Preparation method and application of double liquid grouting material stabilizer

By using ingredients such as comb-type polyacrylamide hyperdispersant in the dual-liquid grouting material stabilizer, the cement hydration reaction time is prolonged and gelled with water glass, which solves the problem of poor reinforcement and sealing effects of grouting materials in dynamic water environments. solve the problem, improve the stability and mechanical properties of the slurry, and meet the construction needs of long-distance transportation and rapid leak plugging.

CN118580018BActive Publication Date: 2024-10-25SHANDONG RIQI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073895.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-25
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Existing grouting materials have poor reinforcement and sealing effects in highly permeable strata in dynamic water environments. They also have slow hydration reaction speed and poor water dispersion resistance, making them unable to meet the construction requirements for rapid leak plugging and long-distance transportation.

Method used

The dual-liquid grouting material stabilizer is used, and the combination of ingredients such as comb-type polyacrylamide hyperdispersant prolongs the hydration reaction time of cement, improves the fluidity and filling properties of the slurry, and rapidly gels with water glass. Prevent slurry from segregating.

Benefits of technology

It can effectively prevent slurry from segregating, increase the fluidity and filling ability of slurry, meet the construction requirements of long-distance transportation and rapid leak plugging, and improve the mechanical properties and water dispersion resistance of grouting materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118580018B_ABST
    Figure CN118580018B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of grouting materials, and discloses a preparation method and application of a dual-liquid grouting material stabilizer. The macromolecular side chains of a comb-type polyacrylamide superdispersant form crisscross "bridges" between cement particles, play a bridging and filling role, overlap each other to form a three-dimensional network structure, bind various components of the slurry together, and prevent cement and aggregate from being dispersed and separated when falling in water; the sulfonic acid hydrophilic groups in the structure can be dissociated into multi-charged large-molecular-weight sulfonic acid anions, and the strong repulsion of like charges causes the coil-like macromolecules to become curved, thereby increasing the solution viscosity and improving the slurry stability; the silicon powder can use its own large specific surface area to fill the pores of the slurry, exert a physical filling effect, form a mutually staggered network structure, make the slurry denser, shorten the gelation time, increase the mechanical properties of the grouting material, and meet the construction requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grouting materials, in particular to a preparation method and application of a double-liquid grouting material stabilizer. Background Art

[0002] With the rapid development of my country's economy, the scale of transportation and water conservancy construction is getting larger and larger. Due to the increasingly complex conditions of underground transportation and water conservancy projects, problems such as collapse, water inrush, and mud gushing have gradually emerged. In order to solve these problems, people often use grouting technology to reinforce and seal underground projects and water conservancy projects; grouting technology is to prepare materials with filling and bonding properties into slurry, and use appropriate pressurized grouting equipment to inject it into the injected body, such as cracks, pores or holes in the stratum, so that the slurry penetrates and fills, and solidifies and hardens, thereby achieving the purpose of reinforcement and sealing; but at present, there is no research and application of grouting materials suitable for complex geological conditions such as long tunnel pipelines, large pipe diameters, and high cross-sectional water pressure at home and abroad. Therefore, how to solve the problems of slow hydration reaction rate of grouting materials, poor water resistance and dispersion, inability to achieve rapid plugging, and poor reinforcement and plugging effects has become a hot topic of current research.

[0003] Shield construction is the main construction method used in the construction of underwater tunnels and underground tunnels, and grouting materials are a key material that can fill the gap at the shield tail in time and provide support to the surrounding rock mass in time, effectively preventing the collapse of the rock mass and controlling the settlement of the surface. Existing grouting materials are divided into two categories: inorganic and organic materials. Inorganic grouting materials are mainly cement, which has the advantages of wide sources, low prices, stable performance, strong durability, and non-toxicity. However, its setting time is too long and it is easily dispersed by passive water, and the slurry has large shrinkage, so it is not suitable for the reinforcement and plugging of highly permeable formations under dynamic water environments. Organic grouting slurry has good injectability and short setting time, but it is costly and has high storage requirements. The stone body strength is lower than that of cement, and there are major environmental safety issues, which are greatly restricted in the plugging project of highly permeable formations under dynamic water environments.

[0004] To solve this problem, Chinese patent CN108911568B has developed a grouting material additive, including sodium aluminate, β-hemihydrate gypsum, borax, polycarboxylic acid water reducer, hydroxyethyl cellulose ether and sodium polyacrylate, etc., which can be added to the slurry to quickly react with the slurry for hydration and achieve rapid plugging; however, it is not suitable for strong permeability formations under dynamic water environment, and there are problems such as unadjustable solidification time and easy segregation of slurry; double liquid slurry is a slurry formed by mixing liquid A stirred by cement slurry and liquid B composed of water glass, etc., which has the characteristics of short gel time and not easily diluted by groundwater. The present invention aims to synthesize a high-efficiency stabilizer specially used for delayed curing of double liquid slurry, which inhibits the hydration reaction of cement in liquid A, prolongs the fluidity of the slurry, and quickly reacts with liquid B to gel, thereby solving the problems of slurry segregation encountered in underwater construction of grouting materials and meeting the construction requirements of long-distance slurry transportation. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a preparation method and application of a dual-liquid grouting material stabilizer, which can effectively prevent slurry segregation, increase slurry fluidity and filling properties, and meet the construction requirements of long-distance slurry transportation.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A double-liquid grouting material stabilizer comprises the following ingredients in percentage by mass: 15-25% glucose, 10-20% sodium gluconate, 3-5% trehalose, 2-4% xylitol, 1.5-3% air entraining agent, 0.1-0.3% sodium benzoate, 2-5% polycarboxylic acid water reducer, 0.05-0.2% retarder, 1-5% comb-type polyacrylamide superdispersant, 0.05-0.1% early strength agent, and the balance deionized water.

