A preparation method of quartz composite material and quartz composite material

Through the mixing and stitching of quartz fiber cloth and metal wire, combined with high-temperature oxidation and multiple impregnation treatment, the close connection problem between quartz composite materials and titanium alloy is solved, and the preparation of quartz composite materials with high strength and high efficiency insulating is achieved. , suitable for high temperature and high pressure environments such as missiles.

CN118580090BActive Publication Date: 2024-11-22SHANGHAI FRP RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411065688.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The prior art is difficult to achieve a close connection between quartz composite materials and titanium alloys, especially when the expansion coefficient is different, it is difficult to achieve a firm connection through direct welding, and the temperature resistance of the silicone rubber adhesive is not sufficient to meet high temperatures. Working conditions.

Method used

The quartz fiber cloth and metal wire are mixed and stitched and weaved. After high-temperature oxidation and multiple impregnation treatments, the acidic silicon sol is impregnated, and combined with the negative pressure impregnation process, a quartz composite material with excellent connection properties is prepared.

Benefits of technology

It achieves the close combination of titanium alloy wire and quartz fiber, meets the mechanical and thermal performance requirements in missiles and other fields, is suitable for welding connections of specific shapes, and expands the scope of application of quartz composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application provides a preparation method of a quartz composite material and a quartz composite material, wherein the preparation method of the quartz composite material mainly includes the production of a first prefabricated braid, pretreatment of the first prefabricated braid, high-temperature aerobic treatment, and at least three times of impregnation treatment of the first prefabricated braid with acidic silica sol, thereby obtaining a preform, and then placing the preform in a high-temperature furnace at 700-800°C for 3h-4h, then cooling the high-temperature furnace to room temperature, and then taking out the preform to obtain the quartz composite material. The quartz composite material prepared by the preparation method of the quartz composite material in the present invention can achieve a close combination of titanium alloy wire and quartz fiber, lay the foundation for the later welding process of the quartz composite material and metal parts, and then achieve a close connection with other metal parts, and meet the mechanical, thermal and other performance requirements under special working conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite materials, and in particular to a preparation method of a quartz composite material and a quartz composite material. Background Art

[0002] Multifunctional composite materials are currently a hot topic of research. They have broad application prospects in aerospace, missiles, transportation and other fields. In the field of missiles, the radome is an important component of the missile. It is located at the head of the aircraft and is a component that integrates wave transmission, heat protection, load bearing and corrosion resistance. Therefore, the materials used in the radome generally need to have at least three functions of heat protection / wave transmission / load bearing. In addition, the quartz composite radome located at the head of the aircraft must be tightly connected with the missile metal body or other material parts through a certain connection method, and withstand the mechanical, thermal and other performance requirements of the missile under the working state, in order to achieve the corresponding functions of the missile. For the connection between quartz composite materials and metal parts, the conventional method generally adopts high-temperature resistant silicone rubber through bonding. This method has the advantages of simple operation and good connection effect. The disadvantage is that the temperature resistance of silicone rubber adhesive is generally lower than 400℃. For working conditions exceeding 400℃, a new connection method needs to be adopted. Welding process is a new process for connecting ceramic materials with metal materials. For quartz composite materials and titanium alloys, due to the large difference in their expansion coefficients, it is difficult to achieve a firm connection between the two materials by direct welding.

[0003] Therefore, a new composite material is urgently needed to overcome the above technical problems. Summary of the invention

[0004] In order to overcome the technical problems existing in the prior art, the present application provides a method for preparing a quartz composite material and a quartz composite material, so that the quartz composite material provided by the present application can have good connection performance, thereby solving the problems raised in the above-mentioned background technology.

[0005] The present application provides a method for preparing a quartz composite material, comprising the following steps:

[0006] Step S1: quartz fiber cloth and metal wire are mixed in a layered manner to obtain a mixed component, and the mixed component is then made into a first prefabricated braid by sewing the fiber yarn, wherein the first prefabricated braid is in a flat plate shape, a rotating body cone shape or a special-shaped structure shape, and the first prefabricated braid is processed in sequence in the following manners to obtain a preform;

[0007] Step S2: placing the first prefabricated braid in a high temperature furnace, heating the high temperature furnace to 450° C. to 500° C. and maintaining the temperature for 2 h to 4 h, so that the first prefabricated braid is treated under aerobic high temperature conditions for 2 h to 4 h;

