A method for preparing a carbon-based supramolecular material for simultaneous adsorption of heavy metals and new pollutants in water
Through microwave-assisted pyrolysis and cross-linking grafting of β-cyclodextrin, a carbon-based supramolecular material with efficient adsorption performance was prepared, which solved the problem of existing biochar being difficult to adsorb heavy metals and new pollutants at the same time, and achieved The simultaneous removal of mercury, cadmium, perfluorooctanoic acid and nonylphenol improves the adsorption effect and simplifies the process.
Patent Information
- Application Number
- CN202411068888.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-08-06
AI Technical Summary
It is difficult for existing biochar to efficiently adsorb heavy metals and new pollutants such as perfluorooctanoic acid and nonylphenol in water at the same time. Moreover, the traditional electric heating process is time-consuming and difficult to balance the material preparation speed and pollution removal efficiency.
Using the method of microwave-assisted pyrolysis and cross-linking grafted β-cyclodextrin, and by optimizing the preparation conditions, carbon-based supramolecular materials with carboxyl functional groups and hydrophobic cavities were prepared to achieve the goal of protecting mercury, cadmium, perfluorooctanoic acid and nonyl Simultaneous adsorption of phenol.
It significantly improves the adsorption capacity of mercury, cadmium, perfluorooctanoic acid and nonylphenol, shortens the reaction time, is energy-saving and environmentally friendly, and the process is simple and easy to be industrialized.
Smart Images

Figure CN118577255B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of material adsorption, and specifically relates to a method for preparing a carbon-based supramolecular material for synchronously adsorbing heavy metals and new pollutants in water, in particular to a carbon-based supramolecular material for synchronously adsorbing mercury, cadmium, perfluorooctanoic acid and nonylphenol in water and a preparation method thereof. Background Art
[0002] Heavy metals (such as mercury, cadmium, etc.) and new pollutants (such as perfluorooctanoic acid, nonylphenol, etc.) are detected in large quantities in the water environment. Among them, mercury and cadmium can exist in the form of simple cations in water, with small radius, strong hydrophilicity, easy to lose electrons and carry positive charge, and have empty orbits that can accept ligands, and have very long half-lives. Compared with heavy metals, perfluorooctanoic acid, nonylphenol and other molecules have more complex structures, larger diameters, and stronger hydrophobicity. Perfluorooctanoic acid contains a strong polar CF bond, and it also contains a specific functional group carboxyl, which is easy to coordinate with heavy metal cations. Nonylphenol contains a benzene ring, and the π bond in the benzene ring will form a negative potential area, which has a strong electrostatic attraction to heavy metal cations, causing perfluorooctanoic acid, nonylphenol and heavy metal cations to have complex interactions. In general, the chemical structure and properties of perfluorooctanoic acid, nonylphenol and heavy metal cations are relatively stable, so they can coexist in water for a long time to form complex pollution, and show high toxicity at low exposure levels, and are ingested by organisms and transmitted step by step through the food chain. Therefore, the simultaneous removal of heavy metal, perfluorooctanoic acid and nonylphenol complex pollution has important scientific significance and application value.
[0003] Adsorption is currently the preferred method for removing typical heavy metal / new pollutants (such as perfluorooctanoic acid, nonylphenol, etc.) combined pollution in water because it can be applied flexibly on a large scale in water and can directly remove pollutants from water. Biochar usually refers to a carbon-rich solid product formed by the pyrolysis of biomass waste raw materials under anoxic or limited oxygen supply. It has the advantages of abundant raw materials, wide sources and low prices. It contains a highly carboxylated porous aromatic carbon skeleton, obvious pore structure, large specific surface area, and oxygen-containing functional groups such as carboxyl and hydroxyl groups, so it has good surface adsorption. The adsorption of perfluorinated compounds and nonylphenol by biochar mainly relies on weak intermolecular interactions (such as hydrophobic interactions and π-π electron donor-acceptor, etc.), but it is difficult to produce directional adsorption of heavy metal ions, and the removal effect is limited. In the research on the adsorption of heavy metals by biochar, most of them are to introduce nitrogen, oxygen or sulfur functional groups that are firmly bound to heavy metals on the surface of biochar to improve the adsorption performance, but such functional groups are highly hydrophilic and difficult to bind to perfluorinated compounds and nonylphenol with strong hydrophobicity. Therefore, the specificity and complexity of the structural properties of complex pollutants often make the existing biochar modification methods lose sight of one thing while focusing on another.