[0008] The preparation method of the comb-shaped polyacrylamide superdispersant is as follows: under a nitrogen atmosphere, 100 parts by weight of acrylamide and deionized water are added to a reaction flask, after stirring evenly, 5-25 parts by weight of a structural formula Styrene sulfonate polyethylene glycol macromolecule, 2-10 parts by weight of olefinic silicon powder and 3-8 parts by weight of ammonium persulfate are reacted at 70-90°C for 1-3h, N,N-dimethylformamide and deionized water are added to precipitate, filtered, washed and dried to obtain a comb-type polyacrylamide superdispersant.

[0009] Furthermore, the preparation method is: placing glucose, sodium gluconate, trehalose, xylitol, air entraining agent, sodium benzoate, polycarboxylic acid water reducer and deionized water in a reaction kettle, stirring for 10-20 minutes at a temperature of 100-120°C and a pressure of 0.4-0.6MPa, adding a retarder, a comb-type polyacrylamide superdispersant and an early strength agent, continuing to stir for 20-40 minutes, filtering and washing, concentrating and drying, grinding through an 80-120 mesh sieve, and obtaining a double-liquid grouting material stabilizer.

[0010] Furthermore, the air entraining agent is triterpenoid saponin, and the early strength agent is triethanolamine.

[0011] Furthermore, the retarder is any one of sodium pyrophosphate, sodium fluorosilicate or citric acid.

[0012] Further, the preparation method of styrene sulfonate polyethylene glycol macromolecule is:

[0013] Step (1), under nitrogen atmosphere, add N-(2-aminoethyl)glycine and methanol to a reaction flask, stir to dissolve, add 4-vinylbenzaldehyde, stir at 20-35°C for 2-5h, then add sodium cyanoborohydride, react at room temperature for 8-16h, filter, concentrate under reduced pressure, separate by column chromatography, and dry to obtain styrene diamine glycine. The preparation reaction formula is as follows:

[0014] ,

[0015] Step (2), under nitrogen atmosphere, add styrene diamine glycine and N, N-dimethylformamide to the reaction flask, stir evenly, add sodium 2-bromoethane sulfonate and triethylamine, react at 60-80°C for 16-32h, extract with ethyl acetate and deionized water, concentrate the organic phase, separate by column chromatography, and obtain styrene sulfonyl glycine. The preparation reaction formula is as follows:

[0016] ,

[0017] Step (3), under nitrogen atmosphere, add polyethylene glycol monomethyl ether and N,N-dimethylformamide to the reaction flask, stir evenly, add styrenesulfonyl glycine, p-toluenesulfonic acid and phenothiazine, react at 120-140°C for 5-12h, concentrate under reduced pressure, and dry to obtain styrenesulfonyl polyethylene glycol macromolecule. The preparation reaction formula is as follows:

[0018] .

[0019] Furthermore, in step (1), the molar ratio of N-(2-aminoethyl)glycine, 4-vinylbenzaldehyde, and sodium cyanoborohydride is 1:1.05-1.2:1.5-2.5.

[0020] Furthermore, in step (2), the molar ratio of styrene diamine glycine, sodium 2-bromoethane sulfonate, and triethylamine is 1:2.3-3.1:4.5-6.

[0021] Furthermore, in step (3), the molar ratio of polyethylene glycol monomethyl ether, styrenesulfonyl glycine, p-toluenesulfonic acid and phenothiazine is 1:2.1-2.3:0.02-0.04:0.005-0.01.

[0022] Furthermore, 100 parts by weight of Portland cement, 10-25 parts by weight of bentonite, 0.5-2.5 parts by weight of a dual-liquid grouting material stabilizer and 360-410 parts by weight of deionized water are evenly mixed to obtain liquid A, and liquid B is prepared from 25-35 parts by weight of water glass with a mass concentration of 1.3-1.4 g / mL and deionized water. Liquid A and liquid B are stirred and mixed at room temperature to obtain a dual-liquid grouting material.

[0023] By adopting the above technical solution, the beneficial effects of the present invention are:

[0024] The invention firstly causes N-(2-aminoethyl)glycine and 4-vinylbenzaldehyde to undergo a reduction amination reaction under the action of sodium cyanoborohydride to obtain styrene diamine glycine, then undergoes a substitution reaction with sodium 2-bromoethane sulfonate to obtain styrene sulfonyl glycine, then undergoes a dehydration esterification reaction with polyethylene glycol monomethyl ether under the action of p-toluenesulfonic acid to obtain styrene sulfonyl polyethylene glycol macromolecules, then initiates polymerization with acrylamide and olefinic silicon powder to obtain a dual-liquid grouting material stabilizer, finally compounds with silicate cement and bentonite to obtain liquid A, and then evenly mixes with liquid B composed of water glass to obtain a dual-liquid grouting material.

