A flame retardant EVA packaging film and preparation method thereof

The flame-retardant EVA encapsulation film that combines new cyclic phosphate ester flame retardants with EVA resin solves the problems of flammability of photovoltaic encapsulation films and toxicity of halogen flame retardants, achieving both efficient flame retardant performance and mechanical properties. Meets green environmental protection standards.

CN118562418BActive Publication Date: 2024-10-11SUZHOU YISHENG OPTICAL MATERIAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411035389.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-11
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Existing photovoltaic encapsulation film materials are flammable and have poor flame retardant properties. They are prone to fires, especially in high-temperature environments. Commonly used halogen flame retardants have problems with toxicity and low-smoke performance, making it difficult to meet green environmental protection standards.

Method used

Using ingredients such as new cyclic phosphate ester flame retardant and silane coupling agent, the flame retardant is prepared through compound reaction under nitrogen protection, and combined with EVA resin, cross-linking agent, antioxidant, etc., and formed into a film through an extruder Prepare a flame-retardant EVA encapsulating film to form a carbon layer to insulate combustion during thermal decomposition.

Benefits of technology

The limiting oxygen index reaches 35-36, the horizontal and vertical combustion test flame retardant grade reaches V-0, and the smoke density is 160-190. The flame retardant performance is significantly better than that of traditional flame retardants, while taking into account the mechanical properties of the film to avoid This eliminates the need to add additional carbon-forming agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118562418B_ABST
    Figure CN118562418B_ABST
Patent Text Reader

Abstract

The present invention provides a flame retardant EVA encapsulation film and a preparation method thereof, comprising the following raw materials: 90-100 parts of EVA resin, 0.5-2 parts of silane coupling agent, 1-2 parts of cross-linking agent, 2-5 parts of flame retardant, 0.5-1 parts of antioxidant, and 0.1-0.5 parts of initiator. The novel cyclic phosphate flame retardant #imgabs0# prepared by the present invention can make the film have excellent flame retardant properties while taking into account mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photovoltaic packaging materials, and particularly relates to a flame-retardant EVA packaging film and a preparation method thereof. Background Art

[0002] As one of the materials of photovoltaic modules, photovoltaic film mainly bonds photovoltaic cells, photovoltaic glass and backplane together, isolates external water vapor while ensuring the light transmission performance of the module, prolongs the life of photovoltaic modules, protects the cells, and packages them into photovoltaic modules that can output direct current. According to the actual application requirements of photovoltaic modules, photovoltaic film should generally have high transparency, high adhesion, good weather resistance, easy storage, good sound insulation, low melting point, easy flow, flame retardancy and other excellent performance characteristics.

[0003] With the substantial development of distributed power generation, more and more photovoltaic modules are used in areas with a large number of residents, such as factories, public buildings, villas, office buildings, etc. The photoelectric conversion of crystalline silicon solar cells will significantly increase the temperature inside the module, which may cause overheating and fire due to mismatch or hot spot effect. The main material of photovoltaic encapsulation film is EVA (ethylene-vinyl acetate copolymer) resin or POE (ethylene-octene copolymer) resin. Both materials have a low oxygen index of less than 20, and are flammable materials. Therefore, the photovoltaic EVA encapsulation film and POE encapsulation film used in the market generally have poor flame retardant properties.

[0004] It is a common practice to change the flammability of the film by adding flame retardants. Halogen flame retardants are the most widely used flame retardants. Although they have high flame retardant efficiency and good effects, they will produce a large amount of black smoke containing toxic gases, which can easily cause poisoning and suffocation. The EU's REACH and RoHS standards restrict halogen flame retardants. Halogen-containing flame retardants are not allowed to be used in the shell and bracket of electronic displays. Therefore, finding non-toxic, low-smoke, green and environmentally friendly high-efficiency flame retardants is the current research focus.

