A kind of recycled aggregate concrete and preparation method thereof

By coating the surface of recycled aggregates with a carbon layer and selecting recycled aggregates with high sphericity, the bottleneck problem of water absorption in low-water cement concrete is solved, the water retention and permeability during the cement hydration process are improved, and the water content is reduced. Autoshrinkage rate and improved compressive strength.

CN118580047BActive Publication Date: 2024-10-08SHENZHEN WENKE LANDSCAPE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411070283.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-08
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

In concrete systems with a low water-to-cement ratio and a large amount of cementitious materials, the water absorption bottleneck of existing recycled aggregates results in the need to add more recycled aggregates to improve water absorption properties, but adding too much will affect the fluidity of the slurry. and impair product performance.

Method used

By coating the surface of the recycled aggregate with a carbon layer, the carbon layer is used to lock in moisture and reduce the accumulation of cement powder particles, thereby improving water retention and permeability. At the same time, recycled aggregates with high sphericity and reasonable particle size distribution are selected. to maintain fluidity and uniformity.

Benefits of technology

It continuously provides water during the cement hydration process, reduces the autogenous shrinkage rate, and improves the fluidity and 28-day compressive strength of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of building materials. More specifically, it relates to a recycled aggregate concrete and a preparation method thereof. The product of the present invention includes: silicate cement, silica ash, fly ash, quartz powder, carbon-coated recycled aggregate wet material, water reducer, and water, wherein the carbon-coated recycled aggregate wet material includes recycled aggregate with a carbon-coated layer on the surface; the carbon-coated recycled aggregate wet material includes moisture, and the moisture accounts for 28-32% of the total mass of the carbon-coated recycled aggregate; the D50 of the quartz powder is 0.02-0.03mm; the D50 of the carbon-coated recycled aggregate wet material is 0.3-0.4mm. The sphericity of the recycled aggregate is 8.8-9.0, and the particle size distribution range of the carbon-coated recycled aggregate wet material is 0.15-0.75mm. The product obtained by the present invention can take into account the comprehensive performance of the product, and while ensuring the basic fluidity of the product, a lower autogenous shrinkage value can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of building materials, and more specifically, relates to a recycled aggregate concrete and a preparation method thereof. Background Art

[0002] Recycled aggregate is a porous aggregate with the characteristics of low apparent density, high porosity, high water absorption and fast water absorption rate. When added to concrete, it has the characteristics of internal curing material.

[0003] For concrete, especially for concrete systems with a low water-cement ratio and a large amount of cementitious materials, the water in its internal pores is often unsaturated. The increase in negative pressure in the capillaries will produce greater shrinkage stress and deformation, which will in turn cause matrix cracking, which is extremely detrimental to the safety and durability of the product after the concrete is cured.

[0004] In the prior art, there are improvements by using super absorbent resins, which have high water absorption and water release efficiency, but they are easy to leave holes after use, reducing the density of the material, thus affecting the mechanical properties and durability of the product. Using recycled aggregates is also one of the ways that can be considered. Its own pores can absorb and release water, and it does not deform during the process of absorbing, storing and releasing water, so it can be used as one of the basic skeletons of the product. Summary of the invention

[0005] The technical problem to be solved by the present invention is: the inventors found that although the addition of recycled aggregate can have a certain improvement effect compared with water-absorbing resin, due to the bottleneck of the water absorption rate of recycled aggregate, for concrete systems with low water-cement ratio and large amount of cementitious materials, more recycled aggregate needs to be added to improve it. However, excessive addition will significantly affect the fluidity of the slurry, and excessive addition is harmful to the improvement of product performance. For this problem, the present invention provides a recycled aggregate concrete and a preparation method thereof.

[0006] The purpose of the present invention is to provide a recycled aggregate concrete.

[0007] Another object of the present invention is to provide a method for preparing recycled aggregate concrete.

