A wear-resistant and corrosion-resistant impeller and its preparation method
By spraying a gradient composite coating of Ni, Cr, WC and Re onto a stainless steel impeller substrate and then calcining it under vacuum to form Fe-based Cr3C2, Ni-Re and Ni-based WC layers, the problem of insufficient wear resistance and corrosion resistance of the impeller was solved, and the preparation of impellers with high wear resistance and high corrosion resistance was achieved.
Patent Information
- Application Number
- CN202410656157.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-05-24
AI Technical Summary
Existing technologies have poor wear resistance and corrosion resistance of impellers, making it difficult to meet the requirements of use in harsh environments. In particular, in seawater pumps, there is a sudden change in material and performance at the interface between the Ni-based WC coating and the stainless steel impeller substrate, resulting in poor bonding strength. Furthermore, pores and cracks are easily generated during the laser cladding process.
Wear-resistant and corrosion-resistant powders made from a mixture of Ni, Cr, WC, and Re are used to form an intermediate coating on the surface of a stainless steel impeller substrate using a supersonic flame spraying process. The coating is then calcined in a vacuum environment to form a gradient composite coating consisting of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside out, ensuring metallurgical bonding between the layers.
A wear-resistant and corrosion-resistant impeller with a microhardness ≥1300HV1.0, a friction and wear coefficient ≤0.55, and a corrosion resistance time ≥648h was prepared, which solved the problem of wear resistance and corrosion resistance of the impeller in harsh environments and improved the bonding strength and performance stability of the impeller.
Smart Images

Figure CN118563320B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of seawater pumps, and more particularly to a wear-resistant and corrosion-resistant impeller and its manufacturing method. Background Technology
[0002] A seawater pump is a specialized device for extracting seawater. It uses the centrifugal force generated by the rotation of an impeller to propel liquid from the center to the edge of the impeller, simultaneously generating pressure to deliver the liquid to the desired location for seawater transport and circulation. It is widely used in marine engineering, offshore oil fields, and marine fisheries. Due to the harsh working environment of seawater pumps, higher performance requirements are placed on them. The impeller plays a crucial role in the pump's performance, thus requiring higher performance specifications: firstly, it must possess excellent corrosion resistance to prevent strong corrosion from corrosive components in seawater, which would accelerate wear and damage, leading to failure; secondly, it must have good wear resistance to prevent surface damage after prolonged operation, which could render it inoperable.
[0003] To achieve high wear resistance and corrosion resistance in impellers, current technologies typically involve laser-coating a Ni-based WC coating onto the stainless steel impeller substrate to impart these properties. However, the performance of the Ni-based WC coating itself limits the extent to which this improves the impeller's wear and corrosion resistance. Furthermore, the significant difference in physicochemical properties between the Ni-based WC coating and the stainless steel impeller substrate leads to poor compatibility and abrupt material and property changes at the interface, resulting in substantial stress concentration. In addition, the rapid heating and cooling processes during laser cladding can also cause localized stress concentration, weakening the bond between the Ni-based WC coating and the impeller substrate, and making the Ni-based WC gradient composite coating prone to cracking. During use, the Ni-based WC coating can easily detach, leading to rapid wear or corrosion of the impeller. In short, laser-coating a Ni-based WC coating onto a stainless steel impeller substrate cannot guarantee the impeller's wear and corrosion resistance.
[0004] To overcome the aforementioned shortcomings, the industry has developed a laser cladding process for Ni-based WC gradient composite coatings on stainless steel impeller substrates. This gradient composite coating creates a continuous transition between different layers, alleviating stress concentration and promoting a more rational stress distribution. This results in a coating with high wear and corrosion resistance on the stainless steel impeller substrate, giving the impeller better wear and corrosion resistance. However, due to the abrupt change in material properties at the interface between the Ni-based WC gradient composite coating and the stainless steel impeller substrate, even with a gradient composite coating, defects such as localized stress concentration and poor bonding strength still exist at the interface. Furthermore, during the laser cladding process, the CO and CO2 gases generated from the reaction of carbon (C) produced by the burning of the WC raw material with oxygen in the air cannot escape in time, leading to porosity on the surface of the Ni-based WC gradient composite coating. This becomes a new hidden danger for corrosion of the stainless steel impeller substrate, increasing the probability of blistering and peeling of the Ni-based WC gradient composite coating, thus limiting the improvement in its wear and corrosion resistance. Although laser cladding of Ni-based WC gradient composite coatings on the impeller substrate surface can improve the impeller's wear resistance and corrosion resistance, due to the superposition of the above-mentioned factors, it is still difficult to meet the requirements of applications with high wear resistance and corrosion resistance. Summary of the Invention
[0005] One of the objectives of this invention is to provide a method for preparing a wear-resistant and corrosion-resistant impeller. The method is simple and easy to operate, and the resulting impeller has both excellent wear resistance and corrosion resistance. This solves the technical problem that the existing impellers have poor wear resistance and corrosion resistance, making it difficult to meet the needs of practical use.
[0006] The second objective of this invention is to provide a wear-resistant and corrosion-resistant impeller with a microhardness ≥1300 HV. 1.0 With a friction and wear coefficient ≤0.55 and a corrosion resistance time ≥648h, it exhibits high wear resistance and high corrosion resistance, meeting practical application requirements.
[0007] To achieve this objective, the present invention adopts the following technical solution:
[0008] A method for preparing a wear-resistant and corrosion-resistant impeller includes the following steps:
[0009] A. After uniformly mixing Ni, Cr, WC and Re, dry to obtain wear-resistant and corrosion-resistant powder;
[0010] B. Prepare the stainless steel impeller base and perform surface treatment on the stainless steel impeller base;
[0011] C. Spray wear-resistant and corrosion-resistant powder onto the surface of the surface-treated stainless steel impeller substrate to form an intermediate coating;
[0012] D. The intermediate coating is calcined under vacuum to diffuse and form a gradient composite coating, resulting in a wear-resistant and corrosion-resistant impeller; wherein, the gradient composite coating comprises, from the inside out, an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer.