[0005] CN1401721B discloses a polyolefin hot melt adhesive and a composite structural film using the hot melt adhesive, wherein hydroxide is added. CN102936483A discloses a single-component silicone sealant for solar photovoltaic modules and a preparation method thereof, wherein silicon-based flame retardants, expanded graphite, and phosphorus-nitrogen-based small molecule additives are added. However, when these additives are added to the cross-linked modified adhesive film, due to the poor compatibility of the small molecule additives and EVA, aging defects occur between the phase interfaces during long-term ultraviolet and wet heat aging, and the flame retardant effect is not good. CN113563829 B relates to a flame-retardant EVA adhesive film, a preparation method and use thereof, but it requires the use of a certain amount of carbon-forming agent, and the flame retardant effect needs to be improved.

[0006] Therefore, there is an urgent need to develop an encapsulation film with excellent flame retardant properties and mechanical properties. Summary of the invention

[0007] The object of the present invention is to provide a flame retardant EVA encapsulation film and a preparation method thereof. In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] A flame retardant EVA packaging film, characterized in that it comprises the following raw materials in parts by weight:

[0009] EVA resin 50-100 parts

[0010] Silane coupling agent 0.5-10 parts

[0011] 1~10 parts of cross-linking agent

[0012] Flame retardant 1-10 parts

[0013] 0.5-5 parts of antioxidant

[0014] Initiator 0.1~5 parts

[0015] The structural formula of the flame retardant is:

[0016]

[0017] In some embodiments, the flame retardant EVA encapsulation film includes the following raw materials:

[0018] EVA resin 90~100 parts

[0019] Silane coupling agent 0.5-2 parts

[0020] 1-2 parts of cross-linking agent

[0021] Flame retardant 2-5 parts

[0022] 0.5-1 part antioxidant

[0023] Initiator 0.1~0.5 parts

[0024] In some embodiments, Prepared by the following method:

[0025]

[0026] Under nitrogen protection, compound I and compound II react in an alkaline catalyst to obtain the flame retardant of the present invention.

[0027] In some embodiments, the silane coupling agent is selected from one or more of vinyl trimethoxysilane, dimethylethoxyvinyl silane, vinyl tri-tert-butoxysilane, vinyl triethoxysilane, vinyl triacetoxysilane and vinyl triisopropoxysilane.

[0028] In some embodiments, the auxiliary crosslinking agent is selected from one or more of tris(2-hydroxyethyl)-isocyanuric acid triacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, and ethoxylated trimethylolpropane triacrylate;

[0029] In some embodiments, the initiator is one or more of 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butylperoxycarbonate-2-ethylhexyl ester, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and tert-butylperoxycarbonate isopropyl ester;

[0030] In some embodiments, the antioxidant is selected from the antioxidant KY-1010 or the antioxidant DLTP.

[0031] In some embodiments, the VA content of the EVA resin is 20-30 wt %, preferably 30 wt %.

[0032] On the other hand, the present invention also provides a method for preparing a flame retardant EVA encapsulation film, comprising the following steps:

[0033] 1) Stir and mix EVA resin, silane coupling agent, cross-linking agent, flame retardant, antioxidant and initiator evenly;

[0034] 2) The mixed material is melt-extruded and formed into a film by an extruder to obtain the flame-retardant EVA packaging film.

[0035] In some embodiments, the mixing method in step 1) is stirring at a rotation speed of 10 to 100 r / min for 1 to 5 hours.

[0036] In some embodiments, the temperature of the melt extrusion in step 2) is 50-100°C, preferably 70-100°C.

[0037] In some embodiments, the extruder in step 2) is a single screw extruder.

[0038] In some embodiments, the extruder in step 2) is a single screw extruder.

[0039] In some embodiments, the method for preparing the flame retardant EVA encapsulation film comprises the following steps:

[0040] According to the above weight ratio, EVA resin, silane coupling agent, co-crosslinking agent, flame retardant, antioxidant and initiator were stirred and mixed at a speed of 50 r / min for 1.0 h to mix evenly;

[0041] The mixed material is added into a single screw extruder, extruded at 70-100° C. to form a film, and then subjected to embossing, cooling, pulling and winding processes to obtain a flame retardant EVA film.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] 1) The novel cyclic phosphate flame retardant prepared by the present invention On the one hand, PO· can be quickly formed when thermally decomposed, effectively inhibiting H· and OH· in the combustion system; on the other hand, when the film is thermally decomposed, the pyrolysis products of the flame retardant dehydrate it, thereby forming a carbon layer on the surface, which wraps around the surface of the EVA and isolates other combustion factors, thereby achieving the purpose of preventing combustion without the need to add additional carbon-forming agents.