[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0009] A recycled aggregate concrete comprising the following raw materials in parts by weight:

[0010] 200-220 parts of Portland cement

[0011] 75-80 parts silica fume

[0012] 30-35 parts fly ash

[0013] 25-35 parts quartz powder

[0014] 280-320 parts of carbon-coated recycled aggregate wet material

[0015] 15-20 parts water reducing agent

[0016] 80-85 parts water

[0017] Wherein, the carbon-coated recycled aggregate wet material comprises recycled aggregate with a carbon-coated layer on the surface;

[0018] The carbon-coated recycled aggregate wet material includes water, and the water accounts for 28-32% of the total mass of the carbon-coated recycled aggregate wet material;

[0019] The D50 of the quartz powder is 0.02-0.03 mm;

[0020] The D50 of the carbon-coated recycled aggregate wet material is 0.3-0.4 mm.

[0021] For a concrete system with a low water-binder ratio, the present invention adds recycled aggregate and allows the recycled aggregate to have a certain moisture content when adding it, so that the water required for hydration can be continuously provided during the cement hydration process. However, the inventors found that the pores of the recycled aggregate itself have a very limited effect on the retention of water, and the cement powder particles are relatively fine. In a concrete system with a low water-binder ratio, a small amount of cement powder that has not been fully exposed to water can easily diffuse into the pores on the surface of the recycled aggregate, thereby quickly consuming the water in the recycled aggregate and blocking its surface pores, resulting in excessive consumption of water in the recycled aggregate, and it is also difficult to fully diffuse and penetrate to the outside, so as to continuously provide the water required for hydration in the middle stage of cement hydration; the present invention performs carbon coating on the surface of the recycled aggregate, and uses the carbon coating layer to better lock the water absorbed into the interior of the recycled aggregate. At the same time, since the carbon coating layer and the surface of the recycled aggregate have different affinity for cement particles, the pore blockage problem caused by the accumulation of surface water powder particles is also reduced to a certain extent, making it easy for water to diffuse and penetrate to the outside.

[0022] Furthermore, the silicate cement is selected from any one of P·O 52.5 silicate cement and P·O 42.5 silicate cement.

[0023] Furthermore, the water reducer is selected from any one of a lignin sulfonate water reducer, a melamine water reducer, an aminosulfonate water reducer, and a polycarboxylic acid water reducer.

[0024] Furthermore, in the carbon-coated recycled aggregate wet material, the sphericity of the recycled aggregate is 8.8-9.0, and the particle size distribution range of the carbon-coated recycled aggregate wet material is 0.15-0.75 mm.

[0025] Furthermore, the inventors have found that by selecting recycled aggregates with relatively high sphericity as the basis, the sphericity of the additive formed after the surface is carbonized can also be relatively high. The relatively high sphericity and the presence of the carbon layer on the surface can make the concrete system still have relatively beneficial fluidity after the product is added, thereby making it easier to mix the various materials, especially in a system with a low water-cement ratio. More uniform mixing will further reduce the relative content of cement powder that has not been fully exposed to water in the early stage, thereby avoiding the pore clogging problem caused by it.

[0026] In addition, the inventors have found that if the particle size distribution range is reasonably selected so that it is distributed within a relatively narrow range, the moisture content of the recycled aggregate particles distributed in different parts of the concrete system will be relatively uniform. As a result, during the cement hydration process, the water replenishment will become more uniform, thereby avoiding the increase in autogenous shrinkage due to local stress concentration.