[0013] Further, in step A, the wear-resistant and corrosion-resistant powder comprises, by mass percentage, 30-60% Ni, 8-16% Cr, 27-45% WC, and 3-9% Re.
[0014] Furthermore, in step D, the thickness of the gradient composite coating is 230–340 μm.
[0015] Further, the specific steps in step A are as follows: Ni, Cr, WC and Re are placed in a 0.8-1L ball mill jar and ball milled for 15-25 minutes to obtain a uniformly mixed wear-resistant and corrosion-resistant powder; the uniformly mixed wear-resistant and corrosion-resistant powder is placed in a drying oven at a temperature of 70-75℃ and dried for 20-30 minutes to obtain a wear-resistant and corrosion-resistant powder.
[0016] Furthermore, in step B, the stainless steel impeller base is made of either 316 stainless steel or 304 stainless steel.
[0017] Further, in step B, a stainless steel impeller base is prepared, and the surface of the stainless steel impeller base is sandblasted and degreased, and then dried to obtain a surface-treated stainless steel impeller base.
[0018] The specific method of the sandblasting treatment is as follows: the stainless steel impeller substrate is placed on a sandblasting machine, and Al2O3 sand particles are sprayed onto the surface of the stainless steel impeller substrate under a vacuum environment of 0.5 to 0.7 MPa.
[0019] The specific method for degreasing is as follows: first, use an air gun to blow clean the surface of the sandblasted stainless steel impeller substrate, and then place the blown stainless steel impeller substrate in a 75% alcohol solution for ultrasonic cleaning for 5-10 minutes.
[0020] Further, in step C, the spraying is a supersonic flame spraying process, and the spraying distance of the supersonic flame spraying process is 170-180mm, the powder feeding rate is 35-45g / min, the spraying temperature is ≤120℃, the hydrogen rate is 30-40L / min, the propane rate is 70-80L / min, and the nitrogen rate is 20-25L / min.
[0021] Furthermore, in step C, the surface-treated stainless steel impeller substrate is preheated before the spraying process.
[0022] The specific method for the preheating treatment is as follows: preheat the surface-treated stainless steel impeller substrate at 400-600℃ for 5-10 minutes.
[0023] Further, the specific steps of step D are as follows: placing the intermediate coating in a vacuum calcination furnace, under a vacuum degree of 10... -2 ~10 -3 In a vacuum environment of Pa, the vacuum sintering furnace is heated from room temperature to 1100-1200℃ at a heating rate of 10-15℃ / min, held at that temperature for 10-30min, and then cooled to room temperature at a cooling rate of 1-5℃ / min. This process diffuses to form a gradient composite coating consisting of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside out, resulting in a wear-resistant and corrosion-resistant impeller.
[0024] A wear-resistant and corrosion-resistant impeller is prepared using the above-described method for preparing wear-resistant and corrosion-resistant impellers, wherein the microhardness of the wear-resistant and corrosion-resistant impeller is ≥1300 HV. 1.0 The coefficient of friction and wear is ≤0.55, and the corrosion resistance time is ≥420h.
[0025] The technical solutions provided in this application embodiment may include the following beneficial effects:
[0026] 1. Wear-resistant and corrosion-resistant metal powder is first coated with an intermediate layer by spraying. Then, the intermediate layer is calcined under vacuum. During the vacuum calcination process, there is a difference in diffusion rate between the components in the wear-resistant and corrosion-resistant powder. Ni diffuses from the outside to the inside. Due to the restriction of Ni diffusion by Re, Ni and WC form a Ni-based WC layer, and Ni and Re form a Ni-Re layer. In addition, since C and Cr in WC have relatively fast diffusion rates during vacuum sintering, and Re does not significantly hinder their diffusion rates, C and Cr penetrate into the interior of the stainless steel impeller substrate and form an Fe-based Cr3C2 layer with Fe in the stainless steel impeller substrate. A gradient composite coating is prepared, which includes an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside to the outside. Among them, WC belongs to the hard ceramic phase, which can effectively improve hardness and wear resistance. Ni has strong resistance to acid and alkali corrosion, which is beneficial to improving corrosion resistance and wear resistance. Utilizing the wear resistance property of WC and the corrosion resistance property of Ni, the Ni-based WC layer has good corrosion resistance and wear resistance, thereby improving the wear resistance and corrosion resistance of the gradient composite coating. In addition, the Fe-based Cr3C2 layer has good wear resistance and corrosion resistance, and the Ni-Re layer has good corrosion resistance. Through the synergy of the three-layer structure of Fe-based Cr3C2 layer, Ni-Re layer and Ni-based WC layer, the wear resistance and corrosion resistance of the gradient composite coating are greatly improved. At the same time, since the Fe-based Cr3C2 layer is formed by the C and Cr in WC penetrating into the impeller substrate, the stainless steel impeller substrate and the gradient composite coating are mutually integrated. The material and performance abrupt changes between the Fe-based Cr3C2 layer and the stainless steel impeller substrate are minimal, and its bonding strength with the impeller substrate is extremely high, resulting in extremely high bonding strength between the gradient composite coating and the stainless steel impeller substrate.
