slice c: a mixture of Dayouguang slice (manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., product number is FG604) and PEI (manufacturer is Saudi Basic Industries Corporation, brand name is PEI 2110), wherein the mass content of PEI is 5%;

[0070] (2) Preparation of surface H-rich + PS / SiO2 microspheres;

[0071] (2.1) Add (NaPO3)6 to a mixed solution of deionized water and isopropanol, stir at 500 rpm for 10 minutes, add PS microspheres, stir at 8000 rpm for 20 minutes to prepare a slurry, and pass the slurry through a sand mill three times;

[0072] (2.2) stirring the slurry at 59.5°C and 200 rpm for 25 min, during which time aqueous ammonia was added dropwise to adjust the pH value to 9;

[0073] (2.3) stirring the slurry at 59.5°C and 200 rpm for 55 min, during which ethyl orthosilicate was added dropwise thereto;

[0074] (2.4) The slurry was stirred at 89.5°C and 200 rpm for 180 min, then cooled, washed, filtered, and dried to obtain a surface-rich NH4 + PS / SiO2 microspheres;

[0075] (2.5) enrich the surface with NH4 + PS / SiO2 microspheres were dispersed in water to obtain a dispersion with a solid content of 15%, and stirred at 200 rpm for 50 min. During this process, dilute hydrochloric acid was added dropwise to adjust the pH value to 5. The dispersion was washed, filtered and dried to obtain a shell layer (i.e., SiO2) with a thickness of 20 nm and a density of 1 g / m 3 The surface is rich in H + PS / SiO2 microspheres;

[0076] Wherein, in steps (2.1) to (2.3), the mass ratio of isopropanol, deionized water, PS microspheres, (NaPO3)6, and tetraethyl orthosilicate is 20:50:15:0.5:4;

[0077] (3) preparing a coating solution;

[0078] The contents of each component in the coating solution are as follows: 15 parts of water-based polyester, surface-rich H + 3 parts of PS / SiO2 microspheres, 0.5 parts of curing agent, 0.02 parts of wetting agent, and 130 parts of water;

[0079] (4) Preparation of polyester films with excellent optical and mechanical properties;

[0080] (4.1) First, raw material slice a, raw material slice b and raw material slice c are crystallized and dried at 150-180°C, and then sent to a corresponding extrusion system for melt extrusion to obtain a melt, the melt extrusion temperature is 260-285°C, and then the melt is cooled on a rotating cooling roller through a die head to obtain a polyester thick sheet;

[0081] (4.2) After coating the coating liquid on both sides of the polyester thick sheet using a slit coating head, it is first stretched 3.5 times in the transverse direction and 3 times in the longitudinal direction in a drying oven at 90°C, and then heat-set at 220°C to obtain a polyester film with excellent optical and mechanical properties.

[0082] The structure of the polyester film with excellent optical and mechanical properties is as follows: Figure 1 As shown, it is composed of an upper coating layer 1, an upper surface layer 2 (made of film-grade slices), a core layer 3 (made of a mixture of large-light slices and PEI), a lower surface layer 4 (made of film-grade slices) and a lower coating layer 5 from top to bottom; the thickness of the upper coating layer 1 and the lower coating layer 5 are both 40nm, and the roughness Ra is 6nm; the thickness of the upper surface layer 2 and the lower surface layer 4 are both 0.5μm; the thickness of the core layer 3 is 3μm; the polyester film with excellent optical and mechanical properties has a longitudinal tensile strength of 240MPa, a transverse tensile strength of 330MPa, a longitudinal elastic modulus of 4.3GPa, a transverse elastic modulus of 6.6GPa, a haze of 0.5%, and a transmittance of 95%.

[0083] Comparative Example 1

[0084] A preparation process of a polyester film, the specific steps are as follows:

[0085] (1) Preparation of raw materials;

[0086] (NaPO3)6;

[0087] A mixed solution of deionized water and isopropyl alcohol;

[0088] PS microspheres: manufacturer is Zhongke Leiming (Beijing) Technology Co., Ltd., item number is PS000050, diameter is 50nm;

[0089] Ammonia water: mass concentration is 10%, the solvent is water;

[0090] Tetraethyl orthosilicate;

[0091] water;

[0092] Water-based polyester: manufacturer is Toyobo Co., Ltd., model number is MD1200;

[0093] Curing agent: water-based closed curing agent, the manufacturer is Anhui Anda Huatai New Materials Co., Ltd., model A05;

[0094] Wetting agent: manufacturer is Evonik Industries, model is surfynol 104E;

[0095] Raw material slice a and raw material slice b: both are film-grade slices (manufacturer: Kanghui New Material Technology Co., Ltd., model: KH2650A);

