A method for preparing a resistor
Through electric field flash burning and current density distribution image analysis, low-pass regression degree is calculated to judge the reproducibility of resistor defective products, solving the problem of low yield of flash burning technology, and improving the preparation efficiency and resource utilization efficiency of varistors .
Patent Information
- Application Number
- CN202410834885.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-26
AI Technical Summary
In the prior art, the yield of flash burning technology is low, resulting in the long recognition cycle of resistor sheet defective products and low preparation efficiency. It is mainly due to the uneven distribution of materials, which makes the product not meet the requirements through reprocessing.
The sintered blank is flashed through an electric field, and the current density distribution image is collected, and the low-pass regression degree is calculated to determine whether the defective resistive sheets meet the secondary sintering processing requirements. Combined with superpixel segmentation algorithm and fuzzy channel analysis, the judgment accuracy is improved.
Effectively quantify the low-pass effect of current density during flash burning, improve the probability of reproducibility of resistive chip defective products, improve production efficiency and resource utilization, and reduce resource waste.
Smart Images

Figure CN118571584B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of data acquisition and intelligent manufacturing, and specifically relates to a method for preparing a resistor. Background Art
[0002] The resistance value of the varistor will produce nonlinear changes with the voltage. This nonlinear characteristic can make it show high impedance under normal working voltage and low impedance under overvoltage, which is of great significance for protecting circuits. In the process of preparing varistors on industrial production lines, various raw materials need to be evenly mixed and sintered through flash burning technology. However, the yield of flash burning technology has always been a technical challenge in this field. After flash burning, it is necessary to wait until the final varistor preparation is completed before testing, and unqualified products can be reprocessed or discarded. This complete production inspection process makes the identification cycle of defective resistors too long, and the preparation efficiency is greatly reduced. The deficiency of the yield of flash burning technology in the prior art is due to the high requirements for the uniformity control of current distribution, and the defective resistors caused by the change of conductivity due to the uneven distribution of materials inside the material are usually difficult to meet the product requirements through reprocessing. Therefore, there is an urgent need for a resistor preparation method to improve the identification of defective flash burning resistors that meet the requirements for secondary processing, thereby improving the production efficiency of preparing varistors. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a resistor to solve one or more technical problems existing in the prior art and at least provide a beneficial choice or create conditions.
[0004] In order to achieve the above object, according to one aspect of the present invention, a method for preparing a resistor is provided, the method comprising the following steps:
[0005] S100, uniformly mixing the resistor raw materials to form a green body to be sintered;
[0006] S200, preheating the green body to be sintered;
[0007] S300, flash-burning the green body to be sintered by an electric field to obtain a finished resistor sheet, and collecting a current density distribution image during the flash-burning process;
[0008] S301, when the resistor obtained by flash burning is a defective resistor, a low-pass regression degree is calculated according to the current density distribution image;
[0009] S302, judging whether the defective resistor chip meets the secondary sintering treatment requirements by combining the low-pass regression;
[0010] Further, in step S100, the method of uniformly mixing the resistor raw materials to form a green body to be sintered is: the raw materials are mixed using a ball mill or a high-speed mixer, wherein the resistor raw materials include zinc oxide, barium oxide, strontium oxide and silicon oxide; the resistor raw materials are mixed in a mold, and then pressed using a tablet press to obtain a green body to be sintered.
[0011] Further, in step S200, the method for preheating the green body to be sintered is: heating the green body to be sintered to 30%-50% of the sintering temperature, the heating equipment is a muffle furnace, and the heating rate is 2K / min-3K / min; if the sintering temperature is not specified, it is heated to 500 degrees Celsius by default.
[0012] Furthermore, in step S300, the sintered green body is flash-burned by an electric field to obtain a finished resistor chip, and the method for collecting the current density distribution image during the flash-burning process is: after applying conductive silver paste on both ends of the green body to be sintered, put it into a flash-burning furnace, set the heating rate in the flash-burning furnace to 10K / min, and heat it to 600 degrees Celsius; after keeping warm for 15 minutes to 20 minutes, open the furnace to cool, connect the two ends of the green body surface to the AC power supply through platinum wires, and then turn on the power to continuously increase the voltage until the flash-burning starts, and scan the green body magnetic field distribution image through a Hall effect sensor, and convert the magnetic field distribution image into a current density distribution image through an inversion algorithm, and the pixel value of each pixel in the current density distribution image is an inversion value; record the current density distribution image from the beginning of the flash-burning and store it in the server until the flash-burning ends to obtain the finished resistor chip.