[0027] 2. The vacuum calcination process used in this technical solution not only achieves a pore-free, crack-free, and fully metallurgically bonded composite gradient coating, ensuring its performance, but also facilitates a complete metallurgical bond between the gradient composite coating and the impeller substrate. This ensures the bonding strength between the gradient composite coating and the impeller substrate, avoiding the defect that even if the composite gradient coating itself has high wear resistance and corrosion resistance, the gradient composite coating obtained by laser cladding process cannot significantly increase the wear resistance and corrosion resistance of the stainless steel impeller substrate, thus failing to obtain an impeller with high wear resistance and corrosion resistance. Attached Figure Description
[0028] Figure 1 This is a scanning electron microscope image of the gradient composite coating in Example 1 of the preparation method of a wear-resistant and corrosion-resistant impeller of the present invention. Detailed Implementation
[0029] This technical solution provides a method for preparing a wear-resistant and corrosion-resistant impeller, including the following steps:
[0030] A. After uniformly mixing Ni, Cr, WC and Re, dry to obtain wear-resistant and corrosion-resistant powder;
[0031] B. Prepare the stainless steel impeller base and perform surface treatment on the stainless steel impeller base;
[0032] C. Spray wear-resistant and corrosion-resistant powder onto the surface of the surface-treated stainless steel impeller substrate to form an intermediate coating;
[0033] D. The intermediate coating is calcined under vacuum to diffuse and form a gradient composite coating, resulting in a wear-resistant and corrosion-resistant impeller; wherein, the gradient composite coating comprises, from the inside out, an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer.
[0034] To address the technical problem of poor wear resistance and corrosion resistance in existing impeller technologies, this technical solution proposes a method for preparing a wear-resistant and corrosion-resistant impeller. The prepared wear-resistant and corrosion-resistant impeller comprises a stainless steel impeller substrate and a gradient composite coating wrapped around the stainless steel impeller substrate. The gradient composite coating, from the inside out, includes an Fe-based Cr3C2 layer (iron-based chromium carbide), a Ni-Re layer (nickel-rhenium layer), and a Ni-based WC layer (nickel-based tungsten carbide layer). This technical solution optimizes the raw materials of the wear-resistant and corrosion-resistant powder and combines spraying and vacuum calcination processes. This not only achieves a pore-free, crack-free impeller with complete metallurgical bonding between the gradient layers, giving the gradient composite coating high wear resistance and corrosion resistance, but also ensures the bonding strength between the gradient composite coating and the impeller substrate. This allows the gradient composite coating to stably adhere to the surface of the stainless steel impeller substrate. When used in harsh environments, it can more effectively resist external impacts, and the gradient composite coating is not easily damaged, thus ensuring the wear resistance and corrosion resistance of the impeller and meeting practical application requirements.
[0035] In order to make the impeller have high wear resistance and high corrosion resistance, the existing technology involves laser cladding a Ni-based WC gradient composite coating on the surface of the stainless steel impeller substrate. Although this can improve the wear resistance and corrosion resistance of the impeller, it is still difficult to meet the requirements of applications with high wear resistance and corrosion resistance.
[0036] The raw materials for the wear-resistant and corrosion-resistant powder in this technical solution include Ni (nickel), Cr (chromium), WC (tungsten carbide), and Re (rhenium). The wear-resistant and corrosion-resistant metal powder is first coated to obtain an intermediate coating, and then the intermediate coating is calcined in vacuum. During the vacuum calcination process, there is a difference in diffusion rate between the components in the wear-resistant and corrosion-resistant powder. Ni diffuses from the outside to the inside, and due to the restriction of Ni diffusion by Re, Ni and WC form a Ni-based WC layer, and Ni and Re form a Ni-Re layer. In addition, since the diffusion rates of C and Cr in WC are relatively fast during vacuum sintering, and Re does not significantly hinder their diffusion rates, C and Cr penetrate into the interior of the stainless steel impeller substrate and form an Fe-based Cr3C2 layer with Fe in the stainless steel impeller substrate. Thus, a gradient composite coating is prepared, which includes an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside to the outside. Among them, WC belongs to the hard ceramic phase, which can effectively improve hardness and wear resistance. Ni has strong resistance to acid and alkali corrosion, which is beneficial to improving corrosion resistance and wear resistance. Utilizing the wear resistance property of WC and the corrosion resistance property of Ni, the Ni-based WC layer has good corrosion resistance and wear resistance, thereby improving the wear resistance and corrosion resistance of the gradient composite coating. In addition, the Fe-based Cr3C2 layer has good wear resistance and corrosion resistance, and the Ni-Re layer has good corrosion resistance. Through the synergy of the three-layer structure of Fe-based Cr3C2 layer, Ni-Re layer and Ni-based WC layer, the wear resistance and corrosion resistance of the gradient composite coating are greatly improved. At the same time, since the Fe-based Cr3C2 layer is formed by the C and Cr in WC penetrating into the impeller substrate, the stainless steel impeller substrate and the gradient composite coating are mutually integrated. The material and performance abrupt changes between the Fe-based Cr3C2 layer and the stainless steel impeller substrate are minimal, and its bonding strength with the impeller substrate is extremely high, resulting in extremely high bonding strength between the gradient composite coating and the stainless steel impeller substrate. Furthermore, the vacuum calcination process used in this technical solution not only achieves a complete metallurgical bond between the gradient layers, free of pores and cracks, ensuring the performance of the composite gradient coating, but also facilitates a complete metallurgical bond between the gradient composite coating and the impeller substrate. This ensures the bonding strength between the gradient composite coating and the impeller substrate, avoiding the defect that even if the composite gradient coating itself has high wear resistance and corrosion resistance, the gradient composite coating obtained by laser cladding process cannot significantly increase the wear resistance and corrosion resistance of the stainless steel impeller substrate, thus failing to obtain an impeller with high wear resistance and corrosion resistance.
[0037] Specifically, existing technologies typically employ laser cladding to deposit a gradient composite coating onto the surface of a stainless steel impeller substrate, creating a metallurgical bond between the gradient layers. However, the rapid heating and cooling processes during laser cladding still result in localized stress concentrations, making it difficult for the gradient layers of the coating, as well as the coating itself, to achieve a complete metallurgical bond with the stainless steel impeller substrate, leading to poor bonding strength. Furthermore, these localized stress concentrations make the gradient composite coating prone to cracking, causing it to detach during use and resulting in rapid wear or corrosion of the impeller. Therefore, even if the gradient composite coating itself possesses high wear and corrosion resistance, the laser cladding process cannot significantly increase the wear and corrosion resistance of the stainless steel impeller substrate, making it difficult to obtain impellers with high wear and corrosion resistance.