[0096] Raw material slice c: a mixture of Dayouguang slice (manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., product number is FG604) and PEI (manufacturer is Saudi Basic Industries Corporation, brand name is PEI 2110), wherein the mass content of PEI is 5%;

[0097] (2) Preparation of surface NH4-rich + PS / SiO2 microspheres;

[0098] (2.1) Add (NaPO3)6 to a mixed solution of deionized water and isopropanol, stir at 500 rpm for 10 minutes, add PS microspheres, stir at 8000 rpm for 20 minutes to prepare a slurry, and pass the slurry through a sand mill three times;

[0099] (2.2) stirring the slurry at 59.5°C and 200 rpm for 25 min, during which time aqueous ammonia was added dropwise to adjust the pH value to 9;

[0100] (2.3) stirring the slurry at 59.5°C and 200 rpm for 55 min, during which ethyl orthosilicate was added dropwise thereto;

[0101] (2.4) The slurry was stirred at 89.5°C and 200 rpm for 180 min, then cooled, washed, filtered, and dried to obtain a surface-rich NH4 + PS / SiO2 microspheres;

[0102] Wherein, in steps (2.1) to (2.3), the mass ratio of isopropanol, deionized water, PS microspheres, (NaPO3)6, and tetraethyl orthosilicate is 20:50:15:0.5:4;

[0103] (3) preparing a coating solution;

[0104] The content of each component in the coating solution is as follows: 15 parts of water-based polyester, NH4-rich + 3 parts of PS / SiO2 microspheres, 0.5 parts of curing agent, 0.02 parts of wetting agent, and 130 parts of water;

[0105] (4) preparing polyester film;

[0106] (4.1) First, raw material slice a, raw material slice b and raw material slice c are crystallized and dried at 150-180°C, and then sent to a corresponding extrusion system for melt extrusion to obtain a melt, the melt extrusion temperature is 260-285°C, and then the melt is cooled on a rotating cooling roller through a die head to obtain a polyester thick sheet;

[0107] (4.2) After coating the coating liquid on both sides of the polyester thick sheet using a slit coating head, it is first stretched 3.5 times in the transverse direction and 3 times in the longitudinal direction in a drying oven at 90°C, and then heat-set at 220°C to obtain a polyester film.

[0108] The final polyester film consists of an upper coating layer, an upper surface layer (made of film-grade slices), a core layer (made of a mixture of optical chips and PEI), a lower surface layer (made of film-grade slices) and a lower coating layer from top to bottom; the thickness of the upper coating layer and the lower coating layer are both 40nm, and the roughness Ra is 6nm; the thickness of the upper surface layer and the lower surface layer are both 0.5μm; the thickness of the core layer is 3μm; the longitudinal tensile strength of the polyester film is 220MPa, the transverse tensile strength is 300MPa, the longitudinal elastic modulus is 4GPa, the transverse elastic modulus is 6GPa, the haze is 1.2%, and the transmittance is 88%.

[0109] Compared with Example 1, the mechanical and optical properties of the polyester film in Comparative Example 1 are significantly reduced. This is because the surface rich in NH4 + PS / SiO2 microspheres were treated with acid, while the surface-enriched NH4 + PS / SiO2 microspheres were prepared by coating liquid, NH4 + The bonding strength with PS / SiO2 microspheres is low, NH4 +It is easy to leave the PS / SiO2 microspheres and enter the coating liquid, which leads to an increase in the ion concentration of the coating liquid, and produces a serious shielding effect on the electrostatic repulsion between the PS / SiO2 microspheres, making it difficult for the PS / SiO2 microspheres to generate a strong enough repulsive force to maintain an ordered crystal structure at low concentrations. In turn, the PS / SiO2 microspheres are disordered during the coating process, forming an irregular aggregation state, and ultimately leading to uneven coating thickness, affecting the performance and quality of the coating, thereby affecting the mechanical and optical properties of the polyester film.

[0110] Example 2

[0111] A process for preparing a polyester film having excellent optical and mechanical properties, the specific steps are as follows:

[0112] (1) Preparation of raw materials;

[0113] (NaPO3)6;

[0114] A mixed solution of deionized water and isopropyl alcohol;

[0115] PS microspheres: The manufacturer is Suzhou Zhiyi Microsphere Technology Co., Ltd., the model is KBsphere® 0.06PS, and the diameter is 60nm;

[0116] Ammonia water: mass concentration is 35%, the solvent is water;

[0117] Tetraethyl orthosilicate;

[0118] water;

[0119] Dilute hydrochloric acid: mass concentration is 36%, the solvent is water;