[0004] β-cyclodextrin has a conical cage-type supramolecular structure of "hydrophobic inside the ring and hydrophilic outside the ring". The shielding of carbon-hydrogen bonds inside the ring is hydrophobic, and can undergo host-guest selective inclusion complexation with perfluorooctanoic acid and nonylphenol. The outside of the ring has hydroxyl groups with different chemical reactivity, which are hydrophilic and can be easily composited with biochar through cross-linking grafting reactions.
[0005] In addition to being a "bridge" for the combination of biochar and β-cyclodextrin, the cross-linking agent selected in the present invention preferably also has the ability to directional combine with heavy metal ions, achieving "killing two birds with one stone". In addition, the existing biochar cross-linking grafting reaction adopts traditional electric heating, and the reaction time is relatively long (generally several hours or even more than ten hours), which makes it difficult to balance the material preparation speed and the decontamination efficiency. Therefore, the present invention selects efficient and energy-saving microwave heating instead of traditional electric heating to achieve rapid compounding of biochar and β-cyclodextrin, and efficiently and simultaneously remove the compound pollution of mercury, cadmium, perfluorooctanoic acid and nonylphenol.
[0006] At present, there are many studies on the removal of single heavy metals and new pollutants (such as perfluorooctanoic acid, nonylphenol, etc.) by adsorbent materials at home and abroad, but there are few reports on adsorbent materials that can achieve simultaneous adsorption of heavy metals and new pollutants (such as perfluorooctanoic acid, nonylphenol, etc.) in water. Therefore, the present invention establishes a method for microwave-assisted biomass pyrolysis and cross-linking and grafting β-cyclodextrin, and obtains a carbon-based supramolecular material that can efficiently and simultaneously remove mercury, cadmium, perfluorooctanoic acid and nonylphenol by optimizing its preparation conditions, characterizing its structural properties and testing its simultaneous adsorption performance. Summary of the invention
[0007] The present invention aims to provide a carbon-based supramolecular material and a preparation method for adsorbing heavy metals (such as mercury, cadmium, etc.) and new pollutants (such as perfluorooctanoic acid, nonylphenol, etc.) in water. On the one hand, it can realize the resource utilization of cellulose biomass waste raw materials, and on the other hand, the prepared carbon-based supramolecular material has both complexing functional groups that can adsorb heavy metal ions and hydrophobic cavities that can selectively encapsulate perfluorooctanoic acid and nonylphenol, thereby realizing the simultaneous removal of pollutants that meet the requirements. The method is simple in process, highly efficient and energy-saving, and the results are easy to replicate and promote, with broad market prospects.
[0008] The present invention solves the technical problem by adopting the following technical solutions:
[0009] A method for preparing a carbon-based supramolecular material for simultaneously adsorbing heavy metals and new pollutants in water comprises the following steps:
[0010] S1. Put the cleaned cellulose biomass into a quartz tube, then introduce inert gas, place it in a microwave tube furnace and pyrolyze it at a heating rate of 5-60°C / min, the pyrolysis temperature is 200-900°C, the pyrolysis time is 2-30min, and the original biochar is obtained after the pyrolysis is completed;
[0011] S2, reacting the original biochar prepared in step S1 with a polyacid anhydride at a mass ratio of 1:0.5 to 1:5, first dissolving the polyacid anhydride in an alkaline polar organic solvent, then adding the original biochar, placing it in a microwave synthesizer for reaction, the reaction temperature is 60-150°C, the reaction time is 5-30min, after the reaction is completed, washing with an alkaline polar organic solvent, a 0.1mol / L sodium hydroxide solution, and deionized water in sequence until neutral, and drying in an oven at 65°C to constant weight to obtain carboxyl-modified biochar;
[0012] S3. The carboxyl-modified biochar prepared in step S2 is reacted with β-cyclodextrin at a mass ratio of 0.5:1 to 5:1. The β-cyclodextrin is first dissolved in a sodium hydroxide solution, and then the carboxyl-modified biochar is added, and the reaction is carried out in a microwave synthesizer. The reaction temperature is 30-120°C and the reaction time is 10-50min. After the reaction is completed, the biochar is cooled to room temperature, washed with ethanol and deionized water in turn until neutral, and dried in an oven at 65°C to constant weight to obtain a carbon-based supramolecular material.