[0013] Further, in step S301, when the resistor obtained by flash burning is a defective resistor, the method for calculating the low-pass regression degree according to the current density distribution image is: for any time, the current density distribution image obtained is an inversion map, and the pixel value corresponding to each pixel in the inversion map is an inversion value; the lower quartile value of each inversion value in the inversion map is recorded as the low-pass threshold of the inversion map, and when the inversion value of the pixel is less than the low-pass threshold, the pixel is defined as a low-pass marking point; the low-pass phase of the low-pass marking point is defined as the difference between the low-pass threshold and its inversion value;
[0014] The fuzzy channel of the low-pass mark point is: the preset channel radius is sr, a parallel line parallel to the electric field direction is drawn through the low-pass mark point, and a cylinder with a radius of sr is drawn with the obtained parallel line as the axis as the fuzzy channel;
[0015] The axial direction of the fuzzy channel includes the front axial direction and the rear axial direction, which respectively represent the two directions of the low-pass marker point along the axis of the fuzzy channel;
[0016] Starting from the low-pass mark point, a fuzzy channel with a length of 2×sr is intercepted along the axial direction of the fuzzy channel as the channel iteration domain. The fuzzy deviation value HVR of the channel iteration domain is: the average value of the low-pass phase of each low-pass mark point in the channel iteration domain is calculated, and the ratio of the obtained average value to the low-pass mark point to which the fuzzy channel belongs is recorded as the fuzzy deviation value;
[0017] With the channel radius as the iteration distance stl, the channel iteration domain is cyclically moved along the axis by stl and the fuzzy deviation value is recalculated. The fuzzy deviation values obtained in each iteration are written into a sequence recorded as the deviation sequence; the first element of the deviation sequence is used to search for the first minimum value that appears and is recorded as the iteration amount nvl; the deviation sub-weight VRWH of the fuzzy channel is calculated according to the fuzzy deviation value:
[0018]
[0019] Where i1 is the accumulated variable, HVR i1 represents the fuzzy deviation value of the iterative domain of the i1th channel, e is a natural constant, Rt_ov(i1) represents the low-pass coverage of the iterative domain of the i1th channel, and the calculation method of the low-pass coverage is: when HVR i1 >1, the low-pass coverage is the ratio of the elements in the set consisting of the inversion values corresponding to the low-pass marker points in the channel iteration domain, whose values are smaller than the inversion values corresponding to the low-pass marker points belonging to the fuzzy channel; when HVR i1 ≤1, the low-pass coverage is 1; then the partial difference weight MVRWH of the low-pass marker point belonging to the fuzzy channel is the sum of the two partial difference sub-weights on different axes;
[0020] For any pixel in the inversion map as the current pixel, identify the moment when the pixel is used as a low-pass marker point during the flash process, and record any continuous moments as low-pass marker points as a low-pass event. The maximum value of each deviation weight obtained under the low-pass event is recorded as a low-pass scalar. The number of moments included in the low-pass event is the low-pass duration value. The low-pass scalar and the low-pass duration value are combined into a binary group recorded as a low-pass feature group. The set composed of each low-pass feature group of the current pixel is recorded as a low-pass set. The low-pass set is linearly fitted by the polyfit function and the slope value is obtained, which is recorded as the low-pass regression degree.
[0021] Since there is a spatial direction dependence phenomenon in the procedure of calculating the low-pass regression degree through the fuzzy channel, it will lead to the problem of insufficient reference to the data outside the fuzzy channel in the space during the time series analysis process. This problem is easy to cause insufficient quantification of a single pixel and cause a lack of judgment accuracy. This problem will be more prominent when the air pressure in the flash furnace is unstable. However, the existing technology cannot solve this problem of insufficient accuracy. In order to better solve this problem and eliminate this phenomenon of missing data reference, the present invention proposes a more preferred solution as follows:
[0022] Preferably, in step S301, when the resistor obtained by flash burning is a defective resistor, the method for calculating the low-pass regression degree according to the current density distribution image is: for any time, the current density distribution image obtained is an inversion map, and the pixel value corresponding to each pixel in the inversion map is an inversion value; the range of the inversion value of any pixel in the flash burning process is calculated as the inversion; the inversion map is segmented into regions according to the inversion amplitude through the super pixel segmentation algorithm, and each region obtained by segmentation is a deconstruction unit;
[0023] Define the average value of each inversion value in the deconstruction unit at any time as the unit inversion value UAri, and the standard deviation of the inversion amplitude corresponding to each pixel in the deconstruction unit as σ, then the derivative rate interval UAZ of the deconstruction unit is: UAZ∈[UAri·(1-σ),UAri·(1+σ)]; take any deconstruction unit as the current deconstruction unit, initialize an area as the mixed unit, set a numerical variable as the iteration stp, which is initially 1; set its starting area as the current deconstruction unit, search for each deconstruction unit adjacent to the mixed unit as the neighboring deconstruction unit, and the derivative vector EUA of the neighboring deconstruction unit is: EUA=UAri / λ stp , where λ is the convergence coefficient, λ∈[1,e]; the mixing condition of the adjacent deconstruction unit is defined as UAri ps <UAZ; When the adjacent deconstruction unit meets the mixed condition, it is merged into the mixed unit; repeat the iteration to merge new adjacent deconstruction units into the mixed unit, and increase the number of iterations by 1 at each iteration until the number of adjacent deconstruction units merged into the mixed unit at the current iteration is 0;
[0024] Set a time length as the retention period TS, the intersection of all the mixed units in the TS period from the current deconstruction unit at any time to its reverse time direction is the hysteresis mixing domain, the range of the inversion value of each structural unit corresponding to the hysteresis mixing domain at this time is the hysteresis mixing distance MTDS, and define the ratio of the intersection number of the mixed unit and the deconstruction unit of the hysteresis mixing domain at this time to the number of deconstruction units in the hysteresis mixing domain as the hybrid composite ratio kurt; the flash burning process obtains all the hybrid composite ratio write sequences recorded as kurt.Ls;
