Light-emitting diode epitaxial wafer and preparation method thereof, and light-emitting diode
By using a specific stacked structure and material combination in GaN-based light-emitting diodes to form a polarization electric field and a high-efficiency electron blocking layer, the Efficiency Droop problem is solved and the luminous efficiency of the light-emitting diode is improved under different currents.
Patent Information
- Application Number
- CN202411035811.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The problem of reduced luminous efficiency of GaN-based light-emitting diodes when the injected current increases is called Efficiency Droop, which is mainly related to electron leakage. Existing methods such as replacing the barrier layer will cause the crystal quality of other quantum well layers to decrease or the barrier to be too low. Difficulty confining holes and electrons.
The sequentially stacked AlxGa1-xN, InyGa1-yN, InzGa1-zN and GaN layers are used as the last barrier layer to form a polarization electric field to consume electrons, and β-Ta2O5 is introduced as the electron blocking layer, combined with a multi-layer P-type GaN structure to improve hole injection efficiency.
It effectively reduces the probability of electron escape and ensures high luminous efficiency. Especially at lower current densities, it improves the luminous efficiency of light-emitting diodes.
Smart Images

Figure CN118572003B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor optoelectronic devices, and in particular to a light emitting diode epitaxial wafer and a preparation method thereof, and a light emitting diode. Background Art
[0002] GaN-based light-emitting diodes generally use InGaN-GaN heterojunctions as quantum well regions. They have advantages such as high luminous efficiency and are currently the most widely used LEDs. However, there are still some phenomena that limit their performance improvement. One of them is the phenomenon that the luminous efficiency decreases with the increase of the injected current, which is generally called the problem of Efficiency Droop. Studies have shown that Efficiency Droop has a strong correlation with leakage electrons. Since P-type AlGaN is generally used as an electron blocking layer in GaN-based light-emitting diodes, the lattice mismatch between the barrier layer (GaN) and the electron blocking layer will form a polarization electric field, generate positive charges, and then reduce the barrier of P-type AlGaN, resulting in electron leakage. The commonly used method is to replace the last barrier layer with a stacked structure of GaN and p-type InGaN, but this structure will cause Mg to diffuse into other quantum well layers, reducing the crystal quality of other quantum well layers. If there is too much In in p-type InGaN, it will cause the barrier to be too low, making it difficult to confine holes and electrons to the active area, which will also reduce the luminous efficiency. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a light emitting diode epitaxial wafer and a preparation method thereof, which can improve the light emitting efficiency of the light emitting diode under different light emitting currents.
[0004] In order to solve the above problems, the present invention discloses a light-emitting diode epitaxial wafer, which comprises a substrate, a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer and a P-type GaN layer sequentially stacked on the substrate;
[0005] The multi-quantum well layer comprises a first multi-quantum well layer, a final well layer and a final barrier layer sequentially stacked on the N-type GaN layer, the first multi-quantum well layer is a periodic structure formed by alternating stacking of quantum well layers and quantum barrier layers, the quantum well layer and the final well layer are both InGaN quantum well layers, and the quantum barrier layer is a GaN quantum barrier layer;
[0006] The final barrier layer includes Al x Ga 1-x N-layer, In y Ga 1-y N-layer, In z Ga 1-zN layer and GaN layer; wherein, the value range of x is 0.05~0.3, the value range of y is 0.01~0.1, the value range of z is 0.01~0.1, and z>y;
[0007] The electron blocking layer is a β-Ta2O5 layer;
[0008] The P-type GaN layer includes a first P-type GaN layer, a P-type In layer, and a α Ga 1-α N layer and a second P-type GaN layer, wherein the value range of α is 0.08~0.15.
[0009] As an improvement of the above technical solution, the Al x Ga 1-x The thickness of the N layer is 3nm~8nm, and the value of x ranges from 0.1~0.2; and / or
[0010] In y Ga 1-y The thickness of the N layer is 1 nm to 3 nm, and the value of y is in the range of 0.02 to 0.04; and / or
[0011] In z Ga 1-z The thickness of the N layer is 1 nm to 3 nm, and the value of z is in the range of 0.05 to 0.1; and / or
[0012] The thickness of the GaN layer is 2nm~6nm.