[0027] A method for preparing recycled aggregate concrete, the specific preparation steps comprising:

[0028] Preparation of carbon-coated recycled aggregate:

[0029] The biochar and CMC solution are dispersed evenly to prepare a glue solution, and then the glue solution is mixed evenly with the recycled aggregate at a mass ratio of 1: (2-2.5), and then spray-dried to obtain precursor particles;

[0030] The precursor particles are heated to 500-550°C under inert gas protection, carbonized for 2-4 hours, cooled, discharged, and sieved to obtain carbon-coated recycled aggregate;

[0031] Soaking the obtained carbon-coated recycled aggregate in water, and then adding it to the recycled aggregate concrete;

[0032] Preparation of recycled concrete:

[0033] soaking the obtained carbon-coated recycled aggregate with water to obtain wet carbon-coated recycled aggregate;

[0034] Firstly, silicate cement, silica fume, fly ash and quartz powder are dry-mixed and stirred to obtain a dry mix;

[0035] dispersing a water reducing agent in water to obtain a water reducing agent solution;

[0036] Then, under stirring, add the water reducing agent solution and the carbon-coated recycled aggregate wet material to the dry mix in sequence. After the addition is completed, continue stirring and mixing to complete the preparation of the concrete.

[0037] In the above preparation process, the biochar is first bonded and coated on the surface of the recycled aggregate using CMC as a binder during the spray drying process, and then the CMC is pyrolyzed and carbonized under high temperature conditions through instant thermal carbonization, and finally the carbonization product and the biochar are firmly coated on the surface of the recycled aggregate.

[0038] Further, the heating to 500-550° C. includes:

[0039] The temperature was continuously raised to 500-550°C at a heating rate of 0.8-1.5°C / min.

[0040] During the preparation process, a relatively fast heating rate is selected during the carbonization process of the biochar itself to obtain relatively larger diffusion pore channels. After the introduction of the binder CMC, a slow heating rate is used during the carbonization process. In this way, it can be ensured that during the carbonization process, the CMC is not pyrolyzed too quickly, resulting in weak interface bonding between the surface biochar and the recycled aggregate. Alternatively, too fast pyrolysis will quickly produce gas, which will cause the pore channels to be too large during the diffusion process. Then, the corresponding moisture retention capacity will also decrease.

[0041] Furthermore, the preparation of the glue solution also includes:

[0042] After mixing the biochar and 10% CMC solution in a mass ratio of 1:(6.8-7.2), stir and disperse them with a stirrer at a speed of 800-900r / min for 2-3h.

[0043] Further, the spray drying comprises:

[0044] The inlet air temperature of the spray dryer is controlled to be 140-145°C, the outlet air temperature is controlled to be 110-115°C, and the main disk speed is controlled to be 8500-8700r / min for spray drying. DETAILED DESCRIPTION

[0045] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0046] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0047] Example 1

[0048] Preparation of carbon-coated recycled aggregate:

[0049] Sugarcane bagasse was used as biomass. After dehydration and drying, it was crushed with a universal grinder at a speed of 6000r / min for 30min, passed through an 80-mesh sieve, and then transferred to a carbonization furnace. In an argon atmosphere, the temperature was raised to 700℃ at a rate of 5℃ / min, and carbonized for 4h. The biochar was then cooled to room temperature with the furnace to obtain biochar.

[0050] Mix and dissolve CMC, i.e. carboxymethyl cellulose, and water to obtain a CMC solution with a mass fraction of 10%;

[0051] The biochar and CMC solution were mixed in a mass ratio of 1:6.8, and then stirred and dispersed with a stirrer at a speed of 800 r / min for 2 h to prepare a glue solution;

[0052] The glue and the recycled aggregate were mixed in a mass ratio of 1:2, and then stirred with a stirrer at a speed of 400 r / min for 2 h to obtain a slurry;

[0053] The sphericity of the recycled aggregate is 8.8;

[0054] The obtained slurry was pumped into a spray dryer, fed at a rate of 400 g / min, the inlet air temperature of the spray dryer was controlled to be 140°C, the outlet air temperature was controlled to be 110°C, and the main disk speed was controlled to be 8500 r / min, and spray drying was performed to obtain precursor particles;

[0055] The precursor particles are transferred into a carbonization furnace, and heated to 500°C at a rate of 0.8°C / min in an argon atmosphere. After carbonization for 2 hours, the particles are cooled, discharged, and sieved to obtain particles with a D50 of 0.3 mm and a particle size distribution range of 0.15-0.75 mm, that is, dry carbon-coated recycled aggregates are obtained;