[0025] Define the ratio of the inversion value of the current deconstruction unit at any moment before the TS period to the unit at that moment as the retention amplitude KU. When KU>1, it is defined that the moment meets the low-pass amplitude; the range of the inversion value of each unit obtained from the current deconstruction unit at any moment to the previous TS period is recorded as the sub-deconstruction distance SUDS; calculate the hybrid weight MUWH of the current deconstruction unit:
[0026]
[0027] Where j1 and j2 are accumulated variables, hs<> is the harmonic mean function, which returns the harmonic mean of the calling sequence; ln() is the logarithmic function with the natural constant e as the base; nrku is the number of moments that meet the low-pass amplitude, kurt j2 Represents the ratio of the hybrid structure that meets the low-pass amplitude at the j2nd moment; MTDS j1 and SUDS j1 They represent the hysteresis distance and deconstruction distance of the j1th low-pass amplitude moment respectively; KU j1 represents the retention amplitude at the j1th moment that meets the low-pass amplitude;
[0028] The set of inversion values corresponding to all pixels in the hysteresis domain obtained by the current deconstruction unit at the end of the flash is recorded as ClssT, and the product of the percentile of the inversion value corresponding to any pixel in the current deconstruction unit in ClssT and the hybrid weight is defined as the low-pass regression degree of the pixel;
[0029] Where e is a natural constant; UAri ps Refers to the unit inversion value of the adjacent deconstruction unit; in the spatial description, two regions are adjacent when the edge lines or edge surfaces of the two regions overlap. In the calculation process of the hybrid weight, when j1 and j2 take the value of 1, it represents the moment when the flash burn ends;
[0030] Beneficial effect: Since the low-pass regression degree is calculated based on the current density distribution image, it can accurately mark the position where the current density low-pass effect collapses during the flash burning process, that is, quantify the risk that the local position cannot be accurately covered or actually covered during the flash burning process, and then can efficiently and accurately quantify the probability of the blank being reproducible or repairable, greatly improving the production efficiency and resource utilization efficiency of repeated processing of defective varistor chips through flash burning technology, and reducing the waste of resources caused by repeated processing of invalid defective varistor chips.
[0031] Further, in step S302, the method for judging whether the defective resistor chip meets the requirements of the secondary sintering treatment in combination with the low-pass regression degree is: performing Z-score method outlier identification on all low-pass regression degrees obtained from the inversion map, and presetting the ratio value FRT, FRT∈[0.5%-3%]; if the ratio of the number of outliers identified to the total number of pixels in the inversion map is greater than or equal to FRT, it is judged that it does not meet the requirements of the secondary sintering treatment, and the identification result is sent to the server; otherwise, it is judged that it meets the requirements of the secondary sintering treatment, and the defective resistor chip is subjected to secondary flash sintering or conventional sintering, and the identification result is sent to the server;
[0032] Preferably, all undefined variables in the present invention, if not clearly defined, can be manually set thresholds.
[0033] The present invention also provides a resistor preparation system, the resistor preparation system comprising: a processor, a memory, and a computer program stored in the memory and executable on the processor, the processor implementing the steps in the resistor preparation method when executing the computer program, the resistor preparation system can be run in computing devices such as desktop computers, notebook computers, PDAs, and cloud data centers, and the executable system may include, but is not limited to, a processor, a memory, and a server cluster, and the processor executes the computer program to run in the following system units:
[0034] A material mixing unit, used for uniformly mixing the resistor raw materials to form a green body to be sintered;
[0035] A preheating unit, used for preheating the green body to be sintered;
[0036] A flash burning data acquisition unit is used to flash burn the sintered green body through an electric field to obtain a finished resistor sheet and to collect a current density distribution image during the flash burning process;
[0037] A distribution image analysis unit is used to calculate the low-pass regression degree according to the current density distribution image when the resistor obtained by flash burning is a defective resistor;
[0038] The server feedback unit is used to judge whether the defective resistor chips meet the requirements of secondary sintering treatment in combination with the low-pass regression.
[0039] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing a resistor, which effectively quantifies the risk that a local position cannot be accurately covered or actually covered during the flash burning process by collecting data on the current density distribution image during the flash burning process, and then can efficiently and accurately quantify the probability that the blank can be remade or repaired, thereby greatly improving the production efficiency and resource utilization efficiency of repeated processing of defective varistor sheets through the flash burning technology, and reducing the waste of resources caused by repeated processing of defective invalid resistor sheets. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The above and other features of the present invention will become more obvious by describing in detail the embodiments shown in the accompanying drawings. The same reference numerals in the accompanying drawings of the present invention represent the same or similar elements. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other accompanying drawings can be obtained based on these accompanying drawings without creative work. In the accompanying drawings:
[0041] Figure 1 Shown is a flow chart of a method for preparing a resistor;
[0042] Figure 2 Shown is a structural diagram of a resistor preparation system. DETAILED DESCRIPTION
[0043] The following will be combined with the embodiments and drawings to clearly and completely describe the concept, specific structure and technical effects of the present invention, so as to fully understand the purpose, scheme and effect of the present invention. It should be noted that the embodiments and features in the embodiments of this application can be combined with each other without conflict.