[0013] As an improvement of the above technical solution, the thickness of the electron blocking layer is 20nm~50nm; and / or
[0014] The thickness of the first P-type GaN layer is 20nm~100nm, and the P-type doping concentration is 1×10 19 cm -3 ~1×10 20 cm -3 ; and / or
[0015] The P-type α Ga 1-α The thickness of the N layer is 10nm~30nm, and the P-type doping concentration is 1×10 17 cm -3 ~1×10 19 cm -3 ; and / or
[0016] The thickness of the second P-type GaN layer is 50nm~150nm, and the P-type doping concentration is 1×10 20 cm -3 ~1×1021 cm -3 .
[0017] As an improvement of the above technical solution, the Al x Ga 1-x The thickness of the N layer is y Ga 1-y 1.5~3 times the thickness of the N layer.
[0018] As an improvement of the above technical solution, the thickness of the GaN layer is z Ga 1-z 1.2~2 times the thickness of the N layer.
[0019] As an improvement of the above technical solution, the In component ratio in the quantum well layer and the final well layer is 0.1-0.2, and the thickness thereof is 3nm-5nm;
[0020] The thickness of the quantum barrier layer is 5nm-15nm.
[0021] Correspondingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which is used to prepare the above-mentioned light-emitting diode epitaxial wafer, and comprises:
[0022] Providing a substrate, and sequentially growing a buffer layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer and a P-type GaN layer on the substrate;
[0023] The multi-quantum well layer comprises a first multi-quantum well layer, a final well layer and a final barrier layer sequentially stacked on the N-type GaN layer, the first multi-quantum well layer is a periodic structure formed by alternating stacking of quantum well layers and quantum barrier layers, the quantum well layer and the final well layer are both InGaN quantum well layers, and the quantum barrier layer is a GaN quantum barrier layer;
[0024] The final barrier layer includes Al x Ga 1-x N-layer, In y Ga 1-y N-layer, In z Ga 1-z N layer and GaN layer; wherein, the value range of x is 0.05~0.3, the value range of y is 0.01~0.1, the value range of z is 0.01~0.1, and z>y;
[0025] The electron blocking layer is a β-Ta2O5 layer;
[0026] The P-type GaN layer includes a first P-type GaN layer, a P-type In layer, and a α Ga 1-αN layer and a second P-type GaN layer, wherein the value range of α is 0.08~0.15.
[0027] As an improvement of the above technical solution, the growth temperature of the quantum well layer and the final well layer is 740° C. to 820° C., and the growth pressure is 100 torr to 300 torr; and / or
[0028] The growth temperature of the quantum barrier layer and the final barrier layer is 850° C. to 950° C., and the growth pressure is 100 torr to 300 torr; and / or
[0029] The growth temperature of the electron blocking layer is 800° C. to 900° C., and the growth pressure is 10 torr to 100 torr; and / or
[0030] The growth temperature of the first P-type GaN layer and the second P-type GaN layer is 900° C. to 1000° C., and the growth pressure is 100 torr to 500 torr; and / or
[0031] The P-type α Ga 1-α The growth temperature of the N layer is 750°C~850°C, and the growth pressure is 100torr~500torr.
[0032] As an improvement of the above technical solution, after the growth of the electron blocking layer is completed, annealing is performed at 900° C. to 950° C. in air or oxygen atmosphere for 10 min to 30 min.
[0033] Correspondingly, the present invention also discloses a light emitting diode, which includes the light emitting diode epitaxial wafer mentioned above.
[0034] The implementation of the present invention has the following beneficial effects:
[0035] In the light emitting diode epitaxial wafer of the present invention, one is to sequentially stack Al x Ga 1-x N-layer, In y Ga 1-y N-layer, In z Ga 1-z N layer and GaN layer are used as the final barrier layer, Al x Ga 1-x N-layer-In y Ga 1-y N-layer interface, In z Ga 1-zThe interface between the N layer and the GaN layer will generate a polarization electric field due to the polarization effect, and then generate negative charges at the interface, which is convenient for consuming electrons and reduces the probability of electron escape. Furthermore, the final barrier layer of the present invention does not introduce Mg doping, does not destroy the quantum well layer structure, and ensures high luminescence efficiency at a lower current density. Second, a β-Ta2O5 layer is introduced on the GaN layer as an electron blocking layer. The lattice mismatch between the GaN (0001) plane and the 010 crystal phase of β-Ta2O5 is less than 3%. Therefore, the final barrier layer has a very weak effect on the electron blocking layer, and the band gap width of β-Ta2O5 reaches about 4.4eV. The combination of the two makes the electron blocking layer have a good electron blocking effect. Third, the P-type GaN layer of the present invention includes a first P-type GaN layer, a P-type In layer, and a plurality of P-type GaN layers stacked in sequence. α Ga 1-α N layer and the second P-type GaN layer, the lower barrier P-type In α Ga 1-α The N layer can store holes, while the first P-type GaN layer and the P-type In α Ga 1-α The heterojunction formed by the N layer and the second P-type GaN layer can effectively accelerate holes and improve the efficiency of hole injection into the multi-quantum well layer. In summary, the light-emitting diode epitaxial wafer of the present invention can effectively improve the light-emitting efficiency under various current densities. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 is a schematic structural diagram of a light emitting diode epitaxial wafer in one embodiment of the present invention;
[0037] Figure 2 It is a flow chart of a method for preparing a light emitting diode epitaxial wafer in one embodiment of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.
