A micron-level quartz wire welding device and method based on laser melting
Through laser melting technology and real-time position adjustment module, the problem of poor welding quality between micron-level quartz wire and samples is solved, high-precision alignment and welding are achieved, and welding quality is improved.
Patent Information
- Application Number
- CN202411044528.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-01
AI Technical Summary
Traditional welding methods are difficult to achieve high-precision alignment and welding of micron-scale quartz wires with samples, which can easily lead to poor welding quality and film burning.
Using a micro-level quartz wire welding device based on laser melting, including suspended tooling, sample table, laser welding module and imaging module, the relative position of micro-level quartz wire and sample is detected and adjusted in real time through the position adjustment module, and the power adjustable The laser beam performs two-step welding and position fine-tuning to ensure high-precision alignment and welding.
The welding quality of micron-scale quartz wire and samples is improved, the impact of the welding process on performance is reduced, welding offset and ablation are avoided, and high-precision positioning and welding are achieved.
Smart Images

Figure CN118577934B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of laser welding technology, and more specifically, relates to a micron-level quartz wire welding device and method based on laser melting. Background Art
[0002] In recent years, more and more research has begun to focus on the milligram-level torsion balance system, which is becoming one of the important means of weak force or weak torque detection. In the milligram-level torsion balance system, quartz wire is widely used as a suspension wire in the torsion balance system due to its high strength and low expansion coefficient, and is used to suspend the test sample.
[0003] At present, the signal-to-noise ratio is one of the important indicators for evaluating the performance of a milligram-level torsion balance. The improvement of the signal-to-noise ratio can be solved from the perspective of reducing dissipation. Studies have found that whether it is a torsion pendulum or a simple pendulum, the dissipation mainly comes from the connection, and the welding connection method can effectively reduce the dissipation. Therefore, the use of welding to connect the quartz wire and the sample can effectively improve the performance of the milligram-level torsion pendulum.
[0004] In the related art, in order to provide good detection sensitivity, micron-sized quartz wire is preferably used as the suspension wire of the milligram-level torsion balance system. However, when the micron-sized quartz wire is welded by the traditional welding method, the micron-sized quartz wire is easy to bend, and the alignment of the micron-sized quartz wire and the sample cannot be completed well. In addition, the welding process is prone to film burning, resulting in poor welding quality between the micron-sized quartz wire and the sample, which urgently needs to be improved. Summary of the invention
[0005] In response to the defects or improvement needs of the prior art, the present application provides a micron-level quartz wire welding device and method based on laser melting, aiming to improve the welding quality between the micron-level quartz wire and the sample.
[0006] The present application provides a micron-level quartz wire welding device based on laser melting, which specifically includes a frame, on which is provided:
[0007] A suspension tool, used for suspending a micron-grade quartz wire on a frame, wherein the end of the micron-grade quartz wire is a quartz rod;
[0008] A sample stage, used for supporting the sample below the micron-sized quartz wire;
[0009] A laser welding module is used to provide a laser beam with adjustable power to form a molten zone in the circumferential direction of the end of the micron-sized quartz wire to achieve welding of the micron-sized quartz wire and the sample;
[0010] An imaging module for real-time detection of the position of micron-scale quartz wires and samples;
[0011] The position adjustment module is used to adjust the relative position of the micron-sized quartz wire and the sample based on the information detected in real time by the imaging module, and to adjust the distance between the laser output from the laser welding module to the surface of the micron-sized quartz wire and the bottom of the end of the micron-sized quartz wire, so as to ensure that the micron-sized quartz wire is aligned with the sample.
[0012] Through the above technical scheme conceived by the present application, compared with the prior art, the position adjustment module and the laser welding module in the present device can cooperate with each other, and under the detection of the imaging module, can cooperate with the sample stage, suspension tooling and other components to perform two front and back melting of the micron-level quartz wire, and two front and back alignment of the micron-level quartz wire and the sample, so as to improve the welding quality of the micron-level quartz wire and the sample, and reduce the impact of the welding operation on the performance of the micron-level quartz wire and the sample.