[0038] Vacuum calcination is a high-temperature calcination process conducted in a low-pressure, low-oxygen, and water-vapor-free environment. Compared to laser cladding, its heating and cooling processes are relatively slow, resulting in lower internal stress during heating and cooling. This not only allows for the formation of a fully metallurgically bonded gradient composite coating between the gradient layers, ensuring its performance, but also facilitates a complete metallurgical bond between the gradient composite coating and the impeller substrate. This ensures the bonding strength between the gradient composite coating and the impeller substrate, avoiding the drawback that even if the gradient composite coating itself has high wear resistance and corrosion resistance, laser cladding cannot significantly increase the wear resistance and corrosion resistance of the stainless steel impeller substrate, thus failing to produce an impeller with high wear resistance and corrosion resistance.
[0039] Furthermore, the raw materials used in the preparation of gradient composite coatings in the prior art typically include Ni and WC. When Ni-based WC gradient composite layers are prepared using Ni and WC, during the laser cladding process, the carbon generated by the burning of the raw material WC easily reacts with oxygen in the air to generate CO and CO2 gases. Moreover, the CO and CO2 gases cannot escape in time during the laser cladding process, which leads to the formation of pores on the surface of the Ni-based WC gradient composite coating. This reduces the density of the Ni-based WC gradient composite coating, creating a hidden danger of corrosion of the stainless steel impeller substrate. It also increases the probability of blistering and peeling of the Ni-based WC gradient composite coating, further making it difficult to obtain impellers with high wear resistance and corrosion resistance even if the gradient composite coating itself has high wear resistance and corrosion resistance.
[0040] In this technical solution, vacuum calcination is performed in a vacuum environment, which reduces the possibility of C generated by WC burn-off being oxidized to produce CO and CO2 gases. In addition, the heating process of vacuum calcination facilitates the timely escape of gases, so that even if CO and CO2 gases are generated during vacuum calcination, they can be discharged in time, thereby ensuring the performance of the gradient composite coating.
[0041] Furthermore, in existing technologies, composite gradient coatings are typically prepared by using raw materials from each gradient layer to prepare each gradient layer. This not only increases the difficulty of preparing gradient composite coatings but also tends to weaken the bonding strength of each gradient layer in the composite gradient coating.
[0042] In this technical solution, to reduce the difficulty of preparing the gradient composite coating while ensuring the bonding strength of each gradient layer in the gradient composite coating, the wear-resistant and corrosion-resistant powder has been specifically optimized. Specifically, the raw materials of the wear-resistant and corrosion-resistant powder include Ni, Cr, WC, and Re. Among these, WC is beneficial for improving hardness and wear resistance; Ni has good mechanical strength and ductility, and strong resistance to acid and alkali corrosion, which is beneficial for improving corrosion resistance and bonding strength; Cr is beneficial for improving corrosion resistance; and Re hinders the diffusion of Ni, which is beneficial for ensuring the performance of Ni. Simultaneously, there are diffusion rate differences among the components Ni, Cr, WC, and Re. During vacuum calcination, Ni diffuses from the outside in, and due to the restriction of Ni diffusion by Re, Ni forms a Ni-based WC layer with WC, and a Ni-Re layer with Re. Furthermore, since both C and Cr in WC diffuse rapidly during vacuum sintering, and Re does not significantly hinder their diffusion, C and Cr penetrate into the stainless steel impeller substrate and form a Fe-based Cr3C2 layer with Fe in the substrate. Therefore, the vacuum calcination process can be used to form a gradient composite coating consisting of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside out, eliminating the need to prepare each gradient layer separately, simplifying the preparation process, and ensuring the metallurgical bonding strength between the gradient layers, thus guaranteeing the performance of the gradient composite coating. Additionally, the high corrosion resistance and toughness of Ni are concentrated in the outer and middle parts of the gradient composite coating, which helps ensure product performance.
[0043] In addition, the addition of Cr in this technical solution allows the C generated from WC burn-off to form an Fe-based Cr3C2 layer with Cr and Fe in the stainless steel impeller substrate. This enables the stainless steel impeller substrate and the gradient composite coating to fuse together, improving the bonding strength between them. In other words, by optimizing the wear-resistant and corrosion-resistant powder formulation, this technical solution utilizes the C generated from WC burn-off to further enhance the bonding strength between the stainless steel impeller substrate and the gradient composite coating. This further resolves the adverse effects of C generated from WC burn-off on impeller performance during laser cladding processes, ensuring the impeller's wear resistance and corrosion resistance.
[0044] In addition, the wear-resistant and corrosion-resistant impeller of this technical solution is prepared by four steps. First, Ni, Cr, WC and Re are mixed evenly and then dried to obtain wear-resistant and corrosion-resistant powder. The drying process helps to remove moisture and volatiles from the powder, avoiding the release of moisture or volatiles during the preparation of the gradient composite coating, which could lead to pores or cracks, thus ensuring the performance of the obtained gradient composite coating.
[0045] Secondly, prepare a stainless steel impeller substrate and perform surface treatment on the stainless steel impeller substrate to remove oil, dust and oxide layers from the surface of the impeller substrate, so as to fully expose its original surface, which is conducive to improving the bonding strength between the gradient composite coating and the stainless steel impeller substrate and ensuring the relevant performance of the impeller.
[0046] Furthermore, a wear-resistant and corrosion-resistant powder is sprayed onto the surface of the surface-treated stainless steel impeller substrate to form an intermediate coating, which is beneficial for the subsequent preparation of composite gradient coatings.
[0047] Finally, the intermediate coating is calcined under vacuum to diffuse and form a gradient composite coating consisting of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside out, resulting in a wear-resistant and corrosion-resistant impeller. The gradient composite coating consisting of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside out can be obtained by using the vacuum calcination process, eliminating the need to prepare each gradient layer separately, simplifying the preparation process and improving production efficiency.