[0120] Water-based polyester: manufacturer is Toyobo Co., Ltd., model number is MD1200;

[0121] Curing agent: water-based closed curing agent, the manufacturer is Anhui Anda Huatai New Materials Co., Ltd., model A05;

[0122] Wetting agent: manufacturer is Evonik Industries, model is surfynol 104E;

[0123] Raw material slice a and raw material slice b: both are membrane grade slices (manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model is FG600);

[0124] Raw material slice c: a mixture of Dayouguang slice (manufacturer is Hefei Lucky Technology Industry Co., Ltd., product name is LK-200) and PEI (manufacturer is Saudi Basic Industries Corporation, brand name is PEI 2110), wherein the mass content of PEI is 10%;

[0125] (2) Preparation of surface H-rich+ PS / SiO2 microspheres;

[0126] (2.1) Add (NaPO3)6 to a mixed solution of deionized water and isopropanol, stir at 800 rpm for 15 minutes, add PS microspheres, stir at 10000 rpm for 25 minutes to prepare a slurry, and pass the slurry through a sand mill 5 times;

[0127] (2.2) stirring the slurry at 60.5°C and 250 rpm for 30 min, during which time aqueous ammonia was added dropwise to adjust the pH value to 10;

[0128] (2.3) stirring the slurry at 60.5°C and 250 rpm for 60 min, during which ethyl orthosilicate was added dropwise thereto;

[0129] (2.4) The slurry was stirred at 90.5°C and 250 rpm for 200 min, then cooled, washed, filtered, and dried to obtain a surface-rich NH4 + PS / SiO2 microspheres;

[0130] (2.5) enrich the surface with NH4 + PS / SiO2 microspheres were dispersed in water to obtain a dispersion with a solid content of 20%, and stirred at 250 rpm for 60 min. During this process, dilute hydrochloric acid was added dropwise to adjust the pH value to 4. The dispersion was washed, filtered and dried to obtain a shell layer (i.e., SiO2) with a thickness of 30 nm and a density of 1.05 g / m 3 The surface is rich in H + PS / SiO2 microspheres;

[0131] Wherein, in steps (2.1) to (2.3), the mass ratio of isopropanol, deionized water, PS microspheres, (NaPO3)6, and tetraethyl orthosilicate is 30:60:20:1:5;

[0132] (3) preparing a coating solution;

[0133] The contents of the components in the coating solution are as follows: 20 parts of water-based polyester, surface-rich H + 5 parts of PS / SiO2 microspheres, 1 part of curing agent, 0.04 parts of wetting agent, and 150 parts of water;

[0134] (4) Preparation of polyester films with excellent optical and mechanical properties;

[0135] (4.1) First, raw material slice a, raw material slice b and raw material slice c are crystallized and dried at 150-180°C, and then sent to a corresponding extrusion system for melt extrusion to obtain a melt, the melt extrusion temperature is 260-285°C, and then the melt is cooled on a rotating cooling roller through a die head to obtain a polyester thick sheet;

[0136] (4.2) After coating the coating liquid on both sides of the polyester thick sheet using a slit coating head, it is first stretched 4.5 times in the transverse direction and 4 times in the longitudinal direction in a drying oven at 180°C, and then heat-set at 245°C to obtain a polyester film with excellent optical and mechanical properties.

[0137] The polyester film with excellent optical and mechanical properties finally obtained is composed of an upper coating layer, an upper surface layer (made of film-grade slices), a core layer (made of a mixture of large-light slices and PEI), a lower surface layer (made of film-grade slices) and a lower coating layer from top to bottom; the thickness of the upper coating layer and the lower coating layer is 60nm, and the roughness Ra is 10nm; the thickness of the upper surface layer and the lower surface layer is 0.75μm; the thickness of the core layer is 4.5μm; the polyester film with excellent optical and mechanical properties has a longitudinal tensile strength of 300MPa, a transverse tensile strength of 380MPa, a longitudinal elastic modulus of 4.8GPa, a transverse elastic modulus of 7GPa, a haze of 0.8%, and a transmittance of 92%.