[0025] Compared with straight-chain dispersants, comb-type polyacrylamide superdispersants have more long-chain structures, and their macromolecular side chains play an adsorption and bridging role in the slurry. Through the criss-crossing "bridges" between the cement particles through the molecular chains, they play a bridging and filling role, overlapping each other to form a three-dimensional network structure, which binds the various components of the slurry together, so that the cement and aggregate do not disperse or separate when falling in the water, binds more free water, makes the structure denser, and has a good water-resistant dispersion effect; at the same time, the comb-type polyacrylamide superdispersant contains sulfonic acid hydrophilic groups, which can dissociate into multi-charged large molecular weight sulfonic acid anions when dissolved in water. The strong repulsion of like charges turns the coil-like macromolecules into curves, increasing the viscosity of the solution, thereby improving the stability of the slurry.

[0026] The comb-type polyacrylamide superdispersant contains styrene sulfonate polyethylene glycol macromolecules and olefinic silicon powder. Under the action of the initiator, the two form a molecular hybrid material through intermolecular bonding, so that the silicon powder particles are firmly fixed in the polymer matrix. The silicon powder can use its own large specific surface area to fill the pores of the slurry and exert a physical filling effect. At the same time, under the action of calcium hydroxide, a cement hydration product, a hydration reaction occurs to generate a gel substance to fill the pores, thereby improving the strength of the grouting material; at the same time, the long-chain structure of the macromolecular compound in the comb-type polyacrylamide superdispersant adsorbs the fine cement particles onto the molecular chain, connects many particles together, and forms an interlaced network structure, making the slurry denser and shortening the gelation time, thereby increasing the mechanical properties of the grouting material to meet construction requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the mass spectrum of styrenediamineglycine.

[0028] Figure 2 This is the mass spectrum of styrenesulfonylglycine.

[0029] Figure 3 This is the mass spectrum of styrenesulfonate polyethylene glycol macromolecule. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0031] Polyethylene glycol monomethyl ether, industrial product, relative molecular mass 1200.

[0032] Preparation of olefinic silicon powder: 20 g of hydroxylated silicon powder, 100 mL of toluene, 20 mL of KH570 and 0.5 g of hydroquinone are added to a 250 ml single-necked flask, and then the silicon powder is suspended in the mixed solution using a magnetic stirring device. The reactor is then adjusted to react in an oil bath at about 80°C. After reacting for 24 hours, the reaction is cooled to room temperature, and the obtained suspension is centrifuged using a low-speed centrifuge to remove the clear liquid obtained by centrifugation. The solid obtained by centrifugation is redissolved in toluene, and then centrifuged again. This is repeated three times to remove residual KH570 and hydroquinone, and the olefinic silicon powder is obtained after vacuum drying.

[0033] Embodiment 1:

[0034] (1) Under nitrogen atmosphere, add 45 mmol of N-(2-aminoethyl)glycine and 225 mL of methanol to a reaction flask. After stirring to dissolve, add 47.25 mmol of 4-vinylbenzaldehyde and stir at 25 °C for 4 h. Then add 67.5 mmol of sodium cyanoborohydride and react at room temperature for 12 h. Filter, concentrate under reduced pressure, separate by column chromatography, and dry to obtain styrene diamine glycine.

[0035] (2) Under nitrogen atmosphere, 40 mmol of styrene diamine glycine and 480 mL of N,N-dimethylformamide were added to a reaction flask. After stirring evenly, 92 mmol of sodium 2-bromoethane sulfonate and 180 mmol of triethylamine were added. The mixture was reacted at 70 °C for 24 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated and separated by column chromatography to obtain styrene sulfonyl glycine.

[0036] (3) Under nitrogen atmosphere, 30 mmol of polyethylene glycol monomethyl ether and 450 mL of N,N-dimethylformamide were added to the reaction flask. After stirring evenly, 66 mmol of styrenesulfonyl glycine, 0.9 mmol of p-toluenesulfonic acid and 0.21 mmol of phenothiazine were added. The mixture was reacted at 130 °C for 9 h. The mixture was concentrated under reduced pressure and dried to obtain styrenesulfonyl polyethylene glycol macromolecules.

[0037] (4) Under nitrogen atmosphere, add 100 g acrylamide and 600 mL deionized water into a reaction flask. After stirring evenly, add 5 g styrenesulfonate polyethylene glycol macromolecule, 2 g olefinic silicon powder and 5 g ammonium persulfate. React at 80 °C for 2 h. Add N,N-dimethylformamide and deionized water to precipitate. Filter, wash and dry to obtain a comb-type polyacrylamide superdispersant.

[0038] (5) 20% glucose, 15% sodium gluconate, 4% trehalose, 3% xylitol, 2% triterpenoid saponin, 0.2% sodium benzoate, 3% polycarboxylic acid water reducer and 51.65% deionized water were placed in a reactor and stirred at a temperature of 110°C and a pressure of 0.5 MPa for 15 min. 0.1% sodium pyrophosphate, 1% comb-type polyacrylamide superdispersant and 0.05% triethanolamine were added and stirred for 30 min. The mixture was filtered, washed, concentrated and dried, and ground through a 100-mesh sieve to obtain a dual-liquid grouting material stabilizer.