[0013] When welding the micron-sized quartz wire and the sample, the position adjustment module can adjust the relative position of the micron-sized quartz wire and the sample. Based on the detection result of the imaging module, the position adjustment module is used to adjust the docking position of the sample and the micron-sized quartz wire, so that the micron-sized quartz wire and the sample are initially in a mutually separated and aligned state, ready for the welding process. The laser welding module then melts the end of the micron-sized quartz wire to form an end melting zone, and then the position of the sample and the micron-sized quartz wire is adjusted through the position adjustment module, so that the sample contacts the melting zone of the micron-sized quartz wire to complete the initial welding.
[0014] After the initial welding, since the power of the laser beam in the laser welding module is adjustable, the position adjustment module can adjust the height of the molten zone that can be formed by the laser welding module at the end of the micron-level quartz wire. At this time, the position adjustment module is used to increase the height of the molten zone that can be formed by the laser welding module at the end of the micron-level quartz wire. After the laser welding module reduces the power to melt the micron-level quartz wire, the position adjustment module is used to readjust the micron-level quartz wire and the sample to center alignment, and the welding is completed.
[0015] As a further preferred embodiment, the laser welding module includes a laser, multiple beam splitters and multiple reflectors. The power of the laser is adjustable. The laser beam emitted by the laser is reflected by the reflector and split by the beam splitter, and then converges at multiple angles on the circumferential surface of the end of the micron-sized quartz wire.
[0016] As further preferred, the position adjustment module includes an angle adjustment mechanism arranged on a frame, and the angle adjustment mechanism is used to adjust the pitch angle of the reflector.
[0017] As further preferred, a reflecting surface of one of the reflecting mirrors intersects with a horizontal plane, and the position adjustment module comprises an adjustment mechanism arranged on a frame for lifting and lowering the reflecting mirror.
[0018] As a further preference, the position adjustment module includes a tool adjustment mechanism disposed on the frame for driving the suspended tool to adjust the position.
[0019] As further preferred, the position adjustment module includes a sample stage adjustment mechanism disposed on a frame for driving the sample stage to adjust its position.
[0020] As further preferred, the welding device also includes a clamp for clamping the end of the micron-sized quartz wire.
[0021] As further preferred, the welding device also includes a clamp adjustment mechanism for driving the clamp to adjust its position.
[0022] A welding method provided in the second aspect of the present application adopts the following technical solution:
[0023] A welding method, implemented based on any one of the micron-level quartz wire welding devices based on laser melting described in the first aspect, comprises the following steps:
[0024] S1. Adjusting the position adjustment module based on the information detected in real time by the imaging module so that the sample is aligned with the center of the micron-sized quartz wire and a gap is left between the sample and the micron-sized quartz wire;
[0025] S2. The bottom of the end of the micron-sized quartz wire is melted to form a molten zone through a laser welding module, and the sample is brought into contact with the molten zone of the micron-sized quartz wire through a position adjustment module to complete the initial welding;
[0026] S3. Reduce the laser power of the laser welding module, and at the same time increase the distance between the laser output from the laser welding module to the surface of the micron-sized quartz wire and the bottom of the end of the micron-sized quartz wire through the position adjustment module, and then use the laser welding module to heat the upper part of the initial melting welding point of the micron-sized quartz wire to a molten state. At the same time, based on the information detected in real time by the imaging module, use the position adjustment module to readjust the sample and the micron-sized quartz wire to the center alignment, so as to complete the welding operation.
[0027] Through the above technical scheme conceived by the present application, compared with the prior art, the method can perform two-step welding and two-step position adjustment on the micron-level quartz wire and the sample, and heat and melt the micron-level quartz wire before the micron-level quartz wire and the sample are bonded, so that welding is not prone to welding deviation, welding ablation and other phenomena, achieving high-precision positioning and welding of the micron-level quartz wire, and improving the welding quality of the micron-level quartz wire and the sample.
[0028] As further preferred, the welding method further comprises:
[0029] In step S1, when adjusting the position adjustment module, the end of the micron-sized quartz wire is also clamped by a clamp;
[0030] In step S3, after the initial welding is completed, the fixture releases the micron-sized quartz wire.
[0031] In general, the above technical solutions conceived by this application have the following technical advantages compared with the prior art:
[0032] 1. The technical solution of this application separates the sample and the micron-sized quartz wire before the initial welding, thereby reducing the laser ablation of the sample during the welding process; and through a two-step welding process, the micron-sized quartz wire is melted and the sample position is fine-tuned during fine welding, thereby achieving high-precision alignment of the micron-sized quartz wire and the sample during welding.