[0138] Example 3

[0139] A process for preparing a polyester film having excellent optical and mechanical properties, the specific steps are as follows:

[0140] (1) Preparation of raw materials;

[0141] (NaPO3)6;

[0142] A mixed solution of deionized water and isopropyl alcohol;

[0143] PS microspheres: The manufacturer is Suzhou Zhiyi Microsphere Technology Co., Ltd., the model is KBsphere® 0.06PS, and the diameter is 60nm;

[0144] Ammonia water: mass concentration is 35%, the solvent is water;

[0145] Tetraethyl orthosilicate;

[0146] water;

[0147] Dilute hydrochloric acid: mass concentration is 36%, the solvent is water;

[0148] Water-based polyester: manufacturer is Toyobo Co., Ltd., model number is MD1200;

[0149] Curing agent: water-based closed curing agent, the manufacturer is Anhui Anda Huatai New Materials Co., Ltd., model A05;

[0150] Wetting agent: manufacturer is Evonik Industries, model is surfynol 104E;

[0151] Raw material slice a and raw material slice b: both are membrane grade slices (manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model is FG600);

[0152] Raw material slice c: a mixture of Dayouguang slice (manufacturer is Hefei Lucky Technology Industry Co., Ltd., product name is LK-200) and PEI (manufacturer is Saudi Basic Industries Corporation, brand name is PEI 2110), wherein the mass content of PEI is 10%;

[0153] (2) Preparation of surface H-rich + PS / SiO2 microspheres;

[0154] (2.1) Add (NaPO3)6 to a mixed solution of deionized water and isopropanol, stir at 800 rpm for 15 minutes, add PS microspheres, stir at 10000 rpm for 25 minutes to prepare a slurry, and pass the slurry through a sand mill 5 times;

[0155] (2.2) stirring the slurry at 60.5°C and 250 rpm for 30 min, during which time aqueous ammonia was added dropwise to adjust the pH value to 10;

[0156] (2.3) stirring the slurry at 60.5°C and 250 rpm for 60 min, during which ethyl orthosilicate was added dropwise thereto;

[0157] (2.4) The slurry was stirred at 90.5°C and 250 rpm for 200 min, then cooled, washed, filtered, and dried to obtain a surface-rich NH4 + PS / SiO2 microspheres;

[0158] (2.5) enrich the surface with NH4 + PS / SiO2 microspheres were dispersed in water to obtain a dispersion with a solid content of 20%, and stirred at 250 rpm for 60 min. During this process, dilute hydrochloric acid was added dropwise to adjust the pH value to 4. The dispersion was washed, filtered and dried to obtain a shell layer (i.e., SiO2) with a thickness of 25 nm and a density of 1.05 g / m 3 The surface is rich in H + PS / SiO2 microspheres;

[0159] Wherein, in steps (2.1) to (2.3), the mass ratio of isopropanol, deionized water, PS microspheres, (NaPO3)6, and tetraethyl orthosilicate is 30:60:20:1:5;

[0160] (3) preparing a coating solution;

[0161] The contents of the components in the coating solution are as follows: 20 parts of water-based polyester, surface-rich H + 5 parts of PS / SiO2 microspheres, 1 part of curing agent, 0.04 parts of wetting agent, and 150 parts of water;

[0162] (4) Preparation of polyester films with excellent optical and mechanical properties;

[0163] (4.1) First, raw material slice a, raw material slice b and raw material slice c are crystallized and dried at 150-180°C, and then sent to a corresponding extrusion system for melt extrusion to obtain a melt, the melt extrusion temperature is 260-285°C, and then the melt is cooled on a rotating cooling roller through a die head to obtain a polyester thick sheet;

[0164] (4.2) After coating the coating liquid on one side of the polyester thick sheet using a slit coating head, it is first stretched 4.5 times in the transverse direction and 4 times in the longitudinal direction in a drying oven at 180°C, and then heat-set at 245°C to obtain a polyester film with excellent optical and mechanical properties.

[0165] The polyester film with excellent optical and mechanical properties finally obtained is composed of a coating from top to bottom, an upper surface layer (made of film-grade slices), a core layer (made of a mixture of large-scale light slices and PEI) and a lower surface layer (made of film-grade slices); the thickness of the coating is 60nm, and the roughness Ra is 10nm; the thickness of the upper surface layer and the lower surface layer are both 0.6μm; the thickness of the core layer is 4μm; the polyester film with excellent optical and mechanical properties has a longitudinal tensile strength of 280MPa, a transverse tensile strength of 360MPa, a longitudinal elastic modulus of 4.6GPa, a transverse elastic modulus of 6.8GPa, a haze of 0.7%, and a transmittance of 93%.