[0039] refer to Figure 1 The present invention discloses a light-emitting diode epitaxial wafer, which includes a substrate 100, a buffer layer 200, a non-doped GaN layer 300, an N-type GaN layer 400, a multi-quantum well layer 500, an electron blocking layer 600 and a P-type GaN layer 700, which are sequentially stacked on the substrate 100. The multi-quantum well layer 500 includes a first multi-quantum well layer 510, a final well layer 520 and a final barrier layer 530 sequentially stacked on the N-type GaN layer 400; the first multi-quantum well layer 510 is a periodic structure composed of quantum well layers 511 and quantum barrier layers 512 alternately stacked. The final barrier layer 530 includes Al2O3 sequentially stacked on the final well layer 520. x Ga 1-x N layer 531, In y Ga1-y N layer 532, In z Ga 1-z N layer 533 and GaN layer 534; Based on the above-mentioned last barrier layer 530, on the one hand, Al x Ga 1-x N layer 531, In y Ga 1-y The N layer 532 has a higher concentration of interface polarization charge, which can more effectively prevent electron leakage; z Ga 1-z The N layer 533 and the GaN layer 534 serve as a transition to avoid a large lattice mismatch with the subsequent electron blocking layer 600 (β-Ta2O5 layer). x Ga 1-x The N layer 531 also prevents carriers from overflowing from the end well layer 520 and reducing the light-emitting efficiency.
[0040] Among them, Al x Ga 1-x The ratio of Al component in the N layer 531 (ie, x) is 0.05-0.3, exemplarily 0.08, 0.13, 0.18, 0.24, 0.25 or 0.29, but not limited thereto, and preferably 0.1-0.2.
[0041] Al x Ga 1-x The thickness of the N layer 531 is 3 nm to 10 nm, and is exemplarily 3.5 nm, 5 nm, 6.5 nm, 8 nm or 9.5 nm, but is not limited thereto, and is preferably 3 nm to 8 nm.
[0042] Among them, y Ga 1-y The proportion of In component in N layer 532 (i.e., y) is 0.01-0.1. If y<0.01, less negative charge is generated by polarization. If y>0.1, the overall barrier height of the last barrier layer 530 is too low, and it is difficult to effectively confine carriers in the last well layer 520 for recombination. Exemplarily, y is 0.02, 0.04, 0.06, or 0.08, but not limited thereto. Preferably, y is 0.02-0.04.
[0043] In y Ga 1-y The thickness of the N layer 532 is 1 nm to 5 nm, and is exemplarily 1.2 nm, 1.5 nm, 1.8 nm, 2.2 nm, 2.6 nm, 3 nm, 3.7 nm or 4.4 nm, but is not limited thereto. Preferably, it is 1 nm to 3 nm.
[0044] Among them, z Ga1-z The proportion of In component in N layer 533 (i.e., z) is 0.01-0.1. The present invention controls y<z≤0.1 to prevent the barrier height of the last barrier layer 530 from being too low. Exemplarily, z is 0.02, 0.04, 0.06, or 0.08, but is not limited thereto. Preferably, z is 0.05-0.1.
[0045] In z Ga 1-z The thickness of the N layer 533 is 1 nm to 5 nm, and is exemplarily 1.2 nm, 1.5 nm, 1.8 nm, 2.2 nm, 2.6 nm, 3 nm, 3.7 nm or 4.4 nm, but is not limited thereto. Preferably, it is 1 nm to 3 nm.
[0046] The thickness of the GaN layer 534 is 2 nm to 8 nm, exemplarily 3 nm, 5 nm, 7 nm or 8 nm, but not limited thereto, preferably 2 nm to 6 nm.