[0033] 2. During laser welding, the laser welding module can split a laser beam into multiple beams, and can perform synchronous heating of multiple points on the end of the micron-level quartz wire in the circumferential direction, thereby ensuring balanced and rapid heating and improving welding quality.
[0034] 3. During the entire welding process, the fixture only contacts the quartz rod at the end of the micron-sized quartz wire, and the laser only heats the micron-sized quartz wire without directly heating the sample. This design can effectively reduce the impact of the welding process on the performance of the micron-sized quartz wire and the sample. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is an overall layout diagram of a micron-level quartz wire welding device based on laser melting provided in an embodiment of the present application;
[0036] Figure 2 is a position layout diagram of an imaging module, a sample stage, and a fixture provided in an embodiment of the present application;
[0037] Figure 3 It is a schematic diagram of the state of the micron-sized quartz wire provided in the embodiment of the present application when undergoing secondary melting;
[0038] Figure 4 It is a path distribution diagram of the laser beam provided in an embodiment of the present application.
[0039] Throughout the drawings, the same reference numerals are used to denote the same elements or structures, wherein:
[0040] 1. Rack; 2. Suspension tooling; 3. Micron-grade quartz wire; 4. Sample; 5. Sample stage; 6. Imaging module; 7. Laser beam; 8. Beam splitter; 9. Reflector; 10. Angle adjustment mechanism; 11. Height adjustment mechanism; 12. Tooling adjustment mechanism; 13. Sample stage adjustment mechanism; 14. Fixture; 15. Fixture adjustment mechanism; 16. Support platform. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0042] The following is combined with Figure 1-4 This application is described in further detail.
[0043] The present application embodiment discloses a micron-level quartz wire welding device based on laser melting. Figure 1-4 The laser melting-based micron-grade quartz wire welding device comprises a frame 1, on which a suspension fixture 2, a sample stage 5, a laser welding module, a position adjustment module and an imaging module 6 are arranged. The suspension fixture 2 is used to suspend the micron-grade quartz wire 3 on the frame 1, and the end of the micron-grade quartz wire 3 is provided with a quartz rod retained after drawing; the sample stage 5 is used to support the sample 4 under the micron-grade quartz wire 3; the laser welding module is used to provide a laser beam 7 with adjustable power to form a molten zone in the circumferential direction of the end of the micron-grade quartz wire 3 to achieve welding of the micron-grade quartz wire 3 and the sample 4; the imaging module 6 is used to detect the positions of the micron-grade quartz wire 3 and the sample 4 in real time; the position adjustment module is used to adjust the relative position of the micron-grade quartz wire 3 and the sample 4 based on the information detected in real time by the imaging module 6, and adjust the distance between the laser output from the laser welding module to the surface of the micron-grade quartz wire 3 and the bottom of the end of the micron-grade quartz wire 3, so as to ensure that the micron-grade quartz wire is aligned with the sample.
[0044] When performing the welding operation between the micron-sized quartz wire 3 and the sample 4, the position adjustment module is first adjusted according to the real-time detection result of the imaging module 6, so that the sample 4 is aligned with the center of the micron-sized quartz wire 3, and the sample 4 and the micron-sized quartz wire 3 are in a separated state. Then the laser welding module is started, and the bottom of the end of the micron-sized quartz wire 3 is heated and melted by the laser beam 7 to form a molten zone. Then the laser welding module is turned off, and the relative position of the sample 4 and the micron-sized quartz wire 3 is adjusted by the position adjustment module, so that the sample 4 contacts the molten zone at the end below the micron-sized quartz wire 3, and the molten zone with temperature at the end of the micron-sized quartz wire 3 is combined with the sample 4 to form the initial welding. Then the laser power of the laser welding module is reduced, and the part of the micron-sized quartz wire 3 located above the molten zone is heated to a molten state. At the same time, according to the real-time detection result of the imaging module 6, the sample 4 and the micron-sized quartz wire 3 are adjusted by the position adjustment module so that the two are adjusted to a center alignment posture, and then the laser welding module is turned off to complete the welding.