[0044] 2) The EVA film provided by the present invention has excellent flame retardant properties, with a limiting oxygen index of 35-36, a flame retardant grade of V-0 in horizontal and vertical combustion tests, and a smoke density of 160-190. The flame retardant properties are significantly better than those of the common flame retardants in the prior art, and the mechanical properties can be taken into account at the same time. DETAILED DESCRIPTION

[0045] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] Preparation Example 1: Preparation of flame retardant

[0047]

[0048] Under nitrogen protection, compound I (14.0 g, 0.1 mol) and compound II (46.8 g, 0.25 mol) were added to xylene (200 mL) and mixed evenly, followed by addition of dibutyltin dilaurate catalyst (0.03 mol), and heated to reflux and stirred for 10 h. After the reaction, the mixture was filtered, and the filtrate was washed with deionized water 3 times (100 mLx3). The organic layer was dried over anhydrous sodium sulfate and concentrated under reduced pressure to obtain a crude product, which was separated and purified by column chromatography to obtain 33.5 g, with a yield of 80.1% and an HPLC purity of 99.1%.

[0049] LC-MS (ESI): [M+H] +=419.2.

[0050] 1 H-NMR (500 MHz, CDCl3): δ (ppm): 8.71 -8.60 (m,4H), 7.88 -7.79 (m,4H), 4.52-4.44 (m,6H), 3.81-3.75 (m,3H).

[0051] Example 1

[0052] A flame retardant EVA packaging film, characterized in that it comprises the following raw materials in parts by weight:

[0053] EVA resin (VA content 30wt%) 100 parts

[0054] 1 part of vinyltrimethoxysilane

[0055] 1 part of trimethylolpropane triacrylate

[0056] Flame retardant 3 parts

[0057] Antioxidant KY-1010 0.5 parts

[0058] 0.2 parts of 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane

[0059] The structural formula of the flame retardant is:

[0060]

[0061] The method for preparing the flame retardant EVA encapsulation film comprises the following steps:

[0062] According to the above weight ratio, EVA resin, silane coupling agent, co-crosslinking agent, flame retardant, antioxidant and initiator were stirred and mixed at a speed of 50 r / min for 1.0 h to mix evenly;

[0063] The mixed material is added into a single screw extruder, extruded at 70-100° C. to form a film, and then subjected to embossing, cooling, pulling and winding processes to obtain a flame retardant EVA film.

[0064] Example 2

[0065] A flame retardant EVA packaging film, characterized in that it comprises the following raw materials in parts by weight:

[0066] EVA resin (VA content 30wt%) 95 parts

[0067] 1.5 parts of dimethylethoxyvinylsilane

[0068] 2 parts of pentaerythritol triacrylate

[0069] Flame retardant 5 parts

[0070] 1 part of antioxidant DLTP

[0071] 0.5 parts of tert-butyl peroxycarbonate-2-ethylhexyl ester

[0072] The structural formula of the flame retardant is:

[0073]

[0074] The method for preparing the flame retardant EVA encapsulation film comprises the following steps:

[0075] According to the above weight ratio, EVA resin, silane coupling agent, co-crosslinking agent, flame retardant, antioxidant and initiator were stirred and mixed at a speed of 50 r / min for 1.0 h to mix evenly;

[0076] The mixed material is added into a single screw extruder, extruded at 70-100° C. to form a film, and then subjected to embossing, cooling, pulling and winding processes to obtain a flame retardant EVA film.