[0013] Moreover, the inert gas in step S1 is argon.
[0014] Moreover, the polyacid anhydride in step S2 is one of pyromellitic anhydride, citric anhydride or ethylenediaminetetraacetic dianhydride.
[0015] Moreover, the alkaline polar organic solvent in step S2 is one of N,N-dimethylformamide or pyridine.
[0016] Moreover, in the step S2, the reaction temperature of the microwave synthesizer is 90-120°C, and the reaction time is 15-25 min.
[0017] Moreover, in step S3, the mass fraction of the sodium hydroxide solution is 5%-20%.
[0018] A carbon-based supramolecular material for simultaneously adsorbing heavy metals and new pollutants in water is used as a material for adsorbing mercury, cadmium, perfluorooctanoic acid and nonylphenol in water. The addition amount of the carbon-based supramolecular material is 1g / L, the reaction time is 12-24h, and the reaction temperature is 25°C.
[0019] Moreover, when the carbon-based supramolecular material simultaneously removes mercury ions and perfluorooctanoic acid from water, the pH value of the solution is 6-8.
[0020] Moreover, when the carbon-based supramolecular materials simultaneously removed cadmium ions and nonylphenol from acidic wastewater, the pH value of the solution was 4-5.
[0021] The advantages and positive effects of the present invention are:
[0022] 1. The present invention uses cellulose biomass as raw material, and prepares carbon-based supramolecular materials by microwave-assisted pyrolysis and cross-linking grafting, so that the carbon-based supramolecular materials have both active functional groups that can adsorb mercury ions and cadmium ions, and hydrophobic cavities that can selectively encapsulate perfluorooctanoic acid and nonylphenol; further optimize its preparation conditions, characterize its structural properties and test its synchronous adsorption performance. The carbon-based supramolecular materials can simultaneously adsorb mercury ions and perfluorooctanoic acid up to 28.13 mg / g and 60.90 ug / g, respectively, which is 2 times higher than the original biochar effect; the carbon-based supramolecular materials can simultaneously adsorb cadmium ions and nonylphenol up to 24.15 mg / g and 10.00 mg / g, respectively, which is 4.5 times higher than the original biochar effect. Under harsh conditions such as acidity, the carbon-based supramolecular materials have good simultaneous removal effects of mercury ions, cadmium ions, perfluorooctanoic acid and nonylphenol, and successfully solve the problem that the molecular design of existing adsorption materials is difficult to achieve due to the significantly different structural properties of mercury ions, cadmium ions, perfluorooctanoic acid and nonylphenol.
[0023] 2. The present invention uses microwave heating technology in the pyrolysis and cross-linking grafting process of cellulose biomass, making full use of the advantages of microwave's non-thermal effect, strong penetration and uniform heating; at the same time, chemical reagents with high-efficiency microwave absorption characteristics (such as N, N-dimethylformamide) are selected, and the alkaline environment required for the reaction can also be provided, killing two birds with one stone, completing the above reaction quickly and efficiently. Compared with the traditional electric heating method, the above microwave-assisted directional preparation method has more significant advantages in shortening the reaction time, reducing the amount of reactants and saving energy, and the process is simple and easy to promote industrialization.