[0056] The obtained dry carbon-coated recycled aggregate was poured into water, soaked for 3 hours, and then filtered out to obtain wet carbon-coated recycled aggregate with a moisture content of 28%;

[0057] The moisture content refers to: based on the total mass of the carbon-coated recycled aggregate wet material, the moisture content is 28% of the total mass;

[0058] Concrete ingredients:

[0059] Calculated by weight, take:

[0060] 200 parts Portland cement

[0061] 75 parts silica fume

[0062] 30 parts fly ash

[0063] 25 parts quartz powder

[0064] 280 parts of carbon-coated recycled aggregate wet material

[0065] 15 parts water reducing agent

[0066] 80 parts water

[0067] The D50 of the quartz powder is 0.02 mm;

[0068] The silicate cement is selected from P·O 52.5 silicate cement;

[0069] The water reducing agent is selected from lignin sulfonate water reducing agent;

[0070] First, silicate cement, silica fume, fly ash and quartz powder are dry-mixed and stirred at a speed of 100 r / min for 30 minutes to obtain a dry mix;

[0071] dispersing a water reducing agent in water to obtain a water reducing agent solution;

[0072] Then, under the stirring state of a rotation speed of 80r / min, add the water reducing agent solution and the carbon-coated recycled aggregate wet material to the dry mix in sequence. After the addition is completed, continue stirring and mixing for 20 minutes to complete the preparation of the concrete.

[0073] Example 2

[0074] Preparation of carbon-coated recycled aggregate:

[0075] Sugarcane bagasse was used as biomass. After dehydration and drying, it was crushed with a universal grinder at a speed of 6000r / min for 30min, passed through an 80-mesh sieve, and then transferred to a carbonization furnace. In an argon atmosphere, the temperature was raised to 700℃ at a rate of 6℃ / min, and carbonized for 4h. The biochar was then cooled to room temperature with the furnace to obtain biochar.

[0076] Mix and dissolve CMC, i.e. carboxymethyl cellulose, and water to obtain a CMC solution with a mass fraction of 10%;

[0077] The biochar and CMC solution were mixed in a mass ratio of 1:7, and then stirred and dispersed with a stirrer at a speed of 850 r / min for 2.5 h to prepare a glue solution;

[0078] The glue and the recycled aggregate were mixed in a mass ratio of 1:2.2, and then stirred with a stirrer at a speed of 400 r / min for 2 h to obtain a slurry;

[0079] The sphericity of the recycled aggregate is 8.9;

[0080] The obtained slurry was pumped into a spray dryer, fed at a rate of 400 g / min, the inlet air temperature of the spray dryer was controlled to be 142°C, the outlet air temperature was controlled to be 112°C, and the main disk speed was controlled to be 8600 r / min, and spray drying was performed to obtain precursor particles;

[0081] The precursor particles are transferred into a carbonization furnace, and heated to 520°C at a rate of 1.2°C / min in an argon atmosphere. After carbonization for 3 hours, the particles are cooled, discharged, and sieved to obtain particles with a D50 of 0.35 mm and a particle size distribution range of 0.15-0.75 mm, that is, dry carbon-coated recycled aggregates.

[0082] The obtained dry carbon-coated recycled aggregate was poured into water, soaked for 3 hours, and then filtered out to obtain wet carbon-coated recycled aggregate with a moisture content of 30%;

[0083] The moisture content refers to: based on the total mass of the carbon-coated recycled aggregate wet material, the moisture content is 30% of the total mass;

[0084] Concrete ingredients:

[0085] Calculated by weight, take:

[0086] 210 parts of Portland cement

[0087] 78 parts silica fume

[0088] 32 parts fly ash

[0089] 28 parts quartz powder

[0090] 300 parts of carbon-coated recycled aggregate wet material

[0091] 18 parts water reducing agent

[0092] 82 parts water

[0093] The D50 of the quartz powder is 0.025 mm;