[0044] like Figure 1 The flowchart of a method for preparing a resistor is shown below. Figure 1 A method for preparing a resistor according to an embodiment of the present invention is described below. The method comprises the following steps:
[0045] Embodiment 1:
[0046] S100, uniformly mixing the resistor raw materials to form a green body to be sintered;
[0047] S200, preheating the green body to be sintered;
[0048] S300, flash-burning the green body to be sintered by an electric field to obtain a finished resistor sheet, and collecting a current density distribution image during the flash-burning process;
[0049] S301, when the resistor obtained by flash burning is a defective resistor, a low-pass regression degree is calculated according to the current density distribution image;
[0050] S302, judging whether the defective resistor chip meets the secondary sintering treatment requirements by combining the low-pass regression;
[0051] Further, in step S100, the method of uniformly mixing the resistor raw materials to form a green body to be sintered is: a ball mill is used in the raw material mixing step, wherein the resistor raw materials include zinc oxide, barium oxide, strontium oxide and silicon oxide; the resistor raw materials are mixed in a mold, and then pressed with a tablet press to obtain the green body to be sintered.
[0052] The green body to be sintered is also called a green body, which refers to the green body before sintering. Meanwhile, the resistor raw material may also include other additives, such as aluminum oxide, bismuth oxide or cobalt oxide.
[0053] Further, in step S200, the method for preheating the green body to be sintered is: heating the green body to be sintered to 500 degrees Celsius, the heating equipment is a muffle furnace, and the heating rate is 2K / min.
[0054] Furthermore, in step S300, the sintered green body is flash-burned by an electric field to obtain a finished resistor chip, and the method for collecting the current density distribution image during the flash burning process is: after applying conductive silver paste on both ends of the green body to be sintered, put it into a flash burning furnace, set the heating rate in the flash burning furnace to 10K / min, and heat it to 600 degrees Celsius; after keeping warm for 15 minutes, open the furnace to cool, connect the two ends of the green body surface to the AC power supply through platinum wires, and then turn on the power to continuously increase the voltage until the flash burning starts, and scan the green body magnetic field distribution image through the Hall effect sensor, convert the magnetic field distribution image into a current density distribution image through an inversion algorithm, record the current density distribution image from the beginning of flash burning and store it on the server until the flash burning ends to obtain the finished resistor chip.
[0055] The current density distribution image is a three-dimensional graph.
[0056] Further, in step S301, when the resistor obtained by flash burning is a defective resistor, the method for calculating the low-pass regression degree according to the current density distribution image is:
[0057] At any time, the current density distribution image obtained is an inversion map, and the pixel value corresponding to each pixel in the inversion map is the inversion value; the lower quartile value of each inversion value in the inversion map is recorded as the low-pass threshold of the inversion map, and when the inversion value of the pixel is less than the low-pass threshold, the pixel is defined as a low-pass marker point; the low-pass phase of the low-pass marker point is defined as the difference between the low-pass threshold and its inversion value;
[0058] The fuzzy channel of the low-pass mark point is: the preset channel radius is sr, a parallel line parallel to the electric field direction is drawn through the low-pass mark point, and a cylinder with a radius of sr is drawn with the obtained parallel line as the axis as the fuzzy channel;
[0059] The axial direction of the fuzzy channel includes the front axial direction and the rear axial direction, which respectively represent the two directions of the low-pass marker point along the axis of the fuzzy channel;
[0060] Starting from the low-pass mark point, a fuzzy channel with a length of 2×sr is intercepted along the axial direction of the fuzzy channel as the channel iteration domain. The fuzzy deviation value HVR of the channel iteration domain is: the average value of the low-pass phase of each low-pass mark point in the channel iteration domain is calculated, and the ratio of the obtained average value to the low-pass mark point to which the fuzzy channel belongs is recorded as the fuzzy deviation value;
[0061] With the channel radius as the iteration distance stl, the channel iteration domain is cyclically moved along the axis by stl and the fuzzy deviation value is recalculated. The fuzzy deviation values obtained in each iteration are written into a sequence recorded as the deviation sequence; the first element of the deviation sequence is used to search for the first minimum value that appears and is recorded as the iteration amount nvl; the deviation sub-weight VRWH of the fuzzy channel is calculated according to the fuzzy deviation value:
[0062]
[0063] Where i1 is the accumulated variable, HVR i1 represents the fuzzy deviation value of the iterative domain of the i1th channel, e is a natural constant, Rt_ov(i1) represents the low-pass coverage of the iterative domain of the i1th channel, and the calculation method of the low-pass coverage is: when HVR i1 >1, the low-pass coverage is the ratio of the elements in the set consisting of the inversion values corresponding to the low-pass marker points in the channel iteration domain, whose values are smaller than the inversion values corresponding to the low-pass marker points belonging to the fuzzy channel; when HVR i1 ≤1, the low-pass coverage is 1; then the partial difference weight MVRWH of the low-pass marker point belonging to the fuzzy channel is the sum of the two partial difference sub-weights on different axes;
[0064] For any pixel in the inversion map as the current pixel, identify the moment when the pixel is used as a low-pass marker point during the flash process, and record any continuous moments as low-pass marker points as a low-pass event. The maximum value of each deviation weight obtained under the low-pass event is recorded as a low-pass scalar. The number of moments included in the low-pass event is the low-pass duration value. The low-pass scalar and the low-pass duration value are combined into a binary group recorded as a low-pass feature group. The set composed of each low-pass feature group of the current pixel is recorded as a low-pass set. The low-pass set is linearly fitted by the polyfit function and the slope value is obtained, which is recorded as the low-pass regression degree.