[0047] Among them, the electron blocking layer 600 is a β-Ta2O5 layer, which has a high potential barrier and a small lattice mismatch with the GaN layer 534, which greatly improves the blocking effect on electrons and improves the luminous efficiency of the light-emitting diode at various current densities.
[0048] The thickness of the electron blocking layer 600 is 20 nm to 80 nm, and is exemplarily 22 nm, 28 nm, 34 nm, 40 nm, 50 nm, 60 nm or 75 nm, but is not limited thereto, and is preferably 20 nm to 50 nm.
[0049] The P-type GaN layer 700 includes a first P-type GaN layer 710, a P-type In layer 720, and a P-type GaN layer 730, which are sequentially stacked on the electron blocking layer 600. α Ga 1-α N layer 720 and second P-type GaN layer 730. Based on this P-type GaN layer 700, a P-type In α Ga 1-α The N layer 720 can store holes. The heterojunction formed by the P-type GaN layer 700 can effectively accelerate holes and improve the efficiency of hole injection into the multi-quantum well layer.
[0050] The thickness of the first P-type GaN layer 710 is 20 nm to 200 nm, and is exemplarily 30 nm, 50 nm, 70 nm, 90 nm, 120 nm or 180 nm, but is not limited thereto. Preferably, the thickness of the first P-type GaN layer 710 is 20 nm to 100 nm.
[0051] The P-type doping concentration of the first P-type GaN layer 710 is 1×10 19 cm -3 ~3×1020 cm -3 ; preferably 1×10 19 cm -3 ~1×10 20 cm -3 .
[0052] Among them, P-type In α Ga 1-α The ratio of the In component in the N layer 720 (ie, α) is 0.08-0.15, and is 0.09, 0.11, 0.13 or 0.14, but not limited thereto, and preferably 0.1-0.15.
[0053] P-type In α Ga 1-α The thickness of the N layer 720 is 10 nm to 50 nm, and is exemplarily 12 nm, 20 nm, 28 nm, 36 nm or 44 nm, but is not limited thereto, and is preferably 10 nm to 30 nm.
[0054] P-type In α Ga 1-α The P-type doping concentration in the N layer 720 is 1×10 17 cm -3 ~5×10 19 cm -3 , preferably 1×10 17 cm -3 ~1×10 19 cm -3 .
[0055] The thickness of the second P-type GaN layer 730 is 50 nm to 200 nm, preferably 50 nm to 150 nm. The P-type doping concentration of the second P-type GaN layer 730 is 8×10 19 cm -3 ~1×10 21 cm -3 ; preferably 1×10 20 cm -3 ~1×10 21 cm -3 .
[0056] Preferably, in one embodiment of the present invention, Al x Ga 1-x The thickness of the N layer 531 is In y Ga 1-y The thickness of the N layer 532 is 1.5 to 3 times of that of the N layer 532. Based on this thickness ratio, the probability of electron leakage can be further reduced.
[0057] Preferably, in one embodiment of the present invention, the thickness of the GaN layer 534 is Inz Ga 1-z The thickness of the N layer 533 is 1.2 to 2 times of that of the N layer 533. Based on this thickness ratio, the probability of electron leakage can be further reduced.
[0058] The quantum well layer 511 and the final well layer 520 are the same, both are InGaN quantum well layers, and the In component ratio is 0.1-0.35, preferably 0.1-0.2. The thickness of the quantum well layer 511 and the final well layer 520 is 3nm-5nm.
[0059] The quantum barrier layer 512 is a GaN quantum barrier layer, and its thickness is 5 nm to 15 nm, preferably 8 nm to 15 nm.
[0060] The period number of the first multi-quantum well layer 510 is 3-15, preferably 5-15, and more preferably 8-15.
[0061] The substrate 100 is a sapphire substrate, a silicon substrate or a silicon carbide substrate, but is not limited thereto.
[0062] The buffer layer 200 is an AlN layer or an AlGaN layer, but is not limited thereto. The buffer layer 200 has a thickness of 20 nm to 80 nm.
[0063] The thickness of the non-doped GaN layer 300 is 1 μm-3 μm.
[0064] The N-type doping (Si) concentration in the N-type GaN layer 400 is 5×10 18 cm -3 ~5×10 19 cm -3 , thickness is 1μm~5μm.