[0039] (6) 100 g of silicate cement, 15 g of bentonite, 0.5 g of a dual-liquid grouting material stabilizer, and 380 g of deionized water were mixed evenly to obtain liquid A. Liquid B was prepared by mixing 30 g of water glass with a mass concentration of 1.36 g / mL and deionized water. Liquid A and liquid B were stirred and mixed at room temperature to obtain a dual-liquid grouting material.

[0040] Embodiment 2:

[0041] (1) Under nitrogen atmosphere, add 90 mmol of N-(2-aminoethyl)glycine and 450 mL of methanol to a reaction flask. After stirring to dissolve, add 94.5 mmol of 4-vinylbenzaldehyde and stir at 35 °C for 2 h. Then add 180 mmol of sodium cyanoborohydride and react at room temperature for 8 h. Filter, concentrate under reduced pressure, separate by column chromatography, and dry to obtain styrene diamine glycine.

[0042] (2) Under nitrogen atmosphere, add 85 mmol of styrene diamine glycine and 1020 mL of N,N-dimethylformamide to a reaction flask. After stirring evenly, add 195.5 mmol of sodium 2-bromoethane sulfonate and 382.5 mmol of triethylamine. The mixture is reacted at 80°C for 16 h. The mixture is extracted with ethyl acetate and deionized water. The organic phase is concentrated and separated by column chromatography to obtain styrene sulfonyl glycine.

[0043] (3) Under nitrogen atmosphere, 60 mmol of polyethylene glycol monomethyl ether and 900 mL of N,N-dimethylformamide were added to the reaction flask. After stirring evenly, 126 mmol of styrenesulfonyl glycine, 1.2 mmol of p-toluenesulfonic acid and 0.3 mmol of phenothiazine were added. The mixture was reacted at 140 °C for 5 h. The mixture was concentrated under reduced pressure and dried to obtain styrenesulfonyl polyethylene glycol macromolecules.

[0044] (4) Under nitrogen atmosphere, add 100 g acrylamide and 500 mL deionized water into a reaction flask. After stirring evenly, add 10 g styrenesulfonate polyethylene glycol macromolecule, 4 g olefinic silicon powder and 3 g ammonium persulfate. React at 90 °C for 1 h. Add N,N-dimethylformamide and deionized water to precipitate. Filter, wash and dry to obtain a comb-type polyacrylamide superdispersant.

[0045] (5) 15% glucose, 20% sodium gluconate, 3% trehalose, 4% xylitol, 1.5% triterpenoid saponin, 0.1% sodium benzoate, 5% polycarboxylic acid water reducer and 49.15% deionized water were placed in a reactor and stirred at a temperature of 120°C and a pressure of 0.6 MPa for 10 min. 0.2% sodium fluorosilicate, 2% comb-type polyacrylamide superdispersant and 0.05% triethanolamine were added and stirred for 20 min. The mixture was filtered, washed, concentrated and dried, and ground through a 120-mesh sieve to obtain a dual-liquid grouting material stabilizer.

[0046] (6) 100 g of silicate cement, 10 g of bentonite, 1 g of a dual-liquid grouting material stabilizer, and 360 g of deionized water were mixed evenly to obtain liquid A. Liquid B was prepared by mixing 25 g of water glass with a mass concentration of 1.4 g / mL and deionized water. Liquid A and liquid B were stirred and mixed at room temperature to obtain a dual-liquid grouting material.

[0047] Embodiment 3:

[0048] (1) Under nitrogen atmosphere, add 35 mmol of N-(2-aminoethyl)glycine and 350 mL of methanol to a reaction flask. After stirring to dissolve, add 42 mmol of 4-vinylbenzaldehyde and stir at 20°C for 5 h. Then add 87.5 mmol of sodium cyanoborohydride and react at room temperature for 16 h. Filter, concentrate under reduced pressure, separate by column chromatography, and dry to obtain styrene diamine glycine.

[0049] (2) Under nitrogen atmosphere, 30 mmol of styrene diamine glycine and 600 mL of N,N-dimethylformamide were added to a reaction flask. After stirring evenly, 93 mmol of sodium 2-bromoethane sulfonate and 180 mmol of triethylamine were added. The mixture was reacted at 60 °C for 32 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated and separated by column chromatography to obtain styrene sulfonyl glycine.

[0050] (3) Under nitrogen atmosphere, 25 mmol of polyethylene glycol monomethyl ether and 625 mL of N,N-dimethylformamide were added to the reaction flask. After stirring evenly, 57.5 mmol of styrenesulfonyl glycine, 1 mmol of p-toluenesulfonic acid and 0.25 mmol of phenothiazine were added. The mixture was reacted at 120 °C for 12 h. The mixture was concentrated under reduced pressure and dried to obtain styrenesulfonyl polyethylene glycol macromolecules.

[0051] (4) Under nitrogen atmosphere, add 100 g acrylamide and 750 mL deionized water into a reaction flask. After stirring evenly, add 15 g styrenesulfonate polyethylene glycol macromolecule, 6 g olefinic silicon powder and 8 g ammonium persulfate. React at 70 °C for 3 h. Add N,N-dimethylformamide and deionized water to precipitate. Filter, wash and dry to obtain a comb-type polyacrylamide superdispersant.