[0045] Furthermore, the frame 1 includes an optical platform and a suspension mounted on the optical platform, the upper end of the suspension has a crossbar extending laterally to above the sample stage 5, and the suspension fixture 2 is mounted on the crossbar to suspend the micron-grade quartz wire 3 above the sample stage 5. To facilitate the clamping of the suspension fixture 2, both ends of the micron-grade quartz wire 3 used retain a tapered area and a quartz rod. When the micron-grade quartz wire 3 is in a vertical state, the upper quartz rod of the micron-grade quartz wire 3 is clamped by the suspension fixture 2, and the lower end (i.e., the end) of the micron-grade quartz wire 3 is used for welding with the sample 4.
[0046] Further, in order to achieve relative position adjustment between the micron-level quartz wire 3 and the sample 4, in some embodiments, the position adjustment module includes a tool adjustment mechanism 12, and the suspension tool 2 is installed on the crossbar of the suspension through the tool adjustment mechanism 12, and the tool adjustment mechanism 12 is used to drive the suspension tool 2 to adjust the position. The tool adjustment mechanism 12 can be a high-precision multi-degree-of-freedom motion platform or a multi-degree-of-freedom robotic arm. In this embodiment, the tool adjustment mechanism 12 is selected as a micron-level multi-degree-of-freedom motion platform.
[0047] Furthermore, the position adjustment module further includes a sample stage adjustment mechanism 13, which is disposed on the frame 1 and is used to drive the sample stage 5 to adjust its position. The sample stage adjustment mechanism 13 can be a three-dimensional adjustment frame, a multi-degree-of-freedom motion platform or a multi-degree-of-freedom mechanical arm.
[0048] For example, Figure 2 As shown, when the sample stage adjustment mechanism 13 is selected as a three-dimensional adjustment frame, the top platform of the three-dimensional adjustment frame is used to place or fix the sample stage 5. The three-dimensional adjustment frame can drive the sample 4 to adjust the posture with multiple degrees of freedom and can adjust the position of the sample 4 in space.
[0049] In some embodiments, the three-dimensional adjustment frame includes three telescopic rods and a top platform. The lower ends of the three telescopic rods are ball-jointed with the frame 1, and the upper ends are ball-jointed with the top platform. The upper connection points and the lower connection points of the three telescopic rods are distributed in a triangular shape, and the three telescopic rods can be adjusted separately.
[0050] Furthermore, the laser welding module includes a laser, multiple beam splitters 8 and multiple reflectors 9. The laser is preferably a CO2 laser. The power of the laser is adjustable. The laser emitted by the laser is converged at multiple angles on the circumferential surface of the end of the micron-sized quartz wire 3 after being split by the beam splitter 8 and reflected by the reflector 9, so that the end of the micron-sized quartz wire 3 is heated and melted.
[0051] Of course, in other embodiments, the laser welding module may include one or more power-adjustable lasers, and the lasers directly heat and weld the ends of the micron-sized quartz wires 3 .
[0052] Further, in some embodiments, a support platform 16 is installed on the rack 1, and a clearance opening is provided in the support platform 16 for avoiding the sample stage 5. The beam splitter 8 and the reflector 9 in the laser welding module are installed on the support platform 16, and the laser is installed on the rack 1, and its output laser can be received by the reflector 9 or the beam splitter 8 in the support platform 16. In some other embodiments, the laser can also be installed on the support platform 16. Of course, in some other embodiments, the support platform 16 may not be provided, and each laser, beam splitter 8 and reflector 9 are supported on the rack 1 by a supporting member.
[0053] Furthermore, the distance between the laser spot formed by the laser welding module at the micron-sized quartz wire 3 and the bottom of the end below the micron-sized quartz wire 3 can be adjusted; that is, the position of the molten zone formed at the end of the micron-sized quartz wire 3 can be adjusted, and this adjustment method has multiple options.
[0054] For example, by driving the micron-sized quartz wire 3 to be raised and lowered by the tooling adjustment mechanism 12 , the relative displacement of the micron-sized quartz wire 3 and the laser welding module can be achieved, thereby achieving the position adjustment of the melting area.