[0065] Accordingly, reference Figure 2 The present invention also provides a method for preparing a light emitting diode epitaxial wafer, which is used to prepare the light emitting diode epitaxial wafer, and specifically comprises the following steps:
[0066] S1: providing a substrate;
[0067] S2: sequentially growing a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer and a P-type GaN layer on the substrate;
[0068] Preferably, in some embodiments of the present invention, step S2 comprises:
[0069] S21: growing a buffer layer on the substrate;
[0070] The buffer layer may be grown by PVD, MOCVD, MBE or VPE, but is not limited thereto.
[0071] Preferably, in one embodiment of the present invention, an AlN layer is grown by PVD as a buffer layer.
[0072] S22: growing a non-doped GaN layer on the buffer layer;
[0073] The non-doped GaN layer may be grown by PVD, MOCVD, MBE or VPE, but is not limited thereto.
[0074] Preferably, in one embodiment of the present invention, the non-doped GaN layer is grown by MOCVD at a growth temperature of 1100° C. to 1150° C. and a growth pressure of 100 torr to 500 torr.
[0075] S23: growing an N-type GaN layer on the non-doped GaN layer;
[0076] The N-type GaN layer may be grown by MOCVD, MBE or VPE, but is not limited thereto.
[0077] Preferably, in one embodiment of the present invention, the N-type GaN layer is grown by MOCVD; the growth temperature is 1100° C. to 1150° C., and the growth pressure is 100 torr to 500 torr.
[0078] S24: growing a multi-quantum well layer on the N-type GaN layer;
[0079] Specifically, step S24 includes the following steps:
[0080] S241: growing a first multi-quantum well layer on the N-type GaN layer;
[0081] In one embodiment of the present invention, a quantum well layer and a quantum barrier layer are periodically grown on an N-type GaN layer by MOCVD until a multi-quantum well layer is obtained. The growth temperature of the quantum well layer is 740°C to 820°C, and the growth pressure is 100 torr to 300 torr. The growth temperature of the quantum barrier layer is 850°C to 950°C, and the growth pressure is 100 torr to 300 torr.
[0082] S242: growing a final well layer on the first multi-quantum well layer;
[0083] The InGaN quantum well layer may be grown by MOCVD, MBE or VPE as the final well layer, but is not limited thereto.
[0084] Preferably, in one embodiment of the present invention, an InGaN quantum well layer is grown by MOCVD as the final well layer; the growth temperature is 740° C. to 820° C., and the growth pressure is 100 torr to 300 torr.
[0085] S243: growing a final barrier layer on the final well layer to obtain a multi-quantum well layer;
[0086] Specifically, in one embodiment of the present invention, Al is grown on the final well layer in sequence by MOCVD. x Ga 1-x N-layer, In y Ga 1-y N-layer, In z Ga 1-z The N layer and the GaN layer form the final barrier layer;
[0087] Among them, the growth temperature of the last barrier layer is 850℃~950℃, and the growth pressure is 100torr~300torr.
[0088] S25: growing an electron blocking layer on the multi-quantum well layer;
[0089] The β-Ta2O5 layer can be grown by PVD, MOCVD or PLD as an electron blocking layer, but is not limited thereto. Specifically, when MOCVD is used for growth, the Ta source used is Ta(C2H5O)5, the O source is O2, and N2 is used as a carrier gas.
[0090] Preferably, in one embodiment of the present invention, a β-Ta2O5 layer is grown by MOCVD as an electron blocking layer, and the growth temperature is 800°C to 900°C and the growth pressure is 10 torr to 100 torr.
[0091] Preferably, in one embodiment, after the electron blocking layer is grown, annealing is performed at 900° C. to 950° C. in an air or oxygen atmosphere for 10 min to 30 min. Based on the annealing treatment, the crystal quality of the β-Ta2O5 layer can be further improved, and its blocking effect on electrons can be enhanced.
[0092] S26: growing a P-type GaN layer on the electron blocking layer;
[0093] Specifically, in one embodiment of the present invention, a first P-type GaN layer, a P-type In layer, and a second P-type GaN layer are sequentially grown on the electron blocking layer. α Ga 1-α N layer and a second P-type GaN layer, that is, a P-type GaN layer is obtained.
[0094] The growth temperature of the first P-type GaN layer and the second P-type GaN layer is 900°C~1000°C, and the growth pressure is 100torr~500torr; the P-type In α Ga 1-α The growth temperature of the N layer is 750°C~850°C, and the growth pressure is 100torr~500torr.
[0095] The present invention will be further described below with specific embodiments:
[0096] Example 1
[0097] This embodiment provides a light emitting diode epitaxial wafer, which includes a substrate, a buffer layer, an undoped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer and a P-type GaN layer stacked in sequence on the substrate.