[0077] Example 3

[0078] A flame retardant EVA packaging film, characterized in that it comprises the following raw materials in parts by weight:

[0079] EVA resin (VA content 30wt%) 90 parts

[0080] 1.0 part of vinyl tri-tert-butoxysilane

[0081] 2 parts of tris(2-hydroxyethyl)-isocyanurate triacrylate

[0082] Flame retardant 4 parts

[0083] 1 part of antioxidant DLTP

[0084] 0.2 parts of tert-butyl peroxyisopropyl carbonate

[0085] The structural formula of the flame retardant is:

[0086]

[0087] The method for preparing the flame retardant EVA encapsulation film comprises the following steps:

[0088] According to the above weight ratio, EVA resin, silane coupling agent, co-crosslinking agent, flame retardant, antioxidant and initiator were stirred and mixed at a speed of 50 r / min for 1.0 h to mix evenly;

[0089] The mixed material is added into a single screw extruder, extruded at 70-100° C. to form a film, and then subjected to embossing, cooling, pulling and winding processes to obtain a flame retardant EVA film.

[0090] Comparative Example 1 Based on Example 1, the flame retardant Replaced with common flame retardant phenoxy cyclophosphazene

[0091] A flame retardant EVA packaging film, characterized in that it comprises the following raw materials in parts by weight:

[0092] EVA resin (VA content 30wt%) 100 parts

[0093] 1 part of vinyltrimethoxysilane

[0094] 1 part of trimethylolpropane triacrylate

[0095] 3 parts of phenoxy cyclophosphazene

[0096] Antioxidant KY-1010 0.5 parts

[0097] 0.2 parts of 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane

[0098] The method for preparing the flame retardant EVA encapsulation film comprises the following steps:

[0099] According to the above weight ratio, EVA resin, silane coupling agent, co-crosslinking agent, flame retardant, antioxidant and initiator were stirred and mixed at a speed of 50 r / min for 1.0 h to mix evenly;

[0100] The mixed material is added into a single screw extruder, extruded at 70-100° C. to form a film, and then subjected to embossing, cooling, pulling and winding processes to obtain a flame retardant EVA film.

[0101] Comparative Example 2 Based on Example 1, the flame retardant Replaced with common flame retardant tris(N,N-tetramethylene)phosphoramide

[0102] A flame retardant EVA packaging film, characterized in that it comprises the following raw materials in parts by weight:

[0103] EVA resin (VA content 30wt%) 100 parts

[0104] 1 part of vinyltrimethoxysilane

[0105] 1 part of trimethylolpropane triacrylate

[0106] 3 parts of tris(N,N-tetramethylene)phosphoramide

[0107] Antioxidant KY-1010 0.5 parts

[0108] 0.2 parts of 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane

[0109] The method for preparing the flame retardant EVA encapsulation film comprises the following steps:

[0110] According to the above weight ratio, EVA resin, silane coupling agent, co-crosslinking agent, flame retardant, antioxidant and initiator were stirred and mixed at a speed of 50 r / min for 1.0 h to mix evenly;

[0111] The mixed material is added into a single screw extruder, extruded at 70-100° C. to form a film, and then subjected to embossing, cooling, pulling and winding processes to obtain a flame retardant EVA film.

[0112] Performance Testing

[0113] The EVA films provided in the above Examples 1 to 3 and Comparative Examples 1 to 2 were sampled according to the method specified in the performance test standard, and their tensile strength, elongation at break, limiting oxygen index, flame retardancy grade, and smoke density were tested.

[0114] The test standards are as follows:

[0115] The thickness of the EVA film is 0.5mm and the size is 300mm x 150mm.

[0116] Tensile strength and elongation at break: GB / T13022-1991; maximum displacement 1000mm, tensile speed 100mm / min.

[0117] Limiting Oxygen Index (LOI): GB / T2406-2009 standard is adopted and tested by JF-3 oxygen index tester.

[0118] Flame retardant grade: According to ANSL-UL94-2009 standard, tested with CZF-5 vertical combustion instrument.

[0119] Smoke density: According to ASTM E662-2017 standard, flameless method.

[0120] The results are shown in Table 1.

[0121] Table 1 Film performance parameters

[0122]

[0123] It can be seen from the data in Table 1 that the adhesive film prepared by the present invention has excellent mechanical properties and flame retardant properties.