[0008] Step S3: taking the first prefabricated braid out of the high-temperature furnace and placing it in an impregnation tank, and impregnating the first prefabricated braid with a first acidic silica sol;

[0009] Step S4: placing the impregnation tank in an oven, setting the oven temperature at 40° C. to 60° C. and maintaining the temperature until the first acidic silica sol completely turns into a solid state;

[0010] Step S5: taking the first prefabricated braid out of the impregnation tank and placing it in the high-temperature furnace, heating the high-temperature furnace to 400° C. to 500° C., so that the first prefabricated braid is treated under aerobic high-temperature conditions for 2 to 4 hours;

[0011] Step S6: taking the first prefabricated braid out of the high-temperature furnace and placing it in an impregnation tank, and impregnating the first prefabricated braid with a second acidic silica sol;

[0012] Step S7: placing the first prefabricated braid in an oven, setting the temperature of the oven to 70°C to 100°C, and keeping the first prefabricated braid at 70°C to 100°C for 2h to 4h; then transferring the first prefabricated braid into the high-temperature furnace, heating the high-temperature furnace to 400°C to 500°C and maintaining it for 2h to 4h, so that the first prefabricated braid is treated under aerobic high-temperature conditions for 2h to 4h;

[0013] Step S8: repeating the step S6 and the step S7 at least twice to obtain the preform;

[0014] Step S9: taking out the preform and placing it in the high temperature furnace, controlling the high temperature furnace to heat up to 700-800°C at 2-4°C / min, placing the preform for 3h-4h, then cooling the high temperature furnace to room temperature, and taking out the preform to obtain the quartz composite material.

[0015] In some embodiments, the impregnation tank is provided with a pumping pipeline for sucking the first acidic silica sol or the second acidic silica sol into the impregnation tank;

[0016] In addition, step S3 further comprises the following steps:

[0017] Step S31: evacuating the interior of the impregnation tank by a vacuum pump to make the interior of the impregnation tank a negative pressure state, and maintaining the negative pressure state for 10 minutes to 20 minutes;

[0018] Step S32: sucking the first acidic silica sol into the immersion tank through the extraction pipeline, and immersing the first prefabricated braided fabric in the first acidic silica sol, and maintaining the negative pressure state in the immersion tank unchanged during the process of sucking the first acidic silica sol;

[0019] Step S33: closing the extraction pipeline, and continuing to maintain the vacuum pump to continuously evacuate the impregnation tank, so that the impregnation tank maintains a negative pressure state for 60 minutes to 120 minutes;

[0020] Step S34: Turn off the vacuum pump to restore the interior of the impregnation tank to normal pressure.

[0021] In some embodiments, the metal wires are laid out in a spacing of 2 mm to 4 mm to form a metal wire mesh;

[0022] The layering method is to lay a layer of the metal wire mesh between every two layers of the quartz fiber cloth to form the hybrid piece.

[0023] In some embodiments, the material of the metal wire may be any one of TC4 titanium alloy wire and TC6 titanium alloy wire;

[0024] The tex value of the fiber yarn is any one of 570, 190 and 195.

[0025] In some embodiments, the diameter of the metal wire is φ0.05 mm to 0.1 mm;

[0026] The suturing method is a lock-through suturing process or a temporary suturing process, and the suturing needle distance of the suturing method is 4mm~5mm.

[0027] In some embodiments, the quartz fiber cloth may be a quartz glass fiber satin cloth having a thickness of 0.1 mm to 0.3 mm.

[0028] In some embodiments, the concentration of the first acidic silica sol is 45% to 50%;

[0029] The concentration of the second acidic silica sol is 25% to 40%.

[0030] In some embodiments, the pressure of the negative pressure state is negative 0.095 MPa~0.1 MPa.

[0031] In some embodiments, the first prefabricated braid is in the shape of a flat plate, a rotating cone, or a special-shaped structure.

[0032] In some embodiments, the present application further provides a quartz composite material, which is prepared by the preparation method of the quartz composite material described in any of the above embodiments.