[0098] The substrate is a sapphire substrate, the buffer layer is an AlN layer with a thickness of 45 nm, the thickness of the undoped GaN layer is 1.5 μm, and the doping element of the N-type GaN layer is Si with a doping concentration of 8×10 18 cm -3 , and its thickness is 2.5μm.
[0099] The multi-quantum well layer includes a first multi-quantum well layer, a final well layer and a final barrier layer stacked sequentially on the N-type GaN layer. The first multi-quantum well layer is a periodic structure with 9 periods. Each period includes a quantum well layer and a quantum barrier layer stacked sequentially. The quantum well layer is In 0.2 Ga 0.8 N layer, with a thickness of 3nm; the quantum barrier layer is GaN layer, with a thickness of 10nm. The final well layer is In 0.2 Ga 0.8 The thickness of the N layer is 3 nm; the final barrier layer includes Al x Ga 1-x N layer (x=0.15), In y Ga 1-y N layer (y=0.03), In z Ga 1-z N layer (z=0.06) and GaN layer; among them, Al x Ga 1-x The thickness of the N layer is 7nm, and the In y Ga 1-y The thickness of the N layer is 1.5nm, and the In z Ga 1-z The thickness of the N layer is 2nm, the thickness of the GaN layer is 6nm, and the electron blocking layer is a β-Ta2O5 layer with a thickness of 50nm.
[0100] The P-type GaN layer includes a first P-type GaN layer, a P-type In layer, and a α Ga 1-α N layer (α = 0.1) and the second P-type GaN layer. The Mg doping concentration in the first P-type GaN layer is 5×10 19 cm -3 , its thickness is 80nm; P-type In αGa 1-α The Mg doping concentration in the N layer is 3×10 18 cm -3 , its thickness is 20nm; the Mg doping concentration in the second P-type GaN layer is 5×10 20 cm -3 , and its thickness is 80nm.
[0101] The method for preparing the light emitting diode epitaxial wafer in this embodiment comprises the following steps:
[0102] (1) Providing a substrate.
[0103] (2) growing a buffer layer on the substrate;
[0104] Among them, an AlN layer is grown by PVD as a buffer layer;
[0105] (3) growing a non-doped GaN layer on the buffer layer;
[0106] The non-doped GaN layer is grown by MOCVD at a growth temperature of 1120° C. and a growth pressure of 200 torr.
[0107] (4) growing an N-type GaN layer on the undoped GaN layer;
[0108] The N-type GaN layer is grown by MOCVD at a growth temperature of 1140° C. and a growth pressure of 300 torr.
[0109] (5) growing a first multi-quantum well layer on the N-type GaN layer;
[0110] Specifically, quantum well layers and quantum barrier layers are periodically grown on the N-type GaN layer by MOCVD until a first multi-quantum well layer is obtained, wherein the growth temperature of the quantum well layer is 750°C and the growth pressure is 200 torr; the growth temperature of the quantum barrier layer is 890°C and the growth pressure is 200 torr.
[0111] (6) growing a final well layer on the first multi-quantum well layer;
[0112] Specifically, MOCVD is used to deposit In 0.2 Ga 0.8 The N layer is used as the end well layer; its growth temperature is 750°C and the growth pressure is 200 torr.
[0113] (7) growing a final barrier layer on the final well layer;
[0114] Specifically, Al is grown in sequence by MOCVD x Ga 1-x N-layer, In y Ga 1-y N-layer, Inz Ga 1-z N layer and GaN layer; their growth temperature is 890°C and their growth pressure is 200torr.
[0115] (8) growing an electron blocking layer on the final barrier layer;
[0116] Specifically, a β-Ta2O5 layer is grown by MOCVD as an electron blocking layer at a growth temperature of 840° C. and a growth pressure of 20 torr.
[0117] (9) Growing a P-type GaN layer on the electron blocking layer;
[0118] Specifically, in one embodiment of the present invention, a first P-type GaN layer, a P-type In layer, and a second P-type GaN layer are sequentially grown on the electron blocking layer. α Ga 1-α N layer and the second P-type GaN layer, that is, a P-type GaN layer is obtained; wherein the growth temperature of the first P-type GaN layer and the second P-type GaN layer is 920°C and the growth pressure is 200torr. α Ga 1-α The growth temperature of the N layer is 750°C and the growth pressure is 200 torr.
[0119] Example 2
[0120] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 1 in that: x Ga 1-x The thickness of the N layer is 6nm, and the In y Ga 1-y The thickness of the N layer is 2.5 nm.