[0048] To further explain, in step A, the wear-resistant and corrosion-resistant powder, calculated by mass percentage, comprises 30-60% Ni, 8-16% Cr, 27-45% WC, and 3-9% Re.
[0049] In a preferred embodiment of this technical solution, by optimizing the raw material ratio of the wear-resistant and corrosion-resistant powder, the performance of the resulting gradient composite coating and the bonding strength between the gradient composite coating and the stainless steel substrate are ensured, which is beneficial to improving the performance of the impeller.
[0050] To further explain, in step D, the thickness of the gradient composite coating is 230–340 μm.
[0051] In a preferred embodiment of this technical solution, optimizing the thickness of the gradient composite coating helps ensure the bonding strength between the gradient composite coating and the stainless steel substrate, thereby ensuring the impeller's performance. Furthermore, since the mass percentages of the components in the wear-resistant and corrosion-resistant powder differ, the thickness of each gradient layer during diffusion is controlled by the mass percentage of each component; that is, components with higher content correspond to thicker layers, while components with lower content correspond to thinner gradient layers. Therefore, when the thickness of the gradient composite coating is determined, the thickness of each gradient layer is also determined. Limiting the thickness of the gradient composite layer also helps ensure its performance, thereby ensuring the impeller's performance.
[0052] To further explain, the specific steps in step A are as follows: Ni, Cr, WC and Re are placed in a 0.8-1L ball mill jar and ball milled for 15-25 minutes to obtain a uniformly mixed wear-resistant and corrosion-resistant powder; the uniformly mixed wear-resistant and corrosion-resistant powder is placed in a drying oven at a temperature of 70-75℃ and dried for 20-30 minutes to obtain the wear-resistant and corrosion-resistant powder.
[0053] In a preferred embodiment of this technical solution, by optimizing the mixing process, uneven mixing can be avoided, which would lead to inconsistent performance in the resulting gradient composite coating and thus affect its performance. Furthermore, optimizing the drying process ensures complete removal of moisture and volatiles from the wear-resistant and corrosion-resistant powder, thereby guaranteeing the performance of the gradient composite coating.
[0054] To further clarify, in step B, the stainless steel impeller base is made of either 316 stainless steel or 304 stainless steel.
[0055] In a preferred embodiment of this technical solution, the stainless steel impeller substrate is made of either 316 stainless steel or 304 stainless steel. Both 316 stainless steel and 304 stainless steel have good wear resistance and corrosion resistance. The stainless steel impeller is made using their excellent mechanical properties, and a gradient composite coating is set on the surface of the stainless steel impeller, which helps to ensure the impeller's high wear resistance and high corrosion resistance.
[0056] Preferably, the stainless steel impeller substrate is made of 304 stainless steel. Compared with 316 stainless steel, 304 stainless steel offers a higher cost-performance ratio, which helps reduce production costs. Furthermore, due to the excellent wear resistance and corrosion resistance of the composite gradient coating, even though the wear resistance and corrosion resistance of the stainless steel impeller substrate made of 304 stainless steel are lower than those made of 316 stainless steel, the impeller's performance can still be ensured, thereby improving the product's cost-effectiveness.
[0057] To further explain, in step B, a stainless steel impeller base is prepared, and the surface of the stainless steel impeller base is sandblasted and degreased. After drying, a surface-treated stainless steel impeller base is obtained.
[0058] The specific method of the sandblasting treatment is as follows: the stainless steel impeller substrate is placed on a sandblasting machine, and Al2O3 sand particles are sprayed onto the surface of the stainless steel impeller substrate under a vacuum environment of 0.5 to 0.7 MPa.
[0059] The specific method for degreasing is as follows: first, use an air gun to blow clean the surface of the sandblasted stainless steel impeller substrate, and then place the blown stainless steel impeller substrate in a 75% alcohol solution for ultrasonic cleaning for 5-10 minutes.
[0060] In a preferred embodiment of this technical solution, the specific method of sandblasting is as follows: the stainless steel impeller substrate is placed on a sandblasting machine, and Al2O3 sand particles are sprayed onto the surface of the stainless steel impeller substrate under a vacuum environment of 0.5 to 0.7 MPa. Through the impact and cutting action of the Al2O3 sand particles, the stains and oxide layer on the surface of the stainless steel impeller substrate are removed, and the surface of the stainless steel impeller substrate is given a certain roughness, which is beneficial to improving the bonding strength between the gradient composite coating and the stainless steel impeller substrate.
[0061] Furthermore, the specific method for degreasing is as follows: First, use an air gun to blow away the surface of the sandblasted stainless steel impeller substrate to remove residual sand particles and dust; then, place the blown stainless steel impeller substrate in a 75% alcohol solution for ultrasonic cleaning for 5-10 minutes to remove surface oil and Al2O3 sand particles, making the surface of the stainless steel impeller substrate clean, burr-free, and with a certain degree of roughness, which is beneficial to ensuring the bonding strength with the gradient composite coating.
[0062] To further clarify, in step C, the spraying is a supersonic flame spraying process, and the spraying distance of the supersonic flame spraying process is 170-180mm, the powder feeding rate is 35-45g / min, the spraying temperature is ≤120℃, the hydrogen rate is 30-40L / min, the propane rate is 70-80L / min, and the nitrogen rate is 20-25L / min.
[0063] Compared with other spraying processes such as laser cladding and flame remelting, the intermediate coating obtained by supersonic flame spraying has higher bonding strength, higher density and hardness, resulting in better wear resistance and corrosion resistance of the prepared impeller. In addition, the stainless steel impeller substrate receives very little heat during the spraying process, making it less prone to deformation.
[0064] To further explain, step C includes preheating the surface-treated stainless steel impeller substrate before the spraying process.
[0065] The specific method for the preheating treatment is as follows: preheat the surface-treated stainless steel impeller substrate at 400-600℃ for 5-10 minutes.