[0166] Example 4

[0167] A process for preparing a polyester film having excellent optical and mechanical properties, the specific steps are as follows:

[0168] (1) Preparation of raw materials;

[0169] (NaPO3)6;

[0170] A mixed solution of deionized water and isopropyl alcohol;

[0171] PS microspheres: manufacturer is Zhongke Leiming (Beijing) Technology Co., Ltd., item number is PS000050, diameter is 50nm;

[0172] Ammonia water: mass concentration is 15%, the solvent is water;

[0173] Tetraethyl orthosilicate;

[0174] water;

[0175] Dilute hydrochloric acid: mass concentration is 25%, the solvent is water;

[0176] Water-based polyester: manufacturer is Toyobo Co., Ltd., model number is MD1200;

[0177] Curing agent: water-based closed curing agent, the manufacturer is Anhui Anda Huatai New Materials Co., Ltd., model A05;

[0178] Wetting agent: manufacturer is Evonik Industries, model is surfynol 104E;

[0179] Raw material slice a and raw material slice b: both are film-grade slices (manufacturer: Kanghui New Material Technology Co., Ltd., model: KH2650A);

[0180] Raw material slice c: a mixture of Dayouguang slice (manufacturer: Sinopec Yizheng Chemical Fiber Co., Ltd., product number: FG604) and PEI (manufacturer: Saudi Basic Industries Corporation, brand: PEI 2110), wherein the mass content of PEI is 6%;

[0181] (2) Preparation of surface H-rich + PS / SiO2 microspheres;

[0182] (2.1) (NaPO3)6 was added to a mixed solution of deionized water and isopropanol, stirred at 600 rpm for 11 minutes, and then PS microspheres were added and stirred at 8500 rpm for 21 minutes to prepare a slurry. The slurry was passed through a sand mill four times;

[0183] (2.2) stirring the slurry at 60°C and 210 rpm for 26 min, during which aqueous ammonia was added dropwise to adjust the pH value to 9.2;

[0184] (2.3) stirring the slurry at 60°C and 210 rpm for 56 min, during which ethyl orthosilicate was added dropwise thereto;

[0185] (2.4) The slurry was stirred at 90°C and 210 rpm for 185 min, then cooled, washed, filtered, and dried to obtain a surface-rich NH4 + PS / SiO2 microspheres;

[0186] (2.5) enrich the surface with NH4 + PS / SiO2 microspheres were dispersed in water to obtain a dispersion with a solid content of 16%. The dispersion was stirred at 210 rpm for 52 min. During this process, dilute hydrochloric acid was added dropwise to adjust the pH value to 4.5. The dispersion was washed, filtered and dried to obtain a shell (i.e., SiO2) with a thickness of 20 nm and a density of 1 g / m 3 The surface is rich in H + PS / SiO2 microspheres;

[0187] Wherein, in steps (2.1) to (2.3), the mass ratio of isopropanol, deionized water, PS microspheres, (NaPO3)6, and tetraethyl orthosilicate is 25:55:17:0.7:4.5;

[0188] (3) preparing a coating solution;

[0189] The contents of the components in the coating solution are as follows: 16 parts of water-based polyester, 16 parts of surface-rich H + 4 parts of PS / SiO2 microspheres, 0.6 parts of curing agent, 0.03 parts of wetting agent, and 135 parts of water;

[0190] (4) Preparation of polyester films with excellent optical and mechanical properties;

[0191] (4.1) First, raw material slice a, raw material slice b and raw material slice c are crystallized and dried at 150-180°C, and then sent to a corresponding extrusion system for melt extrusion to obtain a melt, the melt extrusion temperature is 260-285°C, and then the melt is cooled on a rotating cooling roller through a die head to obtain a polyester thick sheet;

[0192] (4.2) After coating the coating liquid on both sides of the polyester thick sheet using a slit coating head, it is first stretched 3.7 times in the transverse direction and 3.2 times in the longitudinal direction in a drying oven at 120°C, and then heat-set at 230°C to obtain a polyester film with excellent optical and mechanical properties.

[0193] The polyester film with excellent optical and mechanical properties finally obtained is composed of an upper coating layer, an upper surface layer (made of film-grade slices), a core layer (made of a mixture of light-emitting slices and PEI), a lower surface layer (made of film-grade slices) and a lower coating layer from top to bottom; the thickness of the upper coating layer and the lower coating layer are both 45nm, and the roughness Ra is 7nm; the thickness of the upper surface layer is 0.5μm; the thickness of the core layer is 4.5μm; the thickness of the lower surface layer is 0.75μm; the polyester film with excellent optical and mechanical properties has a longitudinal tensile strength of 260MPa, a transverse tensile strength of 350MPa, a longitudinal elastic modulus of 4.5GPa, a transverse elastic modulus of 6.8GPa, a haze of 0.7%, and a transmittance of 93%.