[0033] The present invention has at least the following beneficial effects:

[0034] 1. The preparation method of the quartz composite material provided by the present invention realizes the preparation and engineering application of high-strength and high-efficiency heat-insulating composite materials by first mixing quartz and metal and then performing high-temperature oxidation and multiple impregnation processes, and has excellent application prospects;

[0035] 2. The quartz composite material prepared by the preparation method of the quartz composite material provided by the present invention can achieve close bonding between titanium alloy wire and quartz fiber, lay a foundation for the subsequent welding process of the quartz composite material and metal parts, achieve close connection with other metal parts, and meet the mechanical, thermal and other performance requirements under special working conditions, and thus can be applied to the missile field;

[0036] 3. The quartz composite material prepared by the preparation method of the quartz composite material provided by the present invention can be suitable for a first prefabricated braid of a specific shape, such as a flat plate, a conical rotation shape or an ellipsoid shape, which is conducive to the welding connection and forming of the quartz composite material and metal parts, and is also conducive to expanding the application scope of the quartz composite material. DETAILED DESCRIPTION

[0037] The following specific embodiments illustrate the implementation of the present application, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Although the description of the present application will be introduced in conjunction with some embodiments, this does not mean that the features of this application are limited to the implementation. On the contrary, the purpose of introducing the application in conjunction with the implementation is to cover other options or modifications that may be extended based on the claims of the present application. In order to provide a deep understanding of the present application, the following description will include many specific details. The present application can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present application, some specific details will be omitted in the description. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other without conflict.

[0038] The embodiment of the present application provides a preparation method of a quartz composite material, comprising the following steps: step S1: mixing quartz fiber cloth and metal wire in a layered manner to obtain a mixed piece, and then using fiber yarn to sew the mixed piece into a first prefabricated braid, and using the following methods to sequentially treat the first prefabricated braid to obtain a preform, step S2: placing the first prefabricated braid in a high-temperature furnace, heating the high-temperature furnace to 450°C~500°C and maintaining it for 2h~4h, so that the first prefabricated braid is treated under aerobic high-temperature conditions for 2h~4h; step S3: taking the first prefabricated braid out of the high-temperature furnace and placing it in an impregnation tank, and impregnating the first prefabricated braid with a first acidic silica sol; step S4: placing the impregnation tank in an oven, setting the oven temperature at 40°C~60°C and maintaining it until the first acidic silica sol completely becomes solid; step S5: taking the first prefabricated braid out of the impregnation tank and placing it in a high-temperature furnace, heating the high-temperature furnace to 400°C~5 00℃, so that the first prefabricated braid is treated under aerobic high temperature conditions for 2 to 4 hours; step S6: taking the first prefabricated braid out of the high temperature furnace and placing it in an impregnation tank, and impregnating the first prefabricated braid with the second acidic silica sol; step S7: placing the first prefabricated braid in an oven, setting the oven temperature to 70℃~100℃, and keeping the first prefabricated braid at 70℃~100℃ for 2h~4h; then transferring the first prefabricated braid into a high temperature furnace, The temperature furnace is heated to 400°C~500°C and maintained for 2h~4h, so that the first prefabricated braided fabric is treated under aerobic high temperature conditions for 2h~4h; step S8: repeating steps S6 and S7 at least twice to obtain the preform; step S9: taking out the preform and placing it in a high temperature furnace, controlling the high temperature furnace to heat up to 700~800°C at 2~4°C / min, and placing the preform for 3h~4h, then cooling the high temperature furnace to room temperature, and then taking out the preform to obtain the quartz composite material.

[0039] Specifically, the quartz fiber cloth and the metal wire are mixed in a layered manner so that they can be fully mixed and fully contacted, and then the mixed pieces are woven together with fiber yarns so that the mixed body can always remain in a mixed state during a series of subsequent impregnation and high-temperature treatments to avoid the material from spreading and causing poor performance of the final product. The first prefabricated braid is then softened by high-temperature aerobic treatment so that it can be further mixed and combined, and then impregnated with acidic silica sol.

[0040] In some embodiments, a pumping pipeline is provided on the impregnation tank for sucking the first acidic silica sol or the second acidic silica sol into the impregnation tank; in addition, step S3 also includes the following steps: step S31: evacuating the interior of the impregnation tank through a vacuum pump to make the interior of the impregnation tank a negative pressure state, and maintain the negative pressure state for 10min~20min; step S32: sucking the first acidic silica sol into the impregnation tank through the pumping pipeline, and immersing the first prefabricated woven fabric with the first acidic silica sol, and keeping the negative pressure state in the impregnation tank unchanged during the process of sucking the first acidic silica sol; step S33: closing the pumping pipeline, and continuing to keep the vacuum pump to continuously pump air from the impregnation tank, so that the impregnation