[0094] The silicate cement is selected from P·O 52.5 silicate cement;

[0095] The water reducing agent is selected from melamine-based water reducing agents;

[0096] First, silicate cement, silica fume, fly ash and quartz powder are dry-mixed and stirred at a speed of 100 r / min for 30 minutes to obtain a dry mix;

[0097] dispersing a water reducing agent in water to obtain a water reducing agent solution;

[0098] Then, under the stirring state of a rotation speed of 80r / min, add the water reducing agent solution and the carbon-coated recycled aggregate wet material to the dry mix in sequence. After the addition is completed, continue stirring and mixing for 20 minutes to complete the preparation of the concrete.

[0099] Example 3

[0100] Preparation of carbon-coated recycled aggregate:

[0101] Sugarcane bagasse was used as biomass. After dehydration and drying, it was crushed with a universal grinder at a speed of 6000r / min for 30min, passed through an 80-mesh sieve, and then transferred to a carbonization furnace. In an argon atmosphere, the temperature was raised to 700℃ at a rate of 7℃ / min, and carbonized for 4h. The biochar was then cooled to room temperature with the furnace to obtain biochar.

[0102] Mix and dissolve CMC, i.e. carboxymethyl cellulose, and water to obtain a CMC solution with a mass fraction of 10%;

[0103] The biochar and CMC solution were mixed in a mass ratio of 1:7.2, and then stirred and dispersed with a stirrer at a speed of 900 r / min for 3 h to prepare a glue solution;

[0104] The glue and the recycled aggregate were mixed in a mass ratio of 1:2.5, and then stirred with a stirrer at a speed of 400 r / min for 2 h to obtain a slurry;

[0105] The sphericity of the recycled aggregate is 9.0;

[0106] The obtained slurry was pumped into a spray dryer, fed at a rate of 400 g / min, the inlet air temperature of the spray dryer was controlled to be 145°C, the outlet air temperature was controlled to be 115°C, and the main disk speed was controlled to be 8700 r / min, and spray drying was performed to obtain precursor particles;

[0107] The precursor particles are transferred into a carbonization furnace, and heated to 550°C at a rate of 1.5°C / min in an argon atmosphere. After carbonization for 4 hours, the particles are cooled, discharged, and sieved to obtain particles with a D50 of 0.4 mm and a particle size distribution range of 0.15-0.75 mm, that is, dry carbon-coated recycled aggregates.

[0108] The obtained dry carbon-coated recycled aggregate was poured into water, soaked for 3 hours, and then filtered out to obtain wet carbon-coated recycled aggregate with a moisture content of 32%;

[0109] The moisture content refers to: based on the total mass of the carbon-coated recycled aggregate wet material, the moisture content is 32% of the total mass;

[0110] Concrete ingredients:

[0111] Calculated by weight, take:

[0112] 220 parts of Portland cement

[0113] 80 parts silica fume

[0114] 35 parts fly ash

[0115] 35 parts quartz powder

[0116] 320 parts of carbon-coated recycled aggregate wet material

[0117] 20 parts water reducing agent

[0118] 85 parts water

[0119] The D50 of the quartz powder is 0.03 mm;

[0120] The silicate cement is selected from P·O 52.5 silicate cement;

[0121] The water reducer is selected from polycarboxylic acid water reducer;

[0122] First, silicate cement, silica fume, fly ash and quartz powder are dry-mixed and stirred at a speed of 100 r / min for 30 minutes to obtain a dry mix;

[0123] dispersing a water reducing agent in water to obtain a water reducing agent solution;

[0124] Then, under the stirring state of a rotation speed of 80r / min, add the water reducing agent solution and the carbon-coated recycled aggregate wet material to the dry mix in sequence. After the addition is completed, continue stirring and mixing for 20 minutes to complete the preparation of the concrete.

[0125] Example 4

[0126] Compared with Example 1, this embodiment is different in that:

[0127] The sphericity of the recycled aggregate is 7.5, and the other conditions remain unchanged.