[0194] Example 5

[0195] A process for preparing a polyester film having excellent optical and mechanical properties, the specific steps are as follows:

[0196] (1) Preparation of raw materials;

[0197] (NaPO3)6;

[0198] A mixed solution of deionized water and isopropyl alcohol;

[0199] PS microspheres: The manufacturer is Suzhou Zhiyi Microsphere Technology Co., Ltd., the model is KBsphere® 0.06PS, and the diameter is 60nm;

[0200] Ammonia water: mass concentration is 20%, the solvent is water;

[0201] Tetraethyl orthosilicate;

[0202] water;

[0203] Dilute hydrochloric acid: mass concentration is 30%, the solvent is water;

[0204] Water-based polyester: manufacturer is Toyobo Co., Ltd., model number is MD1200;

[0205] Curing agent: water-based closed curing agent, the manufacturer is Anhui Anda Huatai New Materials Co., Ltd., model A05;

[0206] Wetting agent: manufacturer is Evonik Industries, model is surfynol 104E;

[0207] Raw material slice a and raw material slice b: both are membrane grade slices (manufacturer is Sinopec Yizheng Chemical Fiber Co., Ltd., model is FG600);

[0208] Raw material slice c: a mixture of Dayouguang slice (manufacturer is Hefei Lucky Technology Industry Co., Ltd., product name is LK-200) and PEI (manufacturer is Saudi Basic Industries Corporation, brand name is PEI 2110), wherein the mass content of PEI is 7%;

[0209] (2) Preparation of surface H-rich + PS / SiO2 microspheres;

[0210] (2.1) Add (NaPO3)6 to a mixed solution of deionized water and isopropanol, stir at 700 rpm for 12 minutes, add PS microspheres, stir at 9000 rpm for 22 minutes to prepare a slurry, and pass the slurry through a sand mill three times;

[0211] (2.2) stirring the slurry at 59.5°C and 220 rpm for 27 min, during which aqueous ammonia was added dropwise to adjust the pH value to 9.4;

[0212] (2.3) stirring the slurry at 59.5°C and 220 rpm for 57 min, during which tetraethyl orthosilicate was added dropwise;

[0213] (2.4) The slurry was stirred at 89.5°C and 220 rpm for 190 min, then cooled, washed, filtered, and dried to obtain a surface-rich NH4 + PS / SiO2 microspheres;

[0214] (2.5) enrich the surface with NH4 + PS / SiO2 microspheres were dispersed in water to obtain a dispersion with a solid content of 17%. The dispersion was stirred at 220 rpm for 54 min. During this process, dilute hydrochloric acid was added dropwise to adjust the pH value to 4. The dispersion was washed, filtered and dried to obtain a shell layer (i.e., SiO2) with a thickness of 28 nm and a density of 1.05 g / m 3 The surface is rich in H + PS / SiO2 microspheres;

[0215] Wherein, in steps (2.1) to (2.3), the mass ratio of isopropanol, deionized water, PS microspheres, (NaPO3)6, and tetraethyl orthosilicate is 20:50:15:0.5:4;

[0216] (3) preparing a coating solution;

[0217] The contents of the components in the coating solution are as follows: 17 parts of water-based polyester, 17 parts of surface-rich H + 3 parts of PS / SiO2 microspheres, 0.7 parts of curing agent, 0.02 parts of wetting agent, and 140 parts of water;

[0218] (4) Preparation of polyester films with excellent optical and mechanical properties;

[0219] (4.1) First, raw material slice a, raw material slice b and raw material slice c are crystallized and dried at 150-180°C, and then sent to a corresponding extrusion system for melt extrusion to obtain a melt, the melt extrusion temperature is 260-285°C, and then the melt is cooled on a rotating cooling roller through a die head to obtain a polyester thick sheet;

[0220] (4.2) After coating the coating liquid on both sides of the polyester thick sheet using a slit coating head, it is first stretched 3.9 times in the transverse direction and 3.4 times in the longitudinal direction in a drying oven at 140°C, and then heat-set at 235°C to obtain a polyester film with excellent optical and mechanical properties.

[0221] The polyester film with excellent optical and mechanical properties finally obtained is composed of an upper coating layer, an upper surface layer (made of film-grade slices), a core layer (made of a mixture of large-light slices and PEI), a lower surface layer (made of film-grade slices) and a lower coating layer from top to bottom; the thickness of the upper coating layer and the lower coating layer are both 50nm, and the roughness Ra is 8nm; the thickness of the upper surface layer is 0.7μm; the thickness of the core layer is 4μm; the thickness of the lower surface layer is 0.55μm; the polyester film with excellent optical and mechanical properties has a longitudinal tensile strength of 250MPa, a transverse tensile strength of 360MPa, a longitudinal elastic modulus of 4.6GPa, a transverse elastic modulus of 6.7GPa, a haze of 0.6%, and a transmittance of 94%.