[0121] The rest are the same as in Example 1.
[0122] Example 3
[0123] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 2 in that:
[0124] In z Ga 1-z The thickness of the N layer is 2.5 nm, and the thickness of the GaN layer is 4.5 nm.
[0125] The rest are the same as in Example 2.
[0126] Example 4
[0127] This embodiment provides a light emitting diode epitaxial wafer, which is different from the embodiment 3 in that:
[0128] After the electron blocking layer is grown, annealing is performed at 930°C in an oxygen atmosphere for 20 min.
[0129] The rest are the same as in Example 1.
[0130] Comparative Example 1
[0131] This comparative example provides a light emitting diode epitaxial wafer, which differs from Example 1 in that:
[0132] The final barrier layer is a GaN layer with a thickness of 10nm; the electron blocking layer is an Al 0.4 Ga 0.6 The N layer has a thickness of 30 nm. The P-type GaN layer consists only of P-type GaN, and its Mg doping concentration is 5×10 20 cm -3 , with a thickness of 200nm.
[0133] In this comparative example, the growth conditions of the final barrier layer are the same as the growth conditions of the quantum barrier layer in Example 1.
[0134] The growth temperature of the electron blocking layer is 1120° C. and the growth pressure is 300 torr. The growth conditions of the P-type GaN layer are the same as those of the first P-type GaN layer in Example 1.
[0135] The rest are the same as in Example 1.
[0136] Comparative Example 2
[0137] This comparative example provides a light emitting diode epitaxial wafer, which differs from Example 1 in that:
[0138] The final barrier layer is a GaN layer with a thickness of 10 nm. Its growth conditions are the same as those of the quantum barrier layer in Example 1.
[0139] The rest are the same as in Example 1.
[0140] Comparative Example 3
[0141] This comparative example provides a light emitting diode epitaxial wafer, which differs from Example 1 in that:
[0142] The electron blocking layer is Al 0.4 Ga 0.6 N layer, with a thickness of 30nm; its growth temperature is 1120℃ and the growth pressure is 300torr.
[0143] The rest are the same as in Example 1.
[0144] Comparative Example 4
[0145] This comparative example provides a light emitting diode epitaxial wafer, which differs from Example 1 in that:
[0146] The electron blocking layer is a δ-Ta2O5 layer; its growth temperature is 750°C and the growth pressure is 20 torr.
[0147] The rest are the same as in Example 1.
[0148] Comparative Example 5
[0149] This comparative example provides a light emitting diode epitaxial wafer, which differs from Example 1 in that:
[0150] The P-type GaN layer consists only of P-type GaN, and its Mg doping concentration is 5×10 20 cm -3 The growth conditions of the P-type GaN layer are the same as those of the first P-type GaN layer in Example 1.
[0151] The rest are the same as in Example 1.
[0152] The light emitting diode epitaxial wafers obtained in Examples 1 to 4 and Comparative Examples 1 to 5 were tested, and the specific method is as follows:
[0153] (1) The epitaxial wafer was made into a 10 mil × 24 mil chip, and its luminous power was tested at 60 mA, 120 mA, and 1 A respectively. The luminous power improvement rate was calculated based on the data of comparative example 1.
[0154] Specifically, the luminous power improvement rate = (luminous power of each embodiment / comparative example-luminous power of comparative example 1) / luminous power of comparative example 1; when calculating, the test current used is the same.
[0155] (2) The internal quantum efficiency of each epitaxial wafer at 60 mA and 120 mA was measured using a PL tester, and the attenuation rate was calculated. Specifically, the attenuation rate = (internal quantum efficiency at 60 mA - internal quantum efficiency at 120 mA) / internal quantum efficiency at 60 mA.
[0156] The specific results are shown in the following table:
[0157]
[0158] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light emitting diode epitaxial wafer, characterized in that: It comprises a substrate, a buffer layer, a non-doped GaN layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer and a P-type GaN layer which are sequentially stacked on the substrate; The multi-quantum well layer comprises a first multi-quantum well layer, a final well layer and a final barrier layer sequentially stacked on the N-type GaN layer, the first multi-quantum well layer is a periodic structure formed by alternating stacking of quantum well layers and quantum barrier layers, the quantum well layer and the final well layer are both InGaN quantum well layers, and the quantum barrier layer is a GaN quantum barrier layer; The final barrier layer includes Al x Ga 1-x N-layer, In y Ga 1-y N-layer, In z Ga 1-z N layer and GaN layer; wherein, the value range of x is 0.05~0.3, the value range of y is 0.01~0.1, the value range of z is 0.01~0.1, and z>y; The electron blocking layer is a β-Ta2O5 layer; The P-type GaN layer includes a first P-type GaN layer, a P-type In layer, and a α Ga 1-α N layer and a second P-type GaN layer, wherein the value range of α is 0.08~0.