[0052] (5) 25% glucose, 10% sodium gluconate, 5% trehalose, 2% xylitol, 3% triterpenoid saponin, 0.3% sodium benzoate, 2% polycarboxylic acid water reducer and 49.55% deionized water were placed in a reactor and stirred at a temperature of 100°C and a pressure of 0.4 MPa for 20 min. 0.05% citric acid, 3% comb-type polyacrylamide superdispersant and 0.1% triethanolamine were added and the mixture was stirred for 40 min. The mixture was filtered, washed, concentrated and dried, and ground through an 80-mesh sieve to obtain a dual-liquid grouting material stabilizer.

[0053] (6) 100 g of silicate cement, 25 g of bentonite, 1.5 g of a dual-liquid grouting material stabilizer, and 410 g of deionized water were mixed evenly to obtain liquid A. Liquid B was prepared by mixing 35 g of water glass with a mass concentration of 1.3 g / mL and deionized water. Liquid A and liquid B were stirred and mixed at room temperature to obtain a dual-liquid grouting material.

[0054] Embodiment 4:

[0055] (1) Under nitrogen atmosphere, add 28 mmol of N-(2-aminoethyl)glycine and 180 mL of methanol to a reaction flask. After stirring to dissolve, add 32.2 mmol of 4-vinylbenzaldehyde and stir at 30°C for 4 h. Then add 52 mmol of sodium cyanoborohydride and react at room temperature for 15 h. Filter, concentrate under reduced pressure, separate by column chromatography, and dry to obtain styrene diamine glycine.

[0056] (2) Under nitrogen atmosphere, add 22 mmol of styrene diamine glycine and 330 mL of N,N-dimethylformamide to a reaction flask. After stirring evenly, add 55 mmol of sodium 2-bromoethane sulfonate and 120 mmol of triethylamine. The mixture is reacted at 75 °C for 24 h. The mixture is extracted with ethyl acetate and deionized water. The organic phase is concentrated and separated by column chromatography to obtain styrene sulfonyl glycine.

[0057] (3) Under nitrogen atmosphere, 18 mmol of polyethylene glycol monomethyl ether and 400 mL of N,N-dimethylformamide were added to the reaction flask. After stirring evenly, 40.5 mmol of styrenesulfonyl glycine, 0.45 mmol of p-toluenesulfonic acid and 0.15 mmol of phenothiazine were added. The mixture was reacted at 135 °C for 10 h. The mixture was concentrated under reduced pressure and dried to obtain styrenesulfonyl polyethylene glycol macromolecules.

[0058] (4) Under nitrogen atmosphere, add 100 g acrylamide and 650 mL deionized water into a reaction flask. After stirring evenly, add 20 g styrenesulfonate polyethylene glycol macromolecule, 8 g olefinic silicon powder and 7 g ammonium persulfate. React at 75 °C for 3 h. Add N,N-dimethylformamide and deionized water to precipitate. Filter, wash and dry to obtain a comb-type polyacrylamide superdispersant.

[0059] (5) 22% glucose, 18% sodium gluconate, 4% trehalose, 4% xylitol, 2% triterpenoid saponin, 0.2% sodium benzoate, 3% polycarboxylic acid water reducer and 42.56% deionized water were placed in a reactor and stirred at a temperature of 115 °C and a pressure of 0.55 MPa for 15 min. 0.15% sodium pyrophosphate, 4% comb-type polyacrylamide superdispersant and 0.09% triethanolamine were added and stirred for 35 min. The mixture was filtered, washed, concentrated and dried, and ground through a 110-mesh sieve to obtain a dual-liquid grouting material stabilizer.

[0060] (6) 100 g of silicate cement, 20 g of bentonite, 2.5 g of a dual-liquid grouting material stabilizer, and 400 g of deionized water were mixed evenly to obtain liquid A. Liquid B was prepared by mixing 32 g of water glass with a mass concentration of 1.35 g / mL and deionized water. Liquid A and liquid B were stirred and mixed at room temperature to obtain a dual-liquid grouting material.

[0061] Embodiment 5:

[0062] (1) Under nitrogen atmosphere, add 20 mmol of N-(2-aminoethyl)glycine and 150 mL of methanol to a reaction flask. After stirring to dissolve, add 22.4 mmol of 4-vinylbenzaldehyde and stir at 35 °C for 4 h. Then add 37 mmol of sodium cyanoborohydride and react at room temperature for 12 h. Filter, concentrate under reduced pressure, separate by column chromatography, and dry to obtain styrene diamine glycine.

[0063] (2) Under nitrogen atmosphere, 15 mmol of styrene diamine glycine and 300 mL of N,N-dimethylformamide were added to a reaction flask. After stirring evenly, 42 mmol of sodium 2-bromoethane sulfonate and 78 mmol of triethylamine were added. The mixture was reacted at 70 °C for 24 h. The mixture was extracted with ethyl acetate and deionized water. The organic phase was concentrated and separated by column chromatography to obtain styrene sulfonyl glycine.