[0222] Example 6

[0223] A process for preparing a polyester film having excellent optical and mechanical properties, the specific steps are as follows:

[0224] (1) Preparation of raw materials;

[0225] (NaPO3)6;

[0226] A mixed solution of deionized water and isopropyl alcohol;

[0227] PS microspheres: manufacturer is Zhongke Leiming (Beijing) Technology Co., Ltd., item number is PS000050, diameter is 50nm;

[0228] Ammonia water: mass concentration is 25%, the solvent is water;

[0229] Tetraethyl orthosilicate;

[0230] water;

[0231] Dilute hydrochloric acid: mass concentration is 32%, the solvent is water;

[0232] Water-based polyester: manufacturer is Toyobo Co., Ltd., model number is MD1200;

[0233] Curing agent: water-based closed curing agent, the manufacturer is Anhui Anda Huatai New Materials Co., Ltd., model A05;

[0234] Wetting agent: manufacturer is Evonik Industries, model is surfynol 104E;

[0235] Raw material slice a and raw material slice b: both are film-grade slices (manufacturer: Kanghui New Material Technology Co., Ltd., model: KH2650A);

[0236] Raw material slice c: a mixture of Dayouguang slice (manufacturer: Sinopec Yizheng Chemical Fiber Co., Ltd., product number: FG604) and PEI (manufacturer: Saudi Basic Industries Corporation, brand: PEI 2110), wherein the mass content of PEI is 8%;

[0237] (2) Preparation of surface H-rich + PS / SiO2 microspheres;

[0238] (2.1) (NaPO3)6 was added to a mixed solution of deionized water and isopropanol, stirred at 550 rpm for 14 minutes, and then PS microspheres were added. The mixture was stirred at 9500 rpm for 23 minutes to prepare a slurry, and the slurry was passed through a sand mill for 5 times;

[0239] (2.2) stirring the slurry at 230 rpm and 60 °C for 28 min, during which time aqueous ammonia was added dropwise to adjust the pH value to 9.6;

[0240] (2.3) stirring the slurry at 60.5°C and 230 rpm for 58 min, during which tetraethyl orthosilicate was added dropwise;

[0241] (2.4) The slurry was stirred at 90.5°C and 230 rpm for 195 min, then cooled, washed, filtered, and dried to obtain a surface-rich NH4 + PS / SiO2 microspheres;

[0242] (2.5) enrich the surface with NH4 + PS / SiO2 microspheres were dispersed in water to obtain a dispersion with a solid content of 18%, which was stirred at 230 rpm for 56 min. During this process, dilute hydrochloric acid was added dropwise to adjust the pH value to 5. The microspheres were washed, filtered and dried to obtain a shell layer (i.e., SiO2) with a thickness of 26 nm and a density of 1 g / m 3 The surface is rich in H + PS / SiO2 microspheres;

[0243] Wherein, in steps (2.1) to (2.3), the mass ratio of isopropanol, deionized water, PS microspheres, (NaPO3)6, and tetraethyl orthosilicate is 30:60:20:1:5;

[0244] (3) preparing a coating solution;

[0245] The contents of the components in the coating solution are as follows: 18 parts of water-based polyester, 18 parts of surface-rich H + 5 parts of PS / SiO2 microspheres, 0.8 parts of curing agent, 0.04 parts of wetting agent, and 145 parts of water;

[0246] (4) Preparation of polyester films with excellent optical and mechanical properties;

[0247] (4.1) First, raw material slice a, raw material slice b and raw material slice c are crystallized and dried at 150-180°C, and then sent to a corresponding extrusion system for melt extrusion to obtain a melt, the melt extrusion temperature is 260-285°C, and then the melt is cooled on a rotating cooling roller through a die head to obtain a polyester thick sheet;

[0248] (4.2) After coating the coating liquid on both sides of the polyester thick sheet with a slit coating head, it is first stretched 4.2 times in the transverse direction and 3.6 times in the longitudinal direction in a drying oven at 160°C, and then heat-set at 240°C to obtain a polyester film with excellent optical and mechanical properties.

[0249] The polyester film with excellent optical and mechanical properties finally obtained is composed of an upper coating layer, an upper surface layer (made of film-grade slices), a core layer (made of a mixture of optical slices and PEI), a lower surface layer (made of film-grade slices) and a lower coating layer from top to bottom; the thickness of the upper coating layer and the lower coating layer is 55nm, and the roughness Ra is 9nm; the thickness of the upper surface layer and the lower surface layer is 0.6μm; the thickness of the core layer is 3.5μm; the polyester film with excellent optical and mechanical properties has a longitudinal tensile strength of 280MPa, a transverse tensile strength of 340MPa, a longitudinal elastic modulus of 4.4GPa, a transverse elastic modulus of 6.9GPa, a haze of 0.7%, and a transmittance of 93%.