[0055] For example, the position adjustment module further includes a lifting member disposed on the frame 1 for lifting and lowering the support platform 16. By adjusting the lifting member, the axial adjustment of the laser spot and the end of the micron-sized quartz wire 3 can be achieved, and the position adjustment of the melting area can be achieved. Among them, the lifting member includes but is not limited to a Z-axis linear slide, a cylinder, an electric push rod, a manual telescopic adjustment rod, etc.
[0056] For example, the position adjustment module further includes an angle adjustment mechanism 10 disposed on the support platform 16, and the reflector 9 is mounted on the angle adjustment mechanism 10. By adjusting the angle adjustment mechanism 10, the pitch angle of the reflector 9 can be adjusted, thereby adjusting the pitch angle of the reflected laser, achieving height adjustment of the laser spot on the end of the micron-sized quartz wire 3, and achieving position adjustment of the molten area. The angle adjustment mechanism 10 can be selected as an angle adjustment frame, an electric mirror frame, a cantilever, etc.
[0057] For example, the position adjustment module further includes a height adjustment mechanism 11 installed on the support platform 16, and the beam splitter 8 and the reflector 9 are respectively installed on the support platform 16 through the height adjustment mechanism 11. By adjusting the height adjustment mechanism 11 in sequence, the position adjustment of the light spot formed on the end of the micron-level quartz wire 3 can be achieved. The height adjustment mechanism 11 can be an electric telescopic rod, a pneumatic telescopic rod, or a manual telescopic adjustment rod.
[0058] For ease of understanding, Figure 4A specific implementation scheme is shown. The laser is mounted on a frame 1 (not shown in the figure), a support platform 16 is set up above the frame 1, and the support platform 16 has an escape opening for avoiding the sample stage 5. Three beam splitters 8 and seven reflectors 9 are respectively mounted on the support platform 16 through an angle adjustment mechanism 10 and a height adjustment mechanism 11.
[0059] Among them, a reflector 9 is located at the edge of the support platform 16, which is installed on the corresponding height adjustment mechanism 11 through the angle adjustment mechanism 10, and its reflection surface intersects with the horizontal plane. The reflector 9 is used to reflect the laser emitted by the laser to the top of the support platform 16. Among them, a beam splitter 8 is located in the path of the laser beam 7 reflected by the above-mentioned reflector 9, wherein two beam splitters 8 are symmetrically distributed on both sides of the micron-level quartz wire 3, and two reflectors 9 are symmetrically distributed on both sides of the micron-level quartz wire 3. The two beam splitters 8 correspond to the two laser beams 7 after the first beam splitting, and the two reflectors 9 correspond to the two laser beams 7 after the first beam splitting. The remaining four reflectors 9 are distributed in a matrix around the end of the micron-level quartz wire 3, corresponding to the four laser beams 7 after the second beam splitting. Under this design, three beam splitters 8 and seven reflectors 9 form a lens group for laser beam splitting and reflection, so that the laser beam 7 can be converged on the circumferential surface of the end of the micron-level quartz wire 3 at multiple angles, and the end of the micron-level quartz wire 3 is uniformly heated.
[0060] Specifically, if Figure 4 As shown, when the laser welding module is used, the laser beam 7 emitted by the laser is reflected by the head end reflector 9 (i.e., the reflector 9 located at the edge of the support platform 16, and the reflector 9 is located in the angle adjustment mechanism 10) of the light transmission path, and split by a beam splitter 8, and then the laser beam emitted by the laser is split into two beams. Then, the two laser beams 7 each pass through a reflector 9 and a beam splitter 8, and are reflected and split to form four laser beams 7, and then the four laser beams 7 are respectively reflected by the reflector 9 to the end of the micron-sized quartz wire 3, and the end of the micron-sized quartz wire 3 is heated synchronously at four points to ensure balanced and rapid heating.
[0061] Further, see Figure 1-3 In order to improve the welding quality, the welding device also includes a fixture 14 for clamping the quartz rod at the lower end of the micron-sized quartz wire 3. The fixture 14 is preferably a high-precision temperature-resistant fixture 14, which is designed and processed by MEMS (micro-electromechanical system), and the size of the fixture 14 is in the sub-millimeter order. The fixture 14 can be directly mounted on the frame 1, or indirectly mounted on the frame 1 through a support platform 16. In some embodiments, the fixture 14 has a multi-finger clamp that can be opened and closed to clamp the end quartz rod of the micron-sized quartz wire 3.