[0066] In a preferred embodiment of this technical solution, the stainless steel impeller substrate is preheated to remove stress before spraying, thus preventing it from bending due to stress release during the spraying process and subsequent processes, which would be detrimental to improving the bonding strength between the gradient composite coating and the stainless steel impeller substrate.
[0067] To further explain, step D specifically involves placing the intermediate coating in a vacuum calcination furnace at a vacuum degree of 10... -2 ~10 -3 In a vacuum environment of Pa, the vacuum sintering furnace is heated from room temperature to 1100-1200℃ at a heating rate of 10-15℃ / min, held at that temperature for 10-30min, and then cooled to room temperature at a cooling rate of 1-5℃ / min. This process diffuses to form a gradient composite coating consisting of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside out, resulting in a wear-resistant and corrosion-resistant impeller.
[0068] In a preferred embodiment of this technical solution, by optimizing the parameters in vacuum calcination, it is beneficial to ensure the performance of the gradient composite coating and the bonding strength between the gradient composite coating and the stainless steel impeller substrate, thereby ensuring the performance of the impeller.
[0069] A wear-resistant and corrosion-resistant impeller is prepared using the above-described method for preparing wear-resistant and corrosion-resistant impellers, wherein the microhardness of the wear-resistant and corrosion-resistant impeller is ≥1300 HV. 1.0 The coefficient of friction and wear is ≤0.55, and the corrosion resistance time is ≥420h.
[0070] In a preferred embodiment of this technical solution, higher microhardness corresponds to higher wear resistance; a smaller coefficient of friction and wear also indicates higher wear resistance; and a longer corrosion resistance time results in higher corrosion resistance. In this technical solution, the microhardness of the wear-resistant and corrosion-resistant impeller is ≥1300 HV. 1.0 With a friction and wear coefficient ≤0.55 and a corrosion failure time ≥648h, the impeller is endowed with high wear resistance and high corrosion resistance to meet actual application requirements.
[0071] The technical solution of the present invention will be further illustrated below through specific embodiments.
[0072] Performance testing:
[0073] Microhardness test: The impeller was tested using a microhardness tester with a load of 1000g and a loading time of 10s.
[0074] Friction coefficient test: The impeller was tested for friction and wear using a friction and wear testing machine; the friction pair was Si3N4 balls, the reciprocating friction length was 10mm, the load was 10N, the speed was 0.05m / s, and the sliding distance was 200m.
[0075] Corrosion resistance failure time test: Prepare a 5% sodium chloride solution, place the impeller in the 5% sodium chloride solution, and test the time required for the gradient composite coating on the impeller to fail.
[0076] Example 1
[0077] A. According to the mass percentage, Ni 55%, Cr 9%, WC 27% and Re 9% are placed in a 0.8L ball mill jar and ball milled for 25 minutes to obtain a uniformly mixed wear-resistant and corrosion-resistant powder; the uniformly mixed wear-resistant and corrosion-resistant powder is placed in a drying oven at 70℃ and dried for 25 minutes to obtain dried wear-resistant and corrosion-resistant powder.
[0078] B. Prepare a stainless steel impeller base made of 304 stainless steel. Perform sandblasting and degreasing treatment on the surface of the stainless steel impeller base, and dry it to obtain a surface-treated stainless steel impeller base. The specific method of sandblasting is as follows: place the stainless steel impeller base on a sandblasting machine, and spray Al2O3 sand particles onto the surface of the stainless steel impeller base under a vacuum environment of 0.5MPa. The specific method of degreasing treatment is as follows: first, blow the surface of the sandblasted stainless steel impeller base with an air gun, and then place the blown stainless steel impeller base in a 75% alcohol solution for ultrasonic cleaning for 10 minutes.
[0079] C. The surface-treated stainless steel impeller substrate is preheated at 600℃ for 5 minutes to obtain a preheated stainless steel impeller substrate; the surface of the preheated stainless steel impeller substrate is sprayed with dried wear-resistant and corrosion-resistant powder to form an intermediate coating; wherein, the spraying is a supersonic flame spraying process, and the spraying distance of the supersonic flame spraying process is 170mm, the powder feeding rate is 45g / min, the spraying temperature is 110℃, the hydrogen rate is 35L / min, the propane rate is 80L / min, and the nitrogen rate is 25L / min.
[0080] D. Place the intermediate coating in a vacuum calcination furnace at a vacuum degree of 10. ~3In a vacuum environment of Pa, the vacuum sintering furnace is heated from room temperature to 1120℃ at a heating rate of 15℃ / min, held at that temperature for 30 min, and then cooled back to room temperature at a cooling rate of 5℃ / min. This process allows diffusion to form a gradient composite coating, resulting in a wear-resistant and corrosion-resistant impeller. The gradient composite coating consists of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer, arranged sequentially from the inside out. The scanning electron microscope image of the gradient composite coating is shown below. Figure 1 As shown, the thickness of the gradient composite coating is 300 μm, and the scanning electron microscope image of the gradient composite coating is as follows. Figure 1 As shown.
[0081] Example 2
[0082] A. According to the mass percentage, Ni 30%, Cr 16%, WC 45% and Re 9% are put into a 1L ball mill jar and ball milled for 15 minutes to obtain a uniformly mixed wear-resistant and corrosion-resistant powder; the uniformly mixed wear-resistant and corrosion-resistant powder is placed in a drying oven at 75℃ and dried for 20 minutes to obtain dried wear-resistant and corrosion-resistant powder.
[0083] B. Prepare a stainless steel impeller base made of 316 stainless steel. Perform sandblasting and degreasing treatment on the surface of the stainless steel impeller base, and dry it to obtain a surface-treated stainless steel impeller base. The specific method of sandblasting is as follows: place the stainless steel impeller base on a sandblasting machine, and spray Al2O3 sand particles onto the surface of the stainless steel impeller base under a vacuum environment of 0.6MPa. The specific method of degreasing treatment is as follows: first, blow the surface of the sandblasted stainless steel impeller base with an air gun, and then place the blown stainless steel impeller base in a 75% alcohol solution for ultrasonic cleaning for 8 minutes.