[0124] It can be seen from Example 1 and Comparative Example 1 and Comparative Example 2 that the novel cyclic phosphate flame retardant prepared by the present invention On the one hand, PO· can be quickly formed when thermally decomposed, effectively inhibiting H· and OH· in the combustion system; on the other hand, when the film is thermally decomposed, the flame retardant pyrolysis product dehydrates it, thereby forming a carbon layer on the surface, which is wrapped on the surface of EVA, isolating other combustion factors, and achieving the purpose of preventing combustion without the need to add additional carbon forming agents. The EVA film provided by the present invention has a limiting oxygen index of 35-36, a flame retardant grade of V-0 in the horizontal and vertical combustion test, and a smoke density of 160-190. The flame retardant performance is significantly better than the common flame retardants in the prior art, and the mechanical properties can be taken into account at the same time.

[0125] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A flame retardant EVA encapsulation film, It is characterized in that By weight, it includes the following raw materials: EVA resin 50-100 parts Silane coupling agent 0.5-10 parts 1~10 parts of cross-linking agent Flame retardant 1-10 parts 0.5-5 parts of antioxidant Initiator 0.1~5 parts The structural formula of the flame retardant is: 。 2. The flame retardant EVA encapsulation film according to claim 1, It is characterized in that By weight, it includes the following raw materials: EVA resin 90~100 parts Silane coupling agent 0.5-2 parts 1-2 parts of cross-linking agent Flame retardant 2-5 parts 0.5-1 part antioxidant Initiator 0.1~0.5 parts The structural formula of the flame retardant is: 。 3. The flame retardant EVA encapsulation film according to claim 1 or 2, Features: The silane coupling agent is selected from one or more of vinyl trimethoxysilane, dimethylethoxy vinyl silane, vinyl tri-tert-butoxy silane, vinyl triethoxy silane, vinyl triacetoxy silane and vinyl triisopropoxy silane.

4. The flame retardant EVA encapsulation film according to claim 1 or 2, Features: The auxiliary crosslinking agent is selected from one or more of tris(2-hydroxyethyl)-isocyanuric acid triacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate and ethoxylated trimethylolpropane triacrylate.

5. The flame retardant EVA encapsulation film according to claim 1 or 2, Features: The initiator is one or more of 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane, tert-butylperoxycarbonate-2-ethylhexyl ester, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and tert-butylperoxycarbonate isopropyl ester; The antioxidant is selected from antioxidant KY-1010 or antioxidant DLTP.

6. The flame retardant EVA encapsulation film according to claim 1 or 2, Features: The VA content of the EVA resin is 20-30 wt %.

7. A method for preparing the flame-retardant EVA packaging film according to any one of claims 1 to 6, It is characterized in that The preparation method comprises the following steps: 1) Stir and mix EVA resin, silane coupling agent, cross-linking agent, flame retardant, antioxidant and initiator evenly; 2) The mixed material is melt-extruded and formed into a film by an extruder to obtain the flame-retardant EVA packaging film.

8. The method according to claim 7, It is characterized in that The mixing method in step 1) is stirring at a speed of 10 to 100 r / min for 1 to 5 hours.

9. The method according to claim 7, It is characterized in that Step 2) The temperature of the melt extrusion is 50-100°C.

10. The method according to claim 7, It is characterized in that Step 2) The extruder is a single screw extruder.

Citation Information

Patent Citations

  • Sealant for single-component organosilicon solar photovoltaic modules and preparation method thereof

    CN102936483A

  • A flame-retardant EVA film, its preparation method and applications

    CN113563829B

  • Hot-melt polyolefin adhesive and composite structure film using same

    CN1401721A

  • Fire retardant hydroxymethyl phosphonyl hybrid ring-shaped methylphosphonate compound and preparing method thereof

    CN104926873A

  • Phosphorus-containing acrylate flame retardant, flame retardant EVA adhesive film and preparation methods of phosphorus-containing acrylate flame retardant and flame retardant EVA adhesive film

    CN107603510A