[0062] Furthermore, the welding device also includes a fixture adjustment mechanism 15 for driving the fixture 14 to adjust the position. The fixture adjustment mechanism 15 is preferably a multi-degree-of-freedom motion platform. When the multi-degree-of-freedom motion platform is installed on the support platform 16, the fixture 14 is installed on the moving table of the multi-degree-of-freedom motion platform, and can perform high-precision displacement adjustment in the directions of the X-axis, Y-axis and Z-axis under the drive of the multi-degree-of-freedom motion platform. In other embodiments, the fixture adjustment mechanism 15 can also be selected as a multi-degree-of-freedom manipulator, etc. It should be noted that the adjustment accuracy of each position adjustment mechanism is preferably in the micron level.
[0063] Furthermore, the imaging module 6 includes two high-resolution positioning cameras, which are placed at 90 degrees in a horizontal plane and are used to measure the three-dimensional positions of the micron-sized quartz wire 3 and the sample 4 .
[0064] Furthermore, in some embodiments, the welding device also includes a controller for connecting electrical signals to the position adjustment module, the imaging module 6, the laser welding module and the fixture adjustment mechanism 15. The controller is capable of receiving and processing information, and controlling the operation of the imaging module 6, the fixture adjustment mechanism 15 and the laser welding module. The operating principle of the control module is existing technology and will not be elaborated here.
[0065] For example, when the angle adjustment mechanism 10 is selected as an electric mirror frame, after the initial welding is completed, the controller synchronously adjusts the four electric mirror frames distributed in a matrix around the end of the micron-sized quartz wire 3, and raises the laser output by the laser welding module to the surface of the micron-sized quartz wire 3 to above the initial welding point.
[0066] The present application also discloses a welding method based on any of the above-mentioned micron-level quartz wire welding devices based on laser melting. The welding method comprises the following steps:
[0067] S1: By using the imaging module 6 to detect the vertical posture of the micron-sized quartz wire 3, the position adjustment module is adjusted based on the information detected in real time by the imaging module 6, so that the centers of the sample 4 and the micron-sized quartz wire 3 are aligned and a gap is left between the sample 4 and the micron-sized quartz wire 3.
[0068] When the welding device does not have a clamp 14, the micron-sized quartz wire 3 is in a vertical suspension state due to the deadweight of the end quartz rod. When the device has a clamp 14, the micron-sized quartz wire 3 can be clamped by the clamp 14 to position or adjust the end of the micron-sized quartz wire 3 so that the micron-sized quartz wire 3 is suspended vertically.
[0069] Specifically, in some embodiments, a high-resolution positioning camera is used to measure the deviation between the micron-sized quartz wire 3 and the vertical direction, and the center position of the swing of the micron-sized quartz wire 3 is made in the vertical direction by coarsely adjusting the tooling adjustment mechanism 12 at the upper end; a high-precision temperature-resistant clamp 14 fixed on the clamp adjustment mechanism 15 is then used to pull a small conical area and a quartz rod (preferably about 2 mm) retained at the end of the micron-sized quartz wire 3 to fix the micron-sized quartz wire 3 in the vertical direction; a high-resolution camera is used to measure the position deviation of the sample 4 relative to the micron-sized quartz wire 3, and the angle of the sample 4 is adjusted by the three-dimensional adjustment frame below the sample 4, so that the center of the sample 4 is aligned with the center of the micron-sized quartz wire 3, so that the surface of the sample 4 facing the micron-sized quartz wire 3 is kept level. Preferably, the upper surface of the sample 4 is preferably kept at a distance of about 1 mm from the bottom of the micron-sized quartz wire 3.
[0070] S2: The bottom of the end of the micron-sized quartz wire 3 is heated by the laser welding module to melt the bottom of the end of the micron-sized quartz wire 3 to form a molten zone, so that the micron-sized quartz wire 3 is melted for welding or posture adjustment, and then the laser welding module is turned off, and the position adjustment module is adjusted to make the sample 4 contact with the molten zone of the micron-sized quartz wire 3 to form an initial weld.