[0024] 3. The raw materials used in the present invention are agricultural and forestry waste biomass, which are widely available, cheap and easy to obtain, and realize the resource utilization of agricultural and forestry waste, which has important ecological and economic significance.
[0025] 4. The present invention prepares carbon-based supramolecular materials by microwave-assisted pyrolysis and cross-linking grafting. Through scanning electron microscopy (SEM) and Fourier transform infrared spectroscopy (FTIR) characterization and analysis, it is found that compared with the original biochar, the surface of the carbon-based supramolecular material is attached with particles, and the carbon-based supramolecular material has a particle shape at 3400 (representing OH stretching vibration) and 1726 cm -1 The peak (representing the stretching vibration of the C=O double bond) is greatly enhanced at 2930 cm -1 A new peak appears at (representing CO stretching vibration), indicating that carboxyl groups and β-cyclodextrin have been successfully introduced on the surface of native biochar. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a graph showing the effect of heating rate on mass loss rate in carbon-based supramolecular materials.
[0027] Figure 2This is a graph showing the effect of microwave radiation temperature on the mass loss rate in carbon-based supramolecular materials.
[0028] Figure 3 This is a graph showing the effect of microwave irradiation time on the mass loss rate in carbon-based supramolecular materials.
[0029] Figure 4 This is a graph showing the effect of microwave radiation temperature on the grafting rate in carbon-based supramolecular materials.
[0030] Figure 5 This is a graph showing the effect of microwave irradiation time on the grafting rate in carbon-based supramolecular materials.
[0031] Figure 6 This is a graph showing the effect of the BC:PMDA mass ratio on the grafting rate in carbon-based supramolecular materials.
[0032] Figure 7 This is a graph showing the effect of grafting reaction temperature on the mass loss rate in carbon-based supramolecular materials.
[0033] Figure 8 This is a graph showing the effect of grafting reaction time on mass loss rate in carbon-based supramolecular materials.
[0034] Fig. 9 This is a graph showing the effect of the mass ratio of β-cyclodextrin to carboxyl-modified biochar on the mass loss rate in carbon-based supramolecular materials.
[0035] Fig.10 This is a scanning electron microscope (SEM) image of coconut shell biochar magnified 40,000 times.
[0036] Fig.11 This is a scanning electron microscope (SEM) image of carboxyl-modified biochar magnified 40,000 times.
[0037] Fig.12 This is a scanning electron microscope (SEM) image of the carbon-based supramolecular material magnified 40,000 times.
[0038] Fig.13 This is the Fourier transform infrared spectroscopy (FTIR) analysis result of carbon-based supramolecular materials.
[0039] Fig.14 This is a preparation route map for the carbon-based supramolecular material described in Example 1 of the present invention. DETAILED DESCRIPTION
[0040] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto. Example 1
[0041] A method for preparing a carbon-based supramolecular material for simultaneously adsorbing heavy metals and new pollutants in water comprises the following steps:
[0042] S1. Put the cleaned cellulose biomass into a quartz tube, then introduce inert gas, place it in a microwave tube furnace and pyrolyze it at a heating rate of 5-60°C / min, the pyrolysis temperature is 200-900°C, the pyrolysis time is 2-30min, and the original biochar is obtained after the pyrolysis is completed;
[0043] S2, reacting the original biochar prepared in step S1 with a polyacid anhydride at a mass ratio of 1:0.5 to 1:5, first dissolving the polyacid anhydride in an alkaline polar organic solvent, then adding the original biochar, placing it in a microwave synthesizer for reaction, the reaction temperature is 60-150°C, the reaction time is 5-30min, after the reaction is completed, washing with an alkaline polar organic solvent, a 0.1mol / L sodium hydroxide solution, and deionized water in sequence until neutral, and drying in an oven at 65°C to constant weight to obtain carboxyl-modified biochar;
[0044] S3. The carboxyl-modified biochar prepared in step S2 is reacted with β-cyclodextrin at a mass ratio of 0.5:1 to 5:1. The β-cyclodextrin is first dissolved in a sodium hydroxide solution, and then the carboxyl-modified biochar is added, and the reaction is carried out in a microwave synthesizer. The reaction temperature is 30-120°C and the reaction time is 10-50min. After the reaction is completed, the biochar is cooled to room temperature, washed with ethanol and deionized water in turn until neutral, and dried in an oven at 65°C to constant weight to obtain a carbon-based supramolecular material.