[0084] C. The surface-treated stainless steel impeller substrate is preheated at 500℃ for 8 minutes to obtain a preheated stainless steel impeller substrate; the surface of the preheated stainless steel impeller substrate is sprayed with dried wear-resistant and corrosion-resistant powder to form an intermediate coating; wherein, the spraying is a supersonic flame spraying process, and the spraying distance of the supersonic flame spraying process is 180mm, the powder feeding rate is 45g / min, the spraying temperature is 120℃, the hydrogen rate is 40L / min, the propane rate is 70L / min, and the nitrogen rate is 20L / min.
[0085] D. Place the intermediate coating in a vacuum calcination furnace at a vacuum degree of 10. -2In a vacuum environment of Pa, the vacuum sintering furnace is heated from room temperature to 1100℃ at a heating rate of 10℃ / min, held at that temperature for 20min, and then cooled back to room temperature at a cooling rate of 3℃ / min. This process diffuses to form a gradient composite coating, resulting in a wear-resistant and corrosion-resistant impeller. The gradient composite coating consists of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside out, with a thickness of 230μm.
[0086] Example 3
[0087] A. According to the mass percentage, Ni 60%, Cr 8%, WC 29% and Re 3% are placed into a 0.9L ball mill jar and ball milled for 20 minutes to obtain a uniformly mixed wear-resistant and corrosion-resistant powder; the uniformly mixed wear-resistant and corrosion-resistant powder is placed in a drying oven at 75℃ and dried for 30 minutes to obtain dried wear-resistant and corrosion-resistant powder.
[0088] B. Prepare a stainless steel impeller base made of 304 stainless steel. Perform sandblasting and degreasing treatment on the surface of the stainless steel impeller base, and dry it to obtain a surface-treated stainless steel impeller base. The specific method of sandblasting is as follows: place the stainless steel impeller base on a sandblasting machine, and spray Al2O3 sand particles onto the surface of the stainless steel impeller base under a vacuum environment of 0.7MPa. The specific method of degreasing treatment is as follows: first, blow the surface of the sandblasted stainless steel impeller base with an air gun, and then place the blown stainless steel impeller base in a 75% alcohol solution for ultrasonic cleaning for 5 minutes.
[0089] C. The surface-treated stainless steel impeller substrate is preheated at 400℃ for 10 min to obtain a preheated stainless steel impeller substrate; the surface of the preheated stainless steel impeller substrate is sprayed with dried wear-resistant and corrosion-resistant powder to form an intermediate coating; wherein, the spraying is a supersonic flame spraying process, and the spraying distance of the supersonic flame spraying process is 175 mm, the powder feeding rate is 45 g / min, the spraying temperature is ≤120℃, the hydrogen rate is 30 L / min, the propane rate is 75 L / min, and the nitrogen rate is 23 L / min.
[0090] D. Place the intermediate coating in a vacuum calcination furnace at a vacuum degree of 10. ~3 In a vacuum environment of Pa, the vacuum sintering furnace is heated from room temperature to 1150℃ at a heating rate of 15℃ / min, held at that temperature for 30 min, and then cooled back to room temperature at a cooling rate of 15℃ / min. This process diffuses to form a gradient composite coating, resulting in a wear-resistant and corrosion-resistant impeller. The gradient composite coating consists of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside out, with a thickness of 230 μm.
[0091] Comparative group
[0092] Comparative Example 1
[0093] The preparation method of Comparative Example 1 is the same as that of Example 1, except that the gradient composite coating is prepared by laser cladding process in Comparative Example 1. The gradient composite coating includes a first gradient layer and a second gradient layer. The raw material components of the first gradient layer, by mass percentage, are: Ni 60% and WC 40%.
[0094] Comparative Example 2
[0095] The preparation method of Comparative Example 2 is the same as that of Example 1, except that the raw materials of the wear-resistant and corrosion-resistant powder in Comparative Example 2 do not include Re; that is, the raw materials of the wear-resistant and corrosion-resistant powder, calculated by mass percentage, include Ni 55%, Cr 9% and WC 36%.
[0096] Comparative Example 3
[0097] The preparation method of Comparative Example 3 is the same as that of Example 1, except that the raw materials of the wear-resistant and corrosion-resistant powder in Comparative Example 3 do not include Cr; that is, the raw materials of the wear-resistant and corrosion-resistant powder include Ni 55%, Re 9% and WC 36% by mass percentage.
[0098] The impellers obtained in the above-described embodiment group and comparative example group were subjected to performance tests, and the specific test results are shown in Table 1 below:
[0099] Table 1. Test results of relevant impeller performance.
[0100]
[0101] As can be seen from the test results in Table 1, the impeller prepared by the method of this technical solution has a microhardness ≥1300HV1.0, a friction and wear coefficient ≤0.55, and a corrosion failure time ≥648h, which endows the impeller with high wear resistance and high corrosion resistance. Compared with the stainless steel impeller substrate without any treatment, its performance is greatly improved.
[0102] Comparative Example 1 uses a laser cladding process to prepare a Ni-based WC gradient composite coating. However, due to the abrupt change in material properties at the interface between the Ni-based WC gradient composite coating and the stainless steel impeller substrate, defects such as localized stress concentration and poor bonding strength still exist at the interface, even with the gradient composite coating. Furthermore, during the laser cladding process, the CO and CO2 gases generated by the reaction of carbon produced by the burning of the raw material WC with oxygen in the air cannot escape in time. This leads to the formation of pores on the surface of the Ni-based WC gradient composite coating, which becomes a new hidden danger for corrosion of the stainless steel impeller substrate. This increases the probability of blistering and peeling of the Ni-based WC gradient composite coating, making it prone to localized detachment even with high microhardness during use. This results in a higher coefficient of friction, a shorter corrosion failure time, and decreased wear and corrosion resistance of the impeller.