[0071] When the apparatus has the clamp 14 , the clamp 14 releases the micron-sized quartz wire 3 after the sample 4 comes into contact with the micron-sized quartz wire 3 .
[0072] Specifically, in some embodiments, a CO2 laser is used to heat the end of the micron-sized quartz wire 3, and the heating point is located below the clamp 14, about 2 mm away from the clamping point of the clamp 14, that is, the bottom of the end of the quartz rod; at the same time, the sample 4 is slightly pushed vertically upward by the three-dimensional adjustment frame below the sample 4, and the posture of the sample 4 is kept unchanged during the slightly pushing process, and it only moves in the vertical direction; before the heating point of the sample 4 and the quartz rod are about to contact, the CO2 laser is turned off to prevent the laser from burning and damaging the surface of the sample 4; after the heating point of the sample 4 and the quartz rod are in contact, the clamp 14 slowly releases the micron-sized quartz wire 3, and the release process can be that the jaws in the clamp 14 are partially opened outward to loosen the micron-sized quartz wire 3 to complete the initial welding.
[0073] S3: After the initial welding, the laser power of the laser welding module is reduced, and at the same time, the distance between the laser output from the laser welding module to the surface of the micron-sized quartz wire 3 and the bottom of the end of the micron-sized quartz wire 3 (i.e., the above-mentioned welding point) is increased by the position adjustment module, and then the upper part of the initial melting welding point in the micron-sized quartz wire 3 (i.e., the above-mentioned welding point) is welded by the laser welding module. Figure 3 At the same time, the alignment deviation of the micron-sized quartz wire 3 and the sample 4 is observed in real time by the imaging module 6, and the position adjustment module is used to perform fine adjustment so that the micron-sized quartz wire 3 and the sample 4 are adjusted to the center alignment again, thereby completing the welding operation.
[0074] Specifically, the power of the CO2 laser is reduced, and the horizontal height of the laser beam 7 is raised through the position adjustment module (it can also be: lowering the micron-sized quartz wire 3), and the micron-sized quartz wire 3 is heated by the CO2 laser. The heating part is located a little above the welding point in step S2, preferably about 1 mm away from the welding point, so that it enters a molten state, but the temperature is not too high to burn the sample 4; combined with the alignment deviation, the alignment posture of the micron-sized quartz wire 3 and the sample 4 is adjusted by adjusting the three-dimensional adjustment frame under the sample 4, until the micron-sized quartz wire 3 and the sample 4 are adjusted to the center alignment posture again (the laser welding module can be closed during the adjustment process of the center alignment posture of the micron-sized quartz wire 3 and the sample 4, or before and after the adjustment process), thereby completing the welding operation.
[0075] Regarding the alignment deviation mentioned above, on the one hand, there may be deviations in the alignment process; on the other hand, since the aforementioned initial alignment is performed before laser heating and melting, the position of the micron-sized quartz wire 3 relative to the sample 4 may change during the process of melting at the heating point and then cooling and solidifying, thereby causing alignment deviation of the welding point; in addition, there may be other factors that cause alignment deviation.
[0076] Therefore, this method can reduce the alignment deviation through two-step adjustment, weaken the factors such as the possible change of the position of the micron-sized quartz wire 3 relative to the sample 4 during the previous alignment process due to the melting of the heating point and then cooling and solidification, and by combining the fixture 14 and the special design of the micron-sized quartz wire 3, the straightened state of the sample 4 can be maintained, thereby achieving high-precision alignment in the welding of the micron-sized quartz wire 3 and the sample 4. Separating the sample 4 from the micron-sized quartz wire 3 before the initial welding can reduce the laser ablation of the sample 4 during the welding process and improve the welding quality.
[0077] It should be understood that expressions such as "include" and "may include" used in this application indicate the existence of the disclosed functions, operations or constituent elements, and do not limit one or more additional functions, operations and constituent elements. In this application, terms such as "include" and / or "have" may be interpreted as indicating specific characteristics, numbers, operations, constituent elements, components or combinations thereof, but may not be interpreted as excluding the existence or possibility of adding one or more other characteristics, numbers, operations, constituent elements, components or combinations thereof.