Claims

1. A process for preparing a polyester film having excellent optical and mechanical properties, characterized in that: After coating the surface of the polyester thick sheet with the coating liquid, biaxial stretching and heat setting are performed in sequence to obtain a polyester film with excellent optical and mechanical properties; The coating adopts a slit coating head; The coating liquid is composed of water-based polyester, surface rich in H + PS / SiO2 microspheres, curing agent, wetting agent and water; the surface is rich in H + The density of PS / SiO2 microspheres is 1-1.05g / m 3 ; The content of each component in the coating solution is as follows: 15-20 parts of water-based polyester, surface rich in H + 3-5 parts of PS / SiO2 microspheres, 0.5-1 parts of curing agent, 0.02-0.04 parts of wetting agent, 130-150 parts of water; The surface is rich in H + The preparation process of PS / SiO2 microspheres is as follows: (1) Add (NaPO3)6 to a mixed solution of deionized water and isopropanol, stir at a speed of 500-800 rpm for 10-15 minutes, add PS microspheres, stir at a speed of 8000-1000 rpm for 20-25 minutes to prepare a slurry, and pass the slurry through a sand mill 3-5 times; (2) Stirring the slurry at 60±0.5°C and 200-250 rpm for 25-30 min, during which time 10-35% ammonia water was added dropwise to adjust the pH value to 9-10; (3) stirring the slurry at 60±0.5°C and 200-250 rpm for 55-60 min, during which ethyl orthosilicate was added dropwise; In steps (1) to (3), the mass ratio of isopropanol, deionized water, PS microspheres, (NaPO3)6, and tetraethyl orthosilicate is 20-30:50-60:15-20:0.5-1:4-5; (4) Stir the slurry at 90±0.5°C and 200-250 rpm for 180-200 min, then cool, wash, filter and dry to obtain a NH4-rich + PS / SiO2 microspheres; (5) Enrich the surface with NH4 + The PS / SiO2 microspheres were dispersed in water to obtain a dispersion with a solid content of 15-20%, and stirred at a speed of 200-250 rpm for 50-60 min. During this process, dilute hydrochloric acid with a mass concentration of 20-36% was added dropwise to adjust the pH value to 4-5, washed, filtered, and dried to obtain a dispersion rich in H + PS / SiO2 microspheres; The curing agent reacts during the heat setting process.

2. The process for preparing a polyester film having excellent optical and mechanical properties according to claim 1, characterized in that: The surface is rich in H + In the PS / SiO2 microspheres, the diameter of the PS microspheres is 50-60nm and the thickness of the shell is 20-30nm.

3. The process for preparing a polyester film having excellent optical and mechanical properties according to claim 1, characterized in that: The preparation process of the polyester thick sheet is as follows: first, the raw material slices are crystallized and dried at 150-180°C, and then sent to the corresponding extrusion system for melt extrusion to obtain a melt, the melt extrusion temperature is 260-285°C, and then the melt is cooled on a rotating cooling roller through a die head to obtain a polyester thick sheet.

4. The process for preparing a polyester film having excellent optical and mechanical properties according to claim 1, characterized in that: Biaxial stretching means stretching 3.5-4.5 times transversely and 3-4 times longitudinally in a drying oven at 90-180°C; the heat setting temperature is 220-245°C.

5. A polyester film having excellent optical and mechanical properties, prepared by the process for preparing a polyester film having excellent optical and mechanical properties as claimed in any one of claims 1 to 4, characterized in that: The invention comprises a polyester base film and a coating layer on the surface of the polyester base film.

6. A polyester film having excellent optical and mechanical properties according to claim 5, characterized in that: The coating is located on both sides of the polyester base film, the thickness of a single coating is 40-60 nm, and the roughness Ra of the coating is 6-10 nm.

7. A polyester film having excellent optical and mechanical properties according to claim 5, characterized in that: The polyester base film consists of an upper surface layer, a core layer and a lower surface layer; the raw materials of the upper surface layer and the lower surface layer are both film-grade slices; the raw material of the core layer is a mixture of large-glossy slices and PEI, wherein the mass content of PEI is 5-10%; the thickness of the upper surface layer or the lower surface layer is 0.5-0.75μm, and the thickness of the core layer is 3-4.5μm.

8. The polyester film having excellent optical and mechanical properties according to claim 5, characterized in that: The polyester film with excellent optical and mechanical properties has a longitudinal tensile strength of ≥240MPa, a transverse tensile strength of ≥330MPa, a longitudinal elastic modulus of ≥4.3GPa, a transverse elastic modulus of ≥6.6GPa, a haze of 0.5-0.8%, and a transmittance of 92-95%.