[0128] Example 5

[0129] Compared with Example 1, this embodiment is different in that:

[0130] The particle size distribution range of the dry packaged carbon recycled aggregate is 0.05-1.5 mm, and the other conditions remain unchanged.

[0131] Comparative Example 1

[0132] The difference between this comparative example and Example 1 is that the recycled aggregate is used directly without carbon coating, and the other conditions remain unchanged.

[0133] Comparative Example 2

[0134] Compared with Example 1, this comparative example has the following differences:

[0135] Preparation of carbon-coated recycled aggregate:

[0136] Sugarcane bagasse was used as biomass. After dehydration and drying, it was crushed with a universal grinder at a speed of 6000r / min for 30min, passed through an 80-mesh sieve, and then transferred to a carbonization furnace. In an argon atmosphere, the temperature was raised to 700℃ at a rate of 5℃ / min, and carbonized for 4h. The biochar was then cooled to room temperature with the furnace to obtain biochar.

[0137] Mix and dissolve CMC, i.e. carboxymethyl cellulose, and water to obtain a CMC solution with a mass fraction of 10%;

[0138] The biochar and CMC solution were mixed in a mass ratio of 1:6.8, and then stirred and dispersed with a stirrer at a speed of 800 r / min for 2 h to prepare a glue solution;

[0139] The glue and the recycled aggregate were mixed in a mass ratio of 1:2, and then stirred with a stirrer at a speed of 400 r / min for 2 h to obtain a slurry;

[0140] The sphericity of the recycled aggregate is 8.8;

[0141] The obtained slurry was pumped into a spray dryer, fed at a rate of 400 g / min, the inlet air temperature of the spray dryer was controlled to be 140°C, the outlet air temperature was controlled to be 110°C, and the main disk speed was controlled to be 8500 r / min, and spray drying was performed to obtain precursor particles;

[0142] The precursor particles are transferred into a carbonization furnace, and heated to 500°C at a rate of 5°C / min in an argon atmosphere. After carbonization for 2 hours, the particles are cooled, discharged, and sieved to obtain particles with a D50 of 0.3 mm and a particle size distribution range of 0.15-0.75 mm, that is, dry carbon-coated recycled aggregates are obtained;

[0143] The obtained dry carbon-coated recycled aggregate was poured into water, soaked for 3 hours, and then filtered out to obtain wet carbon-coated recycled aggregate with a moisture content of 28%;

[0144] The moisture content refers to: based on the total mass of the carbon-coated recycled aggregate wet material, the moisture content is 28% of the total mass;

[0145] The rest of the conditions remain unchanged.

[0146] The performance tests were performed on the products obtained in the examples and comparative examples. The specific test methods and test results are as follows:

[0147] The fluidity of the products obtained in each embodiment and comparative example was tested using an HFD-LDD-3 cement mortar fluidity tester. The detailed test results are shown in Table 1.

[0148] The SBT-AS200 autogenous shrinkage tester was used to measure the 7-day autogenous shrinkage rate of the product according to the bellows method. The detailed test results are shown in Table 1.

[0149] The products obtained in each embodiment and comparative example were cast into test blocks with a specification of 50×60×150 mm. After natural curing for 28 days, the compressive strength of each test block was tested using a YAW-300 fully automatic pressure testing machine. The specific test results are shown in Table 1.

[0150] Table 1: Product performance test results

[0151]

[0152] It can be seen from the test results in Table 1 that the product obtained by the present invention can take into account the comprehensive performance of the product, ensure the basic fluidity of the product, obtain a lower autogenous shrinkage value, and have a relatively higher 28d compressive strength.