[0045] like Fig.14 The figure shows the preparation route of the carbon-based supramolecular material prepared in this embodiment.
[0046] The specific steps are as follows:
[0047] The cleaned coconut shell is placed in a quartz tube and placed in a microwave tube furnace for pyrolysis, and then argon gas is introduced to obtain coconut shell biochar after the pyrolysis is completed;
[0048] like Figure 1-Figure 2 As shown, the product mass loss rate (representing a more developed pore structure and a higher adsorption capacity) was used as the evaluation index to optimize the reaction temperature and reaction time during the pyrolysis process, so that the coconut shell biochar had a larger mass loss rate;
[0049] The heating rates during the pyrolysis process were 5 ℃ / min, 10 ℃ / min, 20 ℃ / min, 30 ℃ / min, 40 ℃ / min, and 60 ℃ / min, respectively; the reaction temperatures during the pyrolysis process were 200 ℃, 300 ℃, 400 ℃, 500 ℃, 600 ℃, 700 ℃, 800 ℃, and 900 ℃, respectively; the reaction times during the pyrolysis process were 2 min, 15 min, 20 min, 25 min, and 30 min, respectively; and the mass loss rate of the coconut shell biochar was calculated as shown in formula ①:
[0050] ;
[0051] in, is the mass loss rate; is the mass of coconut shell, g; is the mass of coconut shell biochar, g.
[0052] Therefore, the microwave pyrolysis conditions were determined as follows: heating rate of 30 °C / min, pyrolysis temperature of 800 °C, and pyrolysis time of 25 min.
[0053] The prepared coconut shell biochar was mixed with pyromellitic anhydride and added to N, N-dimethylformamide solution, placed in a microwave synthesizer for reaction. After the reaction was completed, it was washed with N, N-dimethylformamide solution and 0.1 mol / L sodium hydroxide solution in sequence, and then washed with deionized water until neutral, and dried in an oven at 65 °C to constant weight to obtain carboxyl-modified biochar.
[0054] like Figure 4-Figure 6 As shown, taking the grafting rate as the evaluation index, the reaction temperature, reaction time and the mass ratio of coconut shell biochar to pyromellitic anhydride in the carboxyl modification process are optimized to obtain coconut shell biochar with a higher grafting rate.
[0055] The reaction temperatures in the carboxyl modification process were 60 °C, 75 °C, 90 °C, 105 °C, 120 °C, 135 °C, and 150 °C, respectively; the reaction times were 5 min, 10 min, 15 min, 20 min, 25 min, and 30 min, respectively; the mass ratios of coconut shell biochar to pyromellitic anhydride were 1:0.5, 1:1, 1:2, 1:3, 1:4, and 1:5, respectively; the grafting rate of the carboxyl modified biochar was calculated as shown in formula ②:
[0056] ;
[0057] in, is the grafting rate; is the mass of coconut shell biochar, g; is the mass of carboxyl-modified biochar, g.
[0058] Therefore, the optimal microwave-assisted carboxyl modification reaction conditions were determined as follows: reaction temperature of 105 °C, reaction time of 20 min, and the mass ratio of coconut shell biochar to pyromellitic anhydride of 1:4.
[0059] The prepared carboxyl-modified biochar and β-cyclodextrin were added to alkaline solution and placed in a microwave synthesizer for reaction. After the reaction was completed, it was cooled to room temperature and washed with 0.1 mol / L sodium hydroxide solution and ethanol in sequence, then washed with deionized water until neutral, and dried in an oven at 65 °C to constant weight to obtain a carbon-based supramolecular material.