[0064] (3) Under nitrogen atmosphere, 12 mmol of polyethylene glycol monomethyl ether and 300 mL of N,N-dimethylformamide were added to the reaction flask. After stirring evenly, 25.8 mmol of styrenesulfonyl glycine, 0.3 mmol of p-toluenesulfonic acid and 0.01 mmol of phenothiazine were added. The mixture was reacted at 135 °C for 12 h. The mixture was concentrated under reduced pressure and dried to obtain styrenesulfonyl polyethylene glycol macromolecules.

[0065] (4) Under nitrogen atmosphere, add 100 g acrylamide and 600 mL deionized water into a reaction flask. After stirring evenly, add 25 g styrenesulfonate polyethylene glycol macromolecule, 10 g olefinic silicon powder and 6 g ammonium persulfate. React at 90 °C for 3 h. Add N,N-dimethylformamide and deionized water to precipitate. Filter, wash and dry to obtain a comb-type polyacrylamide superdispersant.

[0066] (5) 25% glucose, 15% sodium gluconate, 5% trehalose, 2% xylitol, 3% triterpenoid saponin, 0.3% sodium benzoate, 2.7% polycarboxylic acid water reducer and 41.7% deionized water were placed in a reactor and stirred at a temperature of 110°C and a pressure of 0.45 MPa for 20 min. 0.2% sodium fluorosilicate, 5% comb-type polyacrylamide superdispersant and 0.1% triethanolamine were added and stirred for 40 min. The mixture was filtered, washed, concentrated and dried, and ground through a 100-mesh sieve to obtain a dual-liquid grouting material stabilizer.

[0067] (6) 100 g of silicate cement, 20 g of bentonite, 2.5 g of a dual-liquid grouting material stabilizer, and 390 g of deionized water were mixed evenly to obtain liquid A. Liquid B was prepared by mixing 30 g of water glass with a mass concentration of 1.4 g / mL and deionized water. Liquid A and liquid B were stirred and mixed at room temperature to obtain a dual-liquid grouting material.

[0068] Comparative Example 1:

[0069] (1) Under a nitrogen atmosphere, 100 g of acrylamide and 600 mL of deionized water were added to a reaction flask. After stirring, 5 g of styrenesulfonyl glycine (prepared in Example 1), 2 g of olefinic silicon powder and 5 g of ammonium persulfate were added. The mixture was reacted at 80° C. for 2 h. N,N-dimethylformamide and deionized water were added to precipitate the mixture. The mixture was filtered, washed and dried to obtain a polyacrylamide hyperdispersant.

[0070] (2) 20% glucose, 15% sodium gluconate, 4% trehalose, 3% xylitol, 2% triterpenoid saponin, 0.2% sodium benzoate, 3% polycarboxylic acid water reducer and 51.65% deionized water were placed in a reactor and stirred at a temperature of 110°C and a pressure of 0.5 MPa for 15 min. 0.1% sodium pyrophosphate, 1% polyacrylamide superdispersant and 0.05% triethanolamine were added and stirred for 30 min. The mixture was filtered, washed, concentrated and dried, and ground through a 100-mesh sieve to obtain a dual-liquid grouting material stabilizer.

[0071] (3) 100 g of silicate cement, 15 g of bentonite, 0.5 g of a dual-liquid grouting material stabilizer, and 380 g of deionized water were mixed evenly to obtain liquid A. Liquid B was prepared by mixing 30 g of water glass with a mass concentration of 1.36 g / mL and deionized water. Liquid A and liquid B were stirred and mixed at room temperature to obtain a dual-liquid grouting material.

[0072] Comparative Example 2:

[0073] (1) Under a nitrogen atmosphere, 100 g of acrylamide and 600 mL of deionized water were added to a reaction flask. After stirring, 5 g of styrene diamine glycine (prepared in Example 1), 2 g of olefinic silicon powder and 5 g of ammonium persulfate were added. The mixture was reacted at 80° C. for 2 h. N,N-dimethylformamide and deionized water were added to precipitate the mixture. The mixture was filtered, washed and dried to obtain a polyacrylamide hyperdispersant.

[0074] (2) 20% glucose, 15% sodium gluconate, 4% trehalose, 3% xylitol, 2% triterpenoid saponin, 0.2% sodium benzoate, 3% polycarboxylic acid water reducer and 51.65% deionized water were placed in a reactor and stirred at a temperature of 110°C and a pressure of 0.5 MPa for 15 min. 0.1% sodium pyrophosphate, 1% polyacrylamide superdispersant and 0.05% triethanolamine were added and stirred for 30 min. The mixture was filtered, washed, concentrated and dried, and ground through a 100-mesh sieve to obtain a dual-liquid grouting material stabilizer.

[0075] (3) 100 g of silicate cement, 15 g of bentonite, 0.5 g of a dual-liquid grouting material stabilizer, and 380 g of deionized water were mixed evenly to obtain liquid A. Liquid B was prepared by mixing 30 g of water glass with a mass concentration of 1.36 g / mL and deionized water. Liquid A and liquid B were stirred and mixed at room temperature to obtain a dual-liquid grouting material.

[0076] Comparative Example 3:

[0077] (1) 20% glucose, 15% sodium gluconate, 4% trehalose, 3% xylitol, 2% triterpenoid saponin, 0.2% sodium benzoate, 3% polycarboxylic acid water reducer and 51.65% deionized water were placed in a reactor and stirred at a temperature of 110 °C and a pressure of 0.5 MPa for 15 min. 0.1% sodium pyrophosphate and 0.05% triethanolamine were added and stirred for 30 min. The mixture was filtered, washed, concentrated and dried, and ground through a 100-mesh sieve to obtain a double-liquid grouting material stabilizer.