[0153] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A recycled aggregate concrete, characterized in that: The invention comprises the following raw materials in parts by weight: 200-220 parts of Portland cement 75-80 parts silica fume 30-35 parts fly ash 25-35 parts quartz powder 280-320 parts of carbon-coated recycled aggregate wet material 15-20 parts water reducing agent 80-85 parts water Wherein, the carbon-coated recycled aggregate wet material comprises recycled aggregate with a carbon-coated layer on the surface; The carbon-coated recycled aggregate wet material includes water, and the water accounts for 28-32% of the total mass of the carbon-coated recycled aggregate wet material; The D50 of the quartz powder is 0.02-0.03 mm; The D50 of the carbon-coated recycled aggregate wet material is 0.3-0.4 mm; The method for preparing the carbon-coated recycled aggregate wet material comprises the following steps: The biochar and CMC solution are dispersed evenly to prepare a glue solution, and then the glue solution is mixed evenly with the recycled aggregate at a mass ratio of 1: (2-2.5), and then spray-dried to obtain precursor particles; The precursor particles are placed under inert gas protection, heated at a rate of 0.8-1.5°C / min, and continuously heated to 500-550°C, and carbonized for 2-4 hours, and then cooled, discharged, and sieved to obtain carbon-coated recycled aggregate. The obtained carbon-coated recycled aggregate is soaked in water to obtain carbon-coated recycled aggregate wet material.

2. The recycled aggregate concrete according to claim 1, characterized in that: The silicate cement is selected from any one of P·O 52.5 silicate cement and P·O 42.5 silicate cement.

3. The recycled aggregate concrete according to claim 1, characterized in that: The water reducer is selected from any one of a lignin sulfonate water reducer, a melamine water reducer, an aminosulfonate water reducer, and a polycarboxylic acid water reducer.

4. The recycled aggregate concrete according to claim 1, characterized in that: In the carbon-coated recycled aggregate wet material, the sphericity of the recycled aggregate is 8.8-9.0, and the particle size distribution range of the carbon-coated recycled aggregate wet material is 0.15-0.75 mm.

5. A method for preparing recycled aggregate concrete according to any one of claims 1 to 4, characterized in that: The specific preparation steps include: Preparation of carbon-coated recycled aggregate wet material: The biochar and CMC solution are dispersed evenly to prepare a glue solution, and then the glue solution is mixed evenly with the recycled aggregate at a mass ratio of 1: (2-2.5), and then spray-dried to obtain precursor particles; The precursor particles are heated to 500-550°C at a heating rate of 0.8-1.5°C / min under an inert gas protection state, and carbonized for 2-4 hours, and then cooled, discharged, and sieved to obtain carbon-coated recycled aggregate; soaking the obtained carbon-coated recycled aggregate with water to obtain wet carbon-coated recycled aggregate; Preparation of recycled concrete: Firstly, silicate cement, silica fume, fly ash and quartz powder are dry-mixed and stirred to obtain a dry mix; dispersing a water reducing agent in water to obtain a water reducing agent solution; Then, under stirring, add the water reducing agent solution and the carbon-coated recycled aggregate wet material to the dry mix in sequence. After the addition is completed, continue stirring and mixing to complete the preparation of the concrete.

6. The method for preparing recycled aggregate concrete according to claim 5, characterized in that: The preparation of the glue solution also includes: After mixing the biochar and 10% CMC solution in a mass ratio of 1:(6.8-7.2), stir and disperse them with a stirrer at a speed of 800-900r / min for 2-3h.

7. The method for preparing recycled aggregate concrete according to claim 5, characterized in that: The spray drying comprises: The inlet air temperature of the spray dryer is controlled to be 140-145°C, the outlet air temperature is controlled to be 110-115°C, and the main disk speed is controlled to be 8500-8700r / min for spray drying.

Citation Information

Patent Citations

  • Cement-based material carbon sequestration internal curing agent as well as preparation and application thereof

    CN112876119A

  • Low-shrinkage recycled high-performance concrete and preparation method thereof

    CN113929381A

  • Method of producing recycled aggregate and method of producing concrete

    JP2024100591A

  • permeable concrete using steelmaking slag and waste carbon nanotube and manufacturing method thereof

    KR102489672B1