[0065] The reason for having two partial weights is that the fuzzy channel has two axes, so the fuzzy channel obtains the partial weight twice. The current axis means that the fuzzy channel has two axes, namely the front axis and the back axis.
[0066] Further, in step S302, the method for judging whether the defective resistor chip meets the requirements of the secondary sintering treatment in combination with the low-pass regression degree is: performing Z-score method outlier identification on all low-pass regression degrees obtained from the inversion map, and presetting the ratio value FRT, and the FRT is set to 1%; if the ratio of the number of identified outliers to the total number of pixels in the inversion map is greater than or equal to FRT, it is judged that it does not meet the requirements of the secondary sintering treatment, and the identification result is sent to the server; otherwise, it is judged that it meets the requirements of the secondary sintering treatment, and the defective resistor chip is subjected to conventional sintering, and the identification result is sent to the server.
[0067] Embodiment 2:
[0068] The implementation steps of Example 2 are the same as those of Example 1, except that, in step S301, when the resistor obtained by flash burning is a defective resistor, the method for calculating the low-pass regression degree according to the current density distribution image is replaced by:
[0069] At any time, the current density distribution image obtained is the inversion map, and the pixel value corresponding to each pixel in the inversion map is the inversion value; the range of the inversion value of any pixel in the flash burning process is calculated and recorded as the inversion. The inversion map is segmented into regions according to the inversion amplitude through the superpixel segmentation algorithm, and each region obtained by segmentation is a deconstruction unit;
[0070] Define the average value of each inversion value in the deconstruction unit at any time as the unit inversion value UAri, and the standard deviation of the inversion amplitude corresponding to each pixel in the deconstruction unit as σ, then the derivative rate interval UAZ of the deconstruction unit is: UAZ∈[UAri·(1-σ),UAri·(1+σ)]; take any deconstruction unit as the current deconstruction unit, initialize an area as the mixed unit, set a numerical variable as the iteration stp, which is initially 1; set its starting area as the current deconstruction unit, search for each deconstruction unit adjacent to the mixed unit as the neighboring deconstruction unit, and the derivative vector EUA of the neighboring deconstruction unit is: EUA=UAri / λ stp , where λ is the convergence coefficient, λ∈[1,e]; the mixing condition of the adjacent deconstruction unit is defined as UAri ps <UAZ; When the adjacent deconstruction unit meets the mixed condition, it is merged into the mixed unit; repeat the iteration to merge new adjacent deconstruction units into the mixed unit, and increase the number of iterations by 1 at each iteration until the number of adjacent deconstruction units merged into the mixed unit at the current iteration is 0;
[0071] Set a time length as the retention period TS, the intersection of all the mixed units in the TS period from the current deconstruction unit at any time to its reverse time direction is the hysteresis mixing domain, the range of the inversion value of each structural unit corresponding to the hysteresis mixing domain at this time is the hysteresis mixing distance MTDS, and define the ratio of the intersection number of the mixed unit and the deconstruction unit of the hysteresis mixing domain at this time to the number of deconstruction units in the hysteresis mixing domain as the hybrid composite ratio kurt; the flash burning process obtains all the hybrid composite ratio write sequences recorded as kurt.Ls;
[0072] Define the ratio of the inversion value of the current deconstruction unit at any moment before the TS period to the unit at that moment as the retention amplitude KU. When KU>1, it is defined that the moment meets the low-pass amplitude; the range of the inversion value of each unit obtained from the current deconstruction unit at any moment to the previous TS period is recorded as the sub-deconstruction distance SUDS; calculate the hybrid weight MUWH of the current deconstruction unit:
[0073]
[0074] Where j1 and j2 are accumulated variables, hs<> is the harmonic mean function, which returns the harmonic mean of the calling sequence; ln() is the logarithmic function with the natural constant e as the base; nrku is the number of moments that meet the low-pass amplitude, kurt j2Represents the ratio of the hybrid structure that meets the low-pass amplitude at the j2nd moment; MTDS j1 and SUDS j1 They represent the hysteresis distance and deconstruction distance of the j1th low-pass amplitude moment respectively; KU j1 represents the retention amplitude at the j1th moment that meets the low-pass amplitude;
[0075] The set of inversion values corresponding to all pixels in the hysteresis domain obtained by the current deconstruction unit at the end of the flash is recorded as ClssT, and the product of the percentile of the inversion value corresponding to any pixel in the current deconstruction unit in ClssT and the hybrid weight is defined as the low-pass regression degree of the pixel;
[0076] Where e is a natural constant; UAri ps Refers to the unit inversion value of the adjacent deconstruction unit; in the spatial description, two regions are adjacent when the edge lines or edge surfaces of the two regions overlap. In the calculation process of the hybrid weight, when j1 and j2 take the value of 1, it represents the moment when the flash burn ends;