[0060] like Figure 7-Figure 9 As shown in the figure, since the grafting process of β-cyclodextrin causes mass loss, the mass loss rate is used as an evaluation index to optimize the reaction temperature, reaction time and the mass ratio of carboxyl-modified biochar to β-cyclodextrin in the grafting process, so as to obtain carbon-based supramolecular materials with a smaller mass loss rate;
[0061] The reaction temperatures in the grafting process were 30 ℃, 40 ℃, 50 ℃, 60 ℃, and 70 ℃, respectively; the reaction times were 10 min, 20 min, 30 min, 40 min, and 50 min, respectively; the mass ratios of carboxyl-modified biochar and β-cyclodextrin were 1:0.5, 1:1, 1:2, 1:3, 1:4, and 1:5, respectively; and the mass loss rate of carboxyl-modified biochar and β-cyclodextrin was calculated as shown in formula ③:
[0062] ;
[0063] in, is the mass loss rate; is the mass of carboxyl-modified biochar, g; is the mass of carbon-based supramolecular material, g.
[0064] Therefore, the optimal microwave-assisted cyclodextrin grafting reaction conditions were determined as follows: reaction temperature of 50 °C, reaction time of 30 min, and the mass ratio of carboxyl-modified biochar to β-cyclodextrin of 1:3.
[0065] The preparation conditions of carbon-based supramolecular materials were further optimized by response surface design: Design Expert software was used to design the experiment using central composite design (CCD) to find the relationship between the influencing factors of the grafting process and the grafting rate. The grafting rate was the only response value Y, and the four factors of carboxyl grafting reaction temperature, carboxyl reaction time, carboxyl reactant mass ratio (PMDA: BC) and cyclodextrin mass ratio (β-C: BC) were used as input variables, which were recorded as A, B, C and D respectively. The calculation method is shown in formula ④.
[0066] ;
[0067] in, is the grafting rate; is the mass of coconut shell, g; is the mass of carbon-based supramolecular material, g.
[0068] According to the optimization range of each factor in the single factor grafting experiment results, the experimental level of each process factor is divided into 5 categories, namely -γ, -1, 0, +1, and +γ. The specific experimental factors and distribution levels of the response surface design are shown in Table 1.
[0069] Table 1 Experimental factors and distribution levels of response surface design
[0070]
[0071] The whole experimental matrix has 30 groups, as shown in Table 2.
[0072] Table 2 Response surface design
[0073]
[0074] The variance analysis results of the quadratic multivariate linear regression model are shown in Table 3.
[0075] Table 3 ANOVA results of quadratic multiple linear regression model
[0076]
[0077] Among them, the quadratic multiple regression equation is:
[0078] ;
[0079] As shown in formula ⑤, a quantitative relationship model between the grafting rate of the material and the above preparation parameters was established through quadratic multivariate regression fitting. The correlation coefficient R 2The value of the model was 0.9174, indicating that the model had a good fitting effect. By performing variance analysis on the experimental data, the variance inflation factor of each factor was very close to 1, indicating that there was no distortion in the model fitting process, and the relationship between the grafting rate and each preparation factor could be well explained. The P value corresponding to the model was less than 0.05, indicating that the model was significant. Among them, the interaction of the mass ratio of β-cyclodextrin and carboxyl-modified biochar, carboxylation reaction temperature and carboxylation reaction time in the model had a significant effect on the grafting rate of the material (Table 3). The above quantitative relationship model shows that the interaction of the four factors has a positive correlation with the grafting rate, that is, the grafting rate increases to varying degrees with the increase of the experimental values of any two factors. The above quadratic multivariate regression model was solved to obtain the optimal preparation process conditions of carbon-based supramolecular materials: the carboxylation reaction temperature was 120 ℃, the carboxylation reaction time was 25 min, the mass ratio of PMDA and coconut shell biochar was 3:1, and the mass ratio of β-cyclodextrin and carboxyl-modified biochar was 2:1. The calculated value of the grafting rate obtained by the quadratic multivariate regression model was 10.63%. A group of parallel experiments were carried out under the experimental conditions, and the grafting rate was 11.12%. The theoretical calculated value of the grafting rate was very close to its experimental value, with a relative error of 4.6%, indicating that the multivariate regression model can more truly reflect the influence of various influencing factors on the grafting rate during the directional preparation of the new fiber-carbon supramolecular material, proving that the multivariate regression model is more reliable.