[0103] In Comparative Example 2, because the raw materials of the wear-resistant and corrosion-resistant powder do not include Re, Ni cannot be concentrated in the outer and middle parts of the gradient composite coating, resulting in a larger friction coefficient, a shorter corrosion failure time, and poorer wear resistance and corrosion resistance of the impeller.
[0104] In Comparative Example 3, since the raw materials of the wear-resistant and corrosion-resistant powder do not include Cr, the Fe-based Cr3C2 layer cannot be formed, which leads to a decrease in the wear resistance and corrosion resistance of the gradient composite coating. Furthermore, the bonding strength between the gradient composite coating and the stainless steel impeller substrate decreases, resulting in a higher coefficient of friction, a shorter corrosion failure time, and a decrease in the wear resistance and corrosion resistance of the impeller.
[0105] The technical principles of the present invention have been described above with reference to specific embodiments. These descriptions are merely for explaining the principles of the invention and should not be construed as limiting the scope of protection of the invention in any way. Based on this explanation, those skilled in the art can readily conceive of other specific embodiments of the invention without inventive effort, and these embodiments will all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a wear-resistant and corrosion-resistant impeller, characterized in that, Includes the following steps: A. After uniformly mixing Ni, Cr, WC and Re, dry to obtain wear-resistant and corrosion-resistant powder; B. Prepare the stainless steel impeller base and perform surface treatment on the stainless steel impeller base; C. Spray wear-resistant and corrosion-resistant powder onto the surface of the surface-treated stainless steel impeller substrate to form an intermediate coating; D. The intermediate coating is calcined under vacuum to diffuse and form a gradient composite coating, resulting in a wear-resistant and corrosion-resistant impeller; wherein, the gradient composite coating comprises, from the inside out, an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer.
2. The method for preparing a wear-resistant and corrosion-resistant impeller according to claim 1, characterized in that, In step A, the wear-resistant and corrosion-resistant powder comprises, by mass percentage, 30-60% Ni, 8-16% Cr, 27-45% WC, and 3-9% Re.
3. The method for preparing a wear-resistant and corrosion-resistant impeller according to claim 2, characterized in that, In step D, the thickness of the gradient composite coating is 230–340 μm.
4. The method for preparing a wear-resistant and corrosion-resistant impeller according to claim 1, characterized in that, The specific steps in step A are as follows: Ni, Cr, WC and Re are placed in a 0.8-1L ball mill jar and ball milled for 15-25 minutes to obtain a uniformly mixed wear-resistant and corrosion-resistant powder; the uniformly mixed wear-resistant and corrosion-resistant powder is placed in a drying oven at a temperature of 70-75℃ and dried for 20-30 minutes to obtain a wear-resistant and corrosion-resistant powder.
5. The method for preparing a wear-resistant and corrosion-resistant impeller according to claim 1, characterized in that, In step B, the stainless steel impeller base is made of either 316 stainless steel or 304 stainless steel.
6. The method for preparing a wear-resistant and corrosion-resistant impeller according to claim 1, characterized in that, In step B, a stainless steel impeller base is prepared, and the surface of the stainless steel impeller base is sandblasted and degreased. After drying, a surface-treated stainless steel impeller base is obtained. The specific method of the sandblasting treatment is as follows: the stainless steel impeller substrate is placed on a sandblasting machine, and Al2O3 sand particles are sprayed onto the surface of the stainless steel impeller substrate under a vacuum environment of 0.5 to 0.7 MPa. The specific method for degreasing is as follows: first, use an air gun to blow clean the surface of the sandblasted stainless steel impeller substrate, and then place the blown stainless steel impeller substrate in a 75% alcohol solution for ultrasonic cleaning for 5-10 minutes.
7. The method for preparing a wear-resistant and corrosion-resistant impeller according to claim 1, characterized in that, In step C, the spraying is a supersonic flame spraying process, and the spraying distance of the supersonic flame spraying process is 170-180mm, the powder feeding rate is 35-45g / min, the spraying temperature is ≤120℃, the hydrogen rate is 30-40L / min, the propane rate is 70-80L / min, and the nitrogen rate is 20-25L / min.
8. The method for preparing a wear-resistant and corrosion-resistant impeller according to claim 1, characterized in that, In step C, the surface-treated stainless steel impeller substrate is preheated before the spraying process. The specific method for the preheating treatment is as follows: preheat the surface-treated stainless steel impeller substrate at 400-600℃ for 5-10 minutes.
9. The method for preparing a wear-resistant and corrosion-resistant impeller according to claim 1, characterized in that, The specific steps of step D are as follows: Place the intermediate coating in a vacuum calcination furnace, and calcine it at a vacuum degree of 10... -2 ~10 -3 In a vacuum environment of Pa, the vacuum calcination furnace is heated from room temperature to 1100-1200℃ at a heating rate of 10-15℃ / min, held at that temperature for 10-30min, and then cooled back to room temperature at a cooling rate of 1-5℃ / min. This process diffuses to form a gradient composite coating consisting of an Fe-based Cr3C2 layer, a Ni-Re layer, and a Ni-based WC layer from the inside out, resulting in a wear-resistant and corrosion-resistant impeller.
10. A wear-resistant and corrosion-resistant impeller, characterized in that: The wear-resistant and corrosion-resistant impeller is prepared using the preparation method described in any one of claims 1 to 9, and the microhardness of the wear-resistant and corrosion-resistant impeller is ≥1300 HV. 1.0 The coefficient of friction and wear is ≤0.55, and the corrosion resistance time is ≥420h.
Citation Information
Patent Citations
Composite gradient coating on surface of heavy load gear and method for preparing composite gradient coating on surface of heavy load gear
CN104388887A
Re-contained high-temperature-resisting wolfram-carbide-based metal ceramic composite powder and coating and preparing technology of coating
CN105648296A