[0078] It should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0079] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0080] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0081] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A welding method, It is characterized in that The welding method is implemented by using a micron-level quartz wire welding device based on laser melting, the welding device comprising a frame (1), on which the following components are arranged: A suspension tool (2) is used to suspend a micron-sized quartz wire (3) on a frame (1), wherein the end of the micron-sized quartz wire (3) is a quartz rod; A sample stage (5) for supporting the sample (4) below the micron-sized quartz wire (3); A laser welding module is used to provide a laser beam (7) with adjustable power to form a molten zone in the circumferential direction of the end of the micron-sized quartz wire (3) to achieve welding of the micron-sized quartz wire (3) and the sample (4); An imaging module (6) for detecting the positions of the micron-sized quartz wire (3) and the sample (4) in real time; A position adjustment module, used for adjusting the relative position of the micron-sized quartz wire (3) and the sample (4) based on information detected in real time by the imaging module (6), and adjusting the distance between the laser outputted by the laser welding module to the surface of the micron-sized quartz wire (3) and the bottom of the end of the micron-sized quartz wire (3), so as to ensure that the micron-sized quartz wire is aligned with the sample; The welding method comprises the following steps: S1. Based on the information detected in real time by the imaging module (6), the position adjustment module is adjusted to align the sample (4) with the center of the micron-sized quartz wire (3), and a gap is left between the sample (4) and the micron-sized quartz wire (3); S2. The bottom of the end of the micron-sized quartz wire (3) is melted by a laser welding module to form a molten zone, and the sample (4) is brought into contact with the molten zone of the micron-sized quartz wire (3) by a position adjustment module to complete the initial welding; S3. The laser power of the laser welding module is reduced, and at the same time, the distance between the laser output from the laser welding module to the surface of the micron-sized quartz wire (3) and the bottom of the end of the micron-sized quartz wire (3) is increased through the position adjustment module. Then, the laser welding module is used to heat the upper part of the initial melting welding point of the micron-sized quartz wire (3) to a molten state. At the same time, based on the information detected in real time by the imaging module (6), the position adjustment module is used to readjust the sample (4) and the micron-sized quartz wire (3) to be aligned with the center, thereby completing the welding operation.
2. The welding method according to claim 1, It is characterized in that The welding device used in the welding method also includes a clamp (14) for clamping the end of the micron-sized quartz wire (3), and the welding method also includes: In step S1, when adjusting the position adjustment module, the end of the micron-sized quartz wire (3) is also clamped by the clamp (14); In step S3, after the initial welding is completed, the clamp (14) releases the micron-sized quartz wire (3).
3. The welding method according to claim 1, It is characterized in that In the welding device used in the welding method, the laser welding module comprises a laser, a plurality of beam splitters (8) and a plurality of reflectors (9); the power of the laser is adjustable; the laser beam (7) emitted by the laser is reflected by the reflector (9) and split by the beam splitter (8) and then converges at multiple angles on the circumferential surface of the end of a micron-sized quartz wire (3).
4. The welding method according to claim 3, It is characterized in that In the welding device used in the welding method, the position adjustment module comprises an angle adjustment mechanism (10) arranged on a frame (1), and the angle adjustment mechanism (10) is used to adjust the pitch angle of the reflector (9).
5. The welding method according to claim 3, It is characterized in that In the welding device used in the welding method, a reflection surface of one of the reflectors (9) intersects with a horizontal plane, and the position adjustment module comprises a height adjustment mechanism (11) arranged on a frame (1) and used for lifting and lowering the reflector (9).
6. The welding method according to claim 1, It is characterized in that In the welding device used in the welding method, the position adjustment module comprises a tool adjustment mechanism (12) arranged on a frame (1) and used for driving a suspended tool (2) to adjust its position.
7. The welding method according to claim 1, It is characterized in that In the welding device used in the welding method, the position adjustment module comprises a sample stage adjustment mechanism (13) arranged on a frame (1) and used for driving a sample stage (5) to adjust its position.
8. The welding method according to claim 2, It is characterized in that In the welding device used in the welding method, the welding device also includes a clamp adjustment mechanism (15) for driving the clamp (14) to adjust its position.
Citation Information
Cited By
Quartz wire welding device based on laser melting
CN119897593A
A quartz wire welding device based on laser melting
CN119897593B