[0080] The surface morphology of coconut shell biochar, carboxyl-modified biochar and carbon-based supramolecular materials was analyzed using a Quanta FEG 250 environmental field emission scanning electron microscope. Figure 10-12 The functional groups of coconut shell biochar, carboxyl-modified biochar and carbon-based supramolecular materials were analyzed using a BRUKER Tensor 37 Fourier transform infrared spectrometer. Fig.13 .
[0081] contrast Fig.10 and Fig.11 It can be found that Fig.11 Surface area ratio of medium carboxyl modified biochar Fig.10 The coconut shell biochar is smoother, which may be due to the introduction of anhydride molecules, covering the surface of coconut shell biochar; Fig.11 , Fig.12 The surface of the medium carbon-based supramolecular material is covered with a layer of granular substances, which may be due to the introduction of β-cyclodextrin molecules, which cover the surface of carboxyl-modified biochar. Fig.13 It was found that compared with coconut shell biochar, carbon-based supramolecular materials and carboxyl-modified biochar did not destroy the basic structure of coconut shell biochar. The carboxyl-modified biochar had a high molecular weight at 1726 cm -1The peak of (representing the stretching vibration of C=O double bond) was greatly enhanced, proving that more carboxyl groups were successfully introduced; the carbon-based supramolecular material was at 2930 cm -1 A new peak appears at 3400 cm -1 The peak at (representing OH stretching vibration) was greatly enhanced, proving that the β-cyclodextrin molecules were successfully introduced. Example 2
[0082] In this embodiment, the carbon-based supramolecular material prepared by the method in Example 1 is used to simultaneously remove mercury ions and perfluorooctanoic acid in water, and specifically comprises the following steps:
[0083] Weigh 0.05 g of carbon-based supramolecular material and add it to 50 mL of a solution containing perfluorooctanoic acid (concentration of 100 ug / L) and mercury ions (concentration of 100 mg / L).
[0084] Static adsorption was carried out for 12 h under the conditions of temperature of 25 ℃ and solution pH of 6. The adsorption capacity of mercury ions and perfluorooctanoic acid was 28.13 mg / g and 60.90 ug / g, respectively, which was 2 times higher than that of coconut shell biochar prepared from the same raw materials.
[0085] Static adsorption was carried out for 12 h under the conditions of temperature of 25 ℃ and solution pH of 8. The adsorption capacity of mercury ions and perfluorooctanoic acid was 26.49 mg / g and 58.87 ug / g, respectively, which was more than twice that of coconut shell biochar prepared from the same raw materials.
[0086] The mercury ion content in the filtrate was determined by an inductively coupled plasma emission spectrometer (VISTA-MPX, Varian Corporation, USA), and the perfluorooctanoic acid content was determined by a liquid chromatography-mass spectrometer (LCMS-8050, Shimadzu, Japan). Example 3
[0087] In this embodiment, the carbon-based supramolecular material prepared by the method in Example 1 is used to simultaneously remove cadmium ions and nonylphenol from acidic wastewater, specifically comprising the following steps:
[0088] Weigh 0.05 g of carbon-based supramolecular material and add it to 50 mL of a solution containing nonylphenol (concentration of 10 mg / L) and cadmium ions (concentration of 100 mg / L).
[0089] Under the conditions of static adsorption for 24 h at a temperature of 25 ℃ and a solution pH of 4, the adsorption capacity of cadmium ions was 26.40 mg / g and the adsorption capacity of nonylphenol was 8.06 mg / g, which was nearly 4 times higher than that of coconut shell biochar prepared from the same raw materials.