[0078] (2) 100 g of silicate cement, 15 g of bentonite, 0.5 g of a dual-liquid grouting material stabilizer, and 380 g of deionized water were mixed evenly to obtain liquid A. Liquid B was prepared by mixing 30 g of water glass with a mass concentration of 1.36 g / mL and deionized water. Liquid A and liquid B were stirred and mixed at room temperature to obtain a dual-liquid grouting material.

[0079] Water bleeding rate test: refer to the method in Appendix A of GB / T 3183-1997 "Masonry Cement", place the A liquid prepared in the example and the comparative example in a measuring cylinder, cover it with a double layer of plastic film, keep it at room temperature for 3 hours, and calculate the ratio of the floating water volume to the total volume.

[0080] Slump test: refer to standard JGJ70-90 "Test method for basic properties of building slurry" for testing; use a cross-sectional cone with an upper diameter of 70mm, a lower diameter of 100mm and a height of 60mm to test the slump of liquid A; place the cone on a flat glass plate, put liquid A into the cone and then lift the cone vertically, the height of the slurry loss is the slump.

[0081] Fluidity test: Take a 50cm×50cm square plate, place a metal cylinder with an inner diameter of 8cm and a height of 8cm in the center of the plate, fill the cylinder with liquid A, pull up the cylinder steadily, and measure the diffusion diameter of liquid A.

[0082] Table 1 Slurry performance test

[0083]

[0084] It can be seen from the test results in the above table that with the increase of the content of the comb-type polyacrylamide superdispersant in the double-liquid grouting material stabilizer, the water seepage rate of the grouting material A liquid decreases significantly, and is only 0.08% in Example 5. At the same time, the slump and fluidity increase appropriately, indicating that after adding the double-liquid grouting material stabilizer to the A liquid, the solidification of the A liquid can be delayed, and it has good compatibility with cement, meeting the material performance indicators required to prevent the pipe segment from floating; this is because, on the one hand, compared with the linear dispersant, the comb-type polyacrylamide superdispersant has more long-chain structures, and its macromolecular side chains play an adsorption and bridging role in the slurry. , through the criss-crossing "bridges" formed by molecular chains between cement particles, they play a bridging and filling role, overlapping each other to form a three-dimensional network structure, binding the various components of the slurry together, so that cement and aggregate do not disperse or segregate when falling in the water, binding more free water, making the structure denser, and having a good water-resistant dispersion effect; on the other hand, the comb-type polyacrylamide superdispersant contains sulfonic acid hydrophilic groups, which can dissociate into multi-charged and large molecular weight sulfonic acid anions when dissolved in water. The strong repulsion of like charges turns the coil-like macromolecules into curved shapes, increasing the viscosity of the solution, thereby improving the stability of the slurry.

[0085] Comparative Example 1 does not contain polyethylene glycol long-chain compounds, does not form a three-dimensional network structure, and has a high water seepage rate; Comparative Example 2 does not contain polyethylene glycol long-chain compounds and sulfonic acid groups, only contains carboxylic acid hydrophilic groups, and has limited adsorption performance for cement; Comparative Example 3 does not contain comb-type polyacrylamide superdispersant, the slurry has poor water dispersibility and the worst stability.

[0086] Compressive strength test: Mix liquid A and liquid B evenly and pour them into a specimen mold (a 5 cm cube) before gelling. Use a uniaxial compressive strength tester to measure the compressive strength after 1 hour, 1 day and 28 days. Take the average value of the three tests.

[0087] Table 2 Compressive strength test

[0088]

[0089] It can be seen from the test results in the above table that with the increase of the content of the comb-type polyacrylamide superdispersant in the double-liquid grouting material stabilizer, the compressive strength of the grouting material gradually increases. The compressive strength of Example 4 after 28 days reaches 16.56MPa, while that of Comparative Example 3 is only 6.02MPa. This is because the comb-type polyacrylamide superdispersant contains styrene sulfonate-based polyethylene glycol macromolecules and olefinic silicon powder. Under the action of the initiator, the two form a molecular hybrid material through intermolecular bonding, so that the silicon powder particles are firmly fixed in the polymer matrix. The silicon powder can use its own large specific surface area to fill the pores of the slurry and exert a physical filling effect. At the same time, under the action of the cement hydration product calcium hydroxide, a hydration reaction occurs to generate a gel substance to fill the pores, thereby improving the strength of the grouting material; at the same time, the long-chain structure of the macromolecular compound in the comb-type polyacrylamide superdispersant adsorbs the fine cement particles onto the molecular chain, connects many particles together, and forms an interlaced network structure, making the slurry denser, thereby increasing the mechanical properties of the grouting material.

[0090] Gel time test: Mix liquid A and liquid B according to the designed mixing ratio. Use the cup inversion method to pour the cups containing liquid A and liquid B back and forth until the liquid loses fluidity, which is the gel state. Measure the time from the two liquids mixing to losing fluidity (gelling).