[0077] Table 1: Determination effect of secondary sintering of defective resistor chips
[0078] Comparative Example Example 1 Example 2 Total repair rate of defective resistor chips 52.24% 77.65% 80.27% Secondary sintering determination accuracy - 77.65% 80.27% Secondary sintering judgment false correctness rate - 73.54% 71.91%
[0079] Table 1 shows the comparison of the effects of secondary sintering judgment on defective resistors, where the comparison ratio is that the defective resistors are not analyzed and all the defective resistors are directly subjected to conventional sintering. The total repair rate of defective resistors in the table represents the ratio of the number of resistors that become genuine products after secondary sintering to the number of defective resistors that participate in the secondary sintering. The true accuracy rate of secondary sintering judgment refers to the proportion of defective resistors that are judged to meet the requirements for secondary sintering of defective resistors and are sintered into genuine resistors. The false accuracy rate of secondary sintering judgment refers to the proportion of defective resistors that cannot be sintered into genuine resistors among those that are judged to be unqualified for secondary sintering of defective resistors. It can be seen from the above table that the secondary sintering judgment by this method will greatly improve the resource utilization efficiency of defective resistors during the flash burning process, avoid the consumption of unnecessary processing resources for products that cannot be processed, and has great significance for production costs and waste utilization.
[0080] An embodiment of the present invention provides a resistor manufacturing system, such as Figure 2 The figure shows a structure diagram of a resistor preparation system of the present invention. The resistor preparation system of this embodiment includes: a processor, a memory, and a computer program stored in the memory and executable on the processor. When the processor executes the computer program, the steps in the above-mentioned resistor preparation method embodiment are implemented.
[0081] The system comprises: a memory, a processor, and a computer program stored in the memory and executable on the processor, wherein the processor executes the computer program to run in the following units of the system:
[0082] A material mixing unit, used for uniformly mixing the resistor raw materials to form a green body to be sintered;
[0083] A preheating unit, used for preheating the green body to be sintered;
[0084] A flash burning data acquisition unit is used to flash burn the sintered green body through an electric field to obtain a finished resistor sheet and to collect a current density distribution image during the flash burning process;
[0085] A distribution image analysis unit is used to calculate the low-pass regression degree according to the current density distribution image when the resistor obtained by flash burning is a defective resistor;
[0086] The server feedback unit is used to judge whether the defective resistor chips meet the requirements of secondary sintering treatment in combination with the low-pass regression.
[0087] The resistor preparation system can be run in computing devices such as desktop computers, laptops, PDAs, and cloud servers. The resistor preparation system can include, but is not limited to, a processor and a memory. Those skilled in the art will appreciate that the example is only an example of a resistor preparation system and does not constitute a limitation on a resistor preparation system. It can include more or fewer components than the example, or a combination of certain components, or different components. For example, the resistor preparation system can also include input and output devices, network access devices, buses, etc.
[0088] The processor may be a central processing unit (CPU), or other general-purpose processors, digital signal processors (DSP), application-specific integrated circuits (ASIC), field-programmable gate arrays (FPGA) or other programmable logic devices, discrete gate or transistor logic devices, discrete hardware components, etc. The general-purpose processor may be a microprocessor or any conventional processor, etc. The processor is the control center of the operating system of the resistor preparation system, and uses various interfaces and lines to connect the various parts of the entire resistor preparation system operating system.
[0089] The memory can be used to store the computer program and / or module, and the processor realizes various functions of the preparation system of the resistor by running or executing the computer program and / or module stored in the memory, and calling the data stored in the memory. The memory can mainly include a program storage area and a data storage area, wherein the program storage area can store an operating system, an application required for at least one function (such as a sound playback function, an image playback function, etc.), etc.; the data storage area can store data created according to the use of the mobile phone (such as audio data, a phone book, etc.), etc. In addition, the memory can include a high-speed random access memory, and can also include a non-volatile memory, such as a hard disk, a memory, a plug-in hard disk, a smart memory card (Smart Media Card, SMC), a secure digital (Secure Digital, SD) card, a flash card (Flash Card), at least one disk storage device, a flash memory device, or other volatile solid-state storage devices.
[0090] Although the description of the present invention has been quite detailed and has been described in particular with respect to several described embodiments, it is not intended to be limited to any of these details or embodiments or any particular embodiment, so as to effectively cover the intended scope of the present invention. In addition, the present invention is described above with the embodiments foreseeable by the inventors, and its purpose is to provide a useful description, and those non-substantial changes to the present invention that are not currently foreseen may still represent equivalent changes of the present invention.
Claims
1. A method for preparing a resistor, characterized in that: The method comprises the following steps: S100, uniformly mixing the resistor raw materials to form a green body to be sintered; S200, preheating the green body to be sintered; S300, flash-burning the green body to be sintered by an electric field to obtain a finished resistor sheet, and collecting a current density distribution image during the flash-burning process; S301, when the resistor obtained by flash burning is a defective resistor, a low-pass regression degree is calculated according to the current density distribution image; S302, combining low-pass regression to determine whether the defective resistor meets the secondary sintering treatment requirements; Among them, in S301, the method for calculating the low-pass regression degree according to the current density distribution image is: obtaining a low-pass marking point according to the pixel value comparison of the current density distribution image, and calculating its low-pass phase, dividing the fuzzy channel in combination with the spatial position of the low-pass marking point, iteratively allocating the channel iteration domain in the fuzzy channel according to the preset iteration distance, calculating the fuzzy deviation value according to the low-pass phase of the channel iteration domain, calculating the deviation weight of the fuzzy channel according to the fuzzy deviation value, defining a low-pass event according to the occurrence continuity of the low-pass marking point in the pixel flash process, obtaining a low-pass feature group according to the low-pass event, and calculating the low-pass regression degree through the low-pass feature group; In step S301, when the resistor obtained by flash burning is a defective resistor, the method of calculating the low-pass regression degree according to the current density distribution image is: for any time, the current density distribution image obtained is an inversion map, and the pixel value corresponding to each pixel in the inversion map is an inversion value; the lower quartile value of each inversion value in the inversion map is recorded as the low-pass threshold of the inversion map, and when the inversion value of the pixel is less than the low-pass threshold, the pixel is defined as a low-pass marking point; the low-pass phase of the low-pass marking point is defined as the difference between the low-pass threshold and its inversion value; The fuzzy channel of the low-pass mark point is: the preset channel radius is sr, a parallel line parallel to the electric field direction is drawn through the low-pass mark point, and a cylinder with a radius of sr is drawn with the obtained parallel line as the axis as the fuzzy channel; The axial direction of the fuzzy channel includes the front axial direction and the rear axial direction, which respectively represent the two directions of the low-pass marker point along the axis of the fuzzy channel; Starting from the low-pass mark point, a fuzzy channel with a length of 2×sr is intercepted along the axial direction of the fuzzy channel as the channel iteration domain. The fuzzy deviation value HVR of the channel iteration domain is: the average value of the low-pass phase of each low-pass mark point in the channel iteration domain is calculated, and the ratio of the obtained average value to the low-pass mark point to which the fuzzy channel belongs is recorded as the fuzzy deviation value; Taking the channel radius as the iteration distance stl, the channel iteration domain is cyclically moved along the axial direction by stl and the fuzzy deviation value is recalculated. The fuzzy deviation values obtained in each iteration are written into a sequence recorded as the deviation sequence; the first element of the deviation sequence is used to search for the first minimum value that appears and is recorded as the iteration amount nvl; the deviation sub-weight of the fuzzy channel is calculated according to the fuzzy deviation value, and the deviation weight MVRWH of the low-pass mark point belonging to the fuzzy channel is the sum of the two deviation sub-weights on different axes; For any pixel in the inversion map as the current pixel, identify the moment when the pixel is used as a low-pass marker point during the flash process, and record any continuous moments as low-pass marker points as a low-pass event. The maximum value of each deviation weight obtained under the low-pass event is recorded as a low-pass scalar. The number of moments included in the low-pass event is the low-pass duration value. The low-pass scalar and the low-pass duration value are combined into a binary group recorded as a low-pass feature group. The set composed of each low-pass feature group of the current pixel is recorded as a low-pass set. The low-pass set is linearly fitted by the polyfit function and the slope value is obtained, which is recorded as the low-pass regression degree.
2. The method for preparing a resistor according to claim 1, characterized in that: In step S100, the method of uniformly mixing the resistor raw materials to form a green body to be sintered is: the raw materials are mixed using a ball mill or a high-speed mixer, the mixed resistor raw materials are put into a mold, and the green body to be sintered is obtained by pressing with a tablet press.
3. The method for preparing a resistor according to claim 1, characterized in that: In step S200, the method for preheating the green body to be sintered is: heating the green body to be sintered to 30%-50% of the sintering temperature, the heating equipment is a muffle furnace, and the heating rate is 2K / min-3K / min; if the sintering temperature is not specified, it is heated to 500 degrees Celsius by default.
4. The method for preparing a resistor according to claim 1, characterized in that: In step S300, the sintered green body is flash-burned by an electric field to obtain a finished resistor chip. The method for collecting the current density distribution image during the flash-burning process is as follows: after applying conductive silver paste on both ends of the green body to be sintered, the green body is placed in a flash-burning furnace, and the heating rate in the flash-burning furnace is set to 10K / min, and the temperature is raised to 600 degrees Celsius; After keeping warm for 15 to 20 minutes, open the furnace to cool, connect the two ends of the embryo body to the AC power supply through platinum wire, then turn on the power and continuously increase the voltage until flash burning begins, and scan the embryo body magnetic field distribution image through the Hall effect sensor, and convert the magnetic field distribution image into a current density distribution image through the inversion algorithm. Record the current density distribution image from the beginning of flash burning and store it in the server until the flash burning ends to obtain the finished resistor.
5. The method for preparing a resistor according to claim 1, characterized in that: In step S301, the method for determining whether the resistor obtained by flash burn is a defective resistor is: performing a DC resistance test and a volt-ampere characteristic test on the resistor respectively, and defining the resistor obtained by flash burn as a defective resistor if it fails any one of the tests.
6. The method for preparing a resistor according to claim 1, characterized in that: In step S301, when the resistor obtained by flash burning is a defective resistor, the method of calculating the low-pass regression degree according to the current density distribution image can be replaced by: for any time, the current density distribution image obtained is an inversion map, and the pixel value corresponding to each pixel in the inversion map is an inversion value; the range of the inversion value of any pixel in the flash burning process is calculated and recorded as the inversion; the inversion map is segmented into regions according to the inversion amplitude through the super pixel segmentation algorithm, and each region obtained by segmentation is a deconstruction unit; Define the average value of each inversion value in the deconstruction unit at any time as the unit inversion value UAri, and the standard deviation of the inversion amplitude corresponding to each pixel in the deconstruction unit as σ, then the derivative rate interval UAZ of the deconstruction unit is: UAZ∈[UAri·(1-σ),UAri·(1+σ)]; take any deconstruction unit as the current deconstruction unit, initialize an area as the mixed unit, set a numerical variable as the iteration stp, which is initially 1; set its starting area as the current deconstruction unit, search for each deconstruction unit adjacent to the mixed unit as the neighboring deconstruction unit, and the derivative vector EUA of the neighboring deconstruction unit is: EUA=UAri / λ stp , where λ is the convergence coefficient, λ∈[1,e]; the mixing condition of the adjacent deconstruction unit is defined as UAri ps <UAZ; When the adjacent deconstruction unit meets the mixing condition, it is merged into the mixed unit; the iteration is repeated to merge new adjacent deconstruction units into the mixed unit, and the number of iterations is increased by 1 at each iteration until the number of adjacent deconstruction units merged into the mixed unit at the current iteration is 0; Set a time length as the retention period TS, the intersection of all the mixed units in the TS period from the current deconstruction unit at any time to its reverse time direction is the hysteresis mixing domain, the range of the inversion value of each structural unit corresponding to the hysteresis mixing domain at this time is the hysteresis mixing distance MTDS, and define the ratio of the intersection number of the mixed unit and the deconstruction unit of the hysteresis mixing domain at this time to the number of deconstruction units in the hysteresis mixing domain as the hybrid composite ratio kurt; the flash burning process obtains all the hybrid composite ratio write sequences recorded as kurt.Ls; The ratio of the current deconstruction unit at any moment before the TS period to the unit inversion value at that moment is defined as the retention amplitude KU. When KU>1, it is defined that the moment meets the low-pass amplitude. The range of the inversion value of each unit obtained from the current deconstruction unit at any moment to the previous TS period is recorded as the sub-deconstruction distance SUDS. The mixing weight MUWH of the current deconstruction unit is calculated according to the mixing distance and deconstruction distance at the moment meeting the low-pass amplitude: The set of inversion values corresponding to all pixels in the hysteresis domain obtained by the current deconstruction unit at the end of the flash is recorded as ClssT, and the product of the percentile of the inversion value corresponding to any pixel in the current deconstruction unit in ClssT and the mixing weight is defined as the low-pass regression degree of the pixel.
7. The method for preparing a resistor according to claim 1, characterized in that: In step S302, the method of judging whether the defective resistor chip meets the requirements of the secondary sintering treatment in combination with the low-pass regression degree is: performing Z-score method outlier identification on all low-pass regression degrees obtained from the inversion diagram, and presetting the ratio value FRT, FRT∈[0.5%-3%]; If the ratio of the number of identified abnormal values to the total number of pixels in the inversion map is greater than or equal to FRT, it is judged that it does not meet the requirements of secondary sintering treatment, and the identification result is sent to the server. Otherwise, it is judged that it meets the requirements of secondary sintering treatment, and the defective resistor is subjected to secondary flash sintering or conventional sintering, and the identification result is sent to the server.
8. A resistor preparation system, characterized in that: The resistor preparation system includes: a processor, a memory, and a computer program stored in the memory and executable on the processor. When the processor executes the computer program, the steps in the resistor preparation method described in any one of claims 1 to 7 are implemented. The resistor preparation system runs on a desktop computer, a laptop computer, a PDA, and a computing device in a cloud data center.
Citation Information
Patent Citations
Presintering method of zinc oxide piezoresistor piece
CN107256747A
Ceramic room-temperature sintering method
CN113307624A