[0090] Static adsorption was carried out for 24 h at a temperature of 25 ℃ and a solution pH of 5. The adsorption capacity of mercury ions and nonylphenol was 24.15 mg / g and 10.00 mg / g, respectively, which was 4.5 times higher than that of coconut shell biochar prepared from the same raw materials.
[0091] The cadmium ion content of the filtrate was determined by an inductively coupled plasma emission spectrometer (AgilentICP-MS 7500, Agilent, USA), and the nonylphenol content was determined by an ultraviolet spectrophotometer (UV 2450, Shimadzu, Japan)).
[0092] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.
Claims
1. A method for preparing a carbon-based supramolecular material for simultaneous adsorption of heavy metals and new pollutants in water, characterized in that: The steps include: S1. Put the cleaned cellulose biomass into a quartz tube, then introduce inert gas, place it in a microwave tube furnace and pyrolyze it at a heating rate of 5-60°C / min, the pyrolysis temperature is 300-900°C, the pyrolysis time is 15-30min, and the original biochar is obtained after the pyrolysis is completed; S2, reacting the original biochar prepared in step S1 with a polyacid anhydride at a mass ratio of 1:0.5 to 1:5, first dissolving the polyacid anhydride in N, N-dimethylformamide, then adding the original biochar, placing it in a microwave synthesizer for reaction, the reaction temperature is 60-150°C, the reaction time is 5-30min, after the reaction is completed, washing with N, N-dimethylformamide, 0.1mol / L sodium hydroxide solution, and deionized water in sequence until neutral, and drying in a 65°C oven to constant weight to obtain carboxyl-modified biochar; S3. The carboxyl-modified biochar prepared in step S2 is reacted with β-cyclodextrin at a mass ratio of 0.5:1 to 5:
1. β-cyclodextrin is first dissolved in a sodium hydroxide solution, and then the carboxyl-modified biochar is added and placed in a microwave synthesizer for reaction. The reaction temperature is 30-120°C and the reaction time is 10-50min. After the reaction is completed, it is cooled to room temperature, washed with ethanol and deionized water in turn until neutral, and dried in an oven at 65°C to constant weight to obtain a carbon-based supramolecular material.
2. The method for preparing a carbon-based supramolecular material for simultaneous adsorption of heavy metals and new pollutants in water according to claim 1, characterized in that: The inert gas in step S1 is argon.
3. The method for preparing a carbon-based supramolecular material for simultaneous adsorption of heavy metals and new pollutants in water according to claim 1, characterized in that: The polyacid anhydride in step S2 is one of pyromellitic anhydride, citric anhydride or ethylenediaminetetraacetic dianhydride.
4. The method for preparing a carbon-based supramolecular material for simultaneous adsorption of heavy metals and new pollutants in water according to claim 1, characterized in that: In step S2, the reaction temperature of the microwave synthesizer is 90-120°C, and the reaction time is 15-25 min.
5. The method for preparing a carbon-based supramolecular material for simultaneous adsorption of heavy metals and new pollutants in water according to claim 1, characterized in that: In step S3, the mass fraction of the sodium hydroxide solution is 5%-20%.
6. Application of a carbon-based supramolecular material for simultaneous adsorption of heavy metals and new pollutants in water prepared by the method according to any one of claims 1 to 5 as a material for adsorbing mercury, cadmium, perfluorooctanoic acid and nonylphenol in water, characterized in that: The addition amount of carbon-based supramolecular material is 1 g / L, the reaction time is 12-24 h, and the reaction temperature is 25°C.
7. The use according to claim 6, characterized in that: When the carbon-based supramolecular material simultaneously removes mercury ions and perfluorooctanoic acid from water, the pH value of the solution is 6-8.
8. The use according to claim 6, characterized in that: When the carbon-based supramolecular material simultaneously removes cadmium ions and nonylphenol from acidic wastewater, the pH value of the solution is 4-5.