[0091] Table 3 Gel time test

[0092]

[0093] The present application is described in detail above in conjunction with specific implementation methods and exemplary examples, but these descriptions cannot be understood as limiting the present application. Those skilled in the art understand that, without departing from the spirit and scope of the present application, a variety of equivalent replacements, modifications or improvements can be made to the technical solution of the present application and its implementation methods, all of which fall within the scope of the present application. The scope of protection of the present application shall be subject to the attached claims.

Claims

1. A dual-liquid grouting material stabilizer, characterized in that: The double liquid grouting material stabilizer comprises the following components in percentage by mass: 15-25% glucose, 10-20% sodium gluconate, 3-5% trehalose, 2-4% xylitol, 1.5-3% air entraining agent, 0.1-0.3% sodium benzoate, 2-5% polycarboxylic acid water reducer, 0.05-0.2% retarder, 1-5% comb-type polyacrylamide superdispersant, 0.05-0.1% early strength agent, and the balance deionized water; The preparation method of the comb-shaped polyacrylamide superdispersant is as follows: under a nitrogen atmosphere, 100 parts by weight of acrylamide and deionized water are added to a reaction flask, after stirring evenly, 5-25 parts by weight of a compound having a structural formula Styrene sulfonate polyethylene glycol macromolecule, 2-10 parts by weight of olefinic silicon powder and 3-8 parts by weight of ammonium persulfate are reacted at 70-90°C for 1-3h, N,N-dimethylformamide and deionized water are added to precipitate, filtered, washed and dried to obtain a comb-type polyacrylamide superdispersant.

2. A method for preparing a double-liquid grouting material stabilizer as claimed in claim 1, characterized in that: The preparation method comprises the following steps: placing glucose, sodium gluconate, trehalose, xylitol, air entraining agent, sodium benzoate, polycarboxylic acid water reducer and deionized water in a reaction kettle, stirring for 10-20 minutes at a temperature of 100-120° C. and a pressure of 0.4-0.6 MPa, adding a retarder, a comb-type polyacrylamide superdispersant and an early strength agent, continuing stirring for 20-40 minutes, filtering and washing, concentrating and drying, grinding and passing through an 80-120 mesh sieve, and obtaining a dual-liquid grouting material stabilizer.

3. The method for preparing the double-liquid grouting material stabilizer according to claim 2, characterized in that: The air entraining agent is triterpenoid saponin, and the early strength agent is triethanolamine.

4. The method for preparing the double-liquid grouting material stabilizer according to claim 2, characterized in that: The retarder is any one of sodium pyrophosphate, sodium fluorosilicate or citric acid.

5. The method for preparing the double-liquid grouting material stabilizer according to claim 2, characterized in that: The preparation method of the styrene sulfonate polyethylene glycol macromolecule is as follows: Step (1), under a nitrogen atmosphere, add N-(2-aminoethyl)glycine and methanol to a reaction flask, stir to dissolve, add 4-vinylbenzaldehyde, stir at 20-35°C for 2-5h, then add sodium cyanoborohydride, react at room temperature for 8-16h, filter, concentrate under reduced pressure, separate by column chromatography, and dry to obtain styrene diamine glycine; Step (2), under a nitrogen atmosphere, add styrene diamine glycine and N, N-dimethylformamide to a reaction flask, stir evenly, add sodium 2-bromoethane sulfonate and triethylamine, react at 60-80° C. for 16-32 hours, extract with ethyl acetate and deionized water, concentrate the organic phase, and separate by column chromatography to obtain styrene sulfonyl glycine; Step (3), under nitrogen atmosphere, add polyethylene glycol monomethyl ether and N,N-dimethylformamide to a reaction flask, stir evenly, add styrenesulfonyl glycine, p-toluenesulfonic acid and phenothiazine, react at 120-140° C. for 5-12 h, concentrate under reduced pressure, and dry to obtain styrenesulfonyl polyethylene glycol macromolecules.

6. The method for preparing the double-liquid grouting material stabilizer according to claim 5, characterized in that: In the step (1), the molar ratio of N-(2-aminoethyl)glycine, 4-vinylbenzaldehyde and sodium cyanoborohydride is 1:1.05-1.2:1.5-2.

5.

7. The method for preparing the double-liquid grouting material stabilizer according to claim 5, characterized in that: In the step (2), the molar ratio of styrene diamine glycine, sodium 2-bromoethane sulfonate and triethylamine is 1:2.3-3.1:4.5-6.

8. The method for preparing the double-liquid grouting material stabilizer according to claim 5, characterized in that: In the step (3), the molar ratio of polyethylene glycol monomethyl ether, styrenesulfonyl glycine, p-toluenesulfonic acid and phenothiazine is 1:2.1-2.3:0.02-0.04:0.005-0.

01.

9. An application of the double liquid grouting material stabilizer as claimed in claim 1 in double liquid grouting materials, characterized in that: 100 parts by weight of silicate cement, 10-25 parts by weight of bentonite, 0.5-2.5 parts by weight of a dual-liquid grouting material stabilizer and 360-410 parts by weight of deionized water are uniformly mixed to obtain liquid A; liquid B is prepared from 25-35 parts by weight of water glass with a mass concentration of 1.3-1.4 g / mL and deionized water; liquid A and liquid B are stirred and mixed at room temperature to obtain a dual-liquid grouting material.