15.
2. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The Al x Ga 1-x The thickness of the N layer is 3nm~8nm, and the value of x ranges from 0.1~0.2; and / or In y Ga 1-y The thickness of the N layer is 1 nm to 3 nm, and the value of y is in the range of 0.02 to 0.04; and / or In z Ga 1-z The thickness of the N layer is 1 nm to 3 nm, and the value of z is in the range of 0.05 to 0.1; and / or The thickness of the GaN layer is 2nm~6nm.
3. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the electron blocking layer is 20nm to 50nm; and / or The thickness of the first P-type GaN layer is 20nm~100nm, and the P-type doping concentration is 1×10 19 cm -3 ~1×10 20 cm -3 ; and / or The P-type α Ga 1-α The thickness of the N layer is 10nm~30nm, and the P-type doping concentration is 1×10 17 cm -3 ~1×10 19 cm -3 ; and / or The thickness of the second P-type GaN layer is 50nm-150nm, and the P-type doping concentration is 1×10 20 cm -3 ~1×10 21 cm -3 .
4. The light emitting diode epitaxial wafer according to any one of claims 1 to 3, characterized in that: The Al x Ga 1-x The thickness of the N layer is y Ga 1-y 1.5~3 times the thickness of the N layer.
5. The light emitting diode epitaxial wafer according to any one of claims 1 to 3, characterized in that: The thickness of the GaN layer is z Ga 1-z 1.2~2 times the thickness of the N layer.
6. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The In component ratio in the quantum well layer and the final well layer is 0.1-0.2, and the thickness thereof is 3nm-5nm; The thickness of the quantum barrier layer is 5nm-15nm.
7. A method for preparing a light emitting diode epitaxial wafer, for preparing the light emitting diode epitaxial wafer according to any one of claims 1 to 6, characterized in that: include: Providing a substrate, and sequentially growing a buffer layer, an N-type GaN layer, a multi-quantum well layer, an electron blocking layer and a P-type GaN layer on the substrate; The multi-quantum well layer comprises a first multi-quantum well layer, a final well layer and a final barrier layer sequentially stacked on the N-type GaN layer, the first multi-quantum well layer is a periodic structure formed by alternating stacking of quantum well layers and quantum barrier layers, the quantum well layer and the final well layer are both InGaN quantum well layers, and the quantum barrier layer is a GaN quantum barrier layer; The final barrier layer includes Al x Ga 1-x N-layer, In y Ga 1-y N-layer, In z Ga 1-z N layer and GaN layer; wherein, the value range of x is 0.05~0.3, the value range of y is 0.01~0.1, the value range of z is 0.01~0.1, and z>y; The electron blocking layer is a β-Ta2O5 layer; The P-type GaN layer includes a first P-type GaN layer, a P-type In layer, and a α Ga 1-α N layer and a second P-type GaN layer, wherein the value range of α is 0.08~0.
15.
8. The method for preparing a light emitting diode epitaxial wafer according to claim 7, characterized in that: The growth temperature of the quantum well layer and the final well layer is 740° C. to 820° C., and the growth pressure is 100 torr to 300 torr; and / or The growth temperature of the quantum barrier layer and the final barrier layer is 850° C. to 950° C., and the growth pressure is 100 torr to 300 torr; and / or The growth temperature of the electron blocking layer is 800° C. to 900° C., and the growth pressure is 10 torr to 100 torr; and / or The growth temperature of the first P-type GaN layer and the second P-type GaN layer is 900° C. to 1000° C., and the growth pressure is 100 torr to 500 torr; and / or The P-type α Ga 1-α The growth temperature of the N layer is 750°C~850°C, and the growth pressure is 100torr~500torr.
9. The method for preparing a light emitting diode epitaxial wafer according to claim 8, characterized in that: After the electron blocking layer is grown, annealing is performed at 900° C. to 950° C. for 10 min to 30 min in air or oxygen atmosphere.
10. A light emitting diode, characterized in that: It comprises the light emitting diode epitaxial wafer as described in any one of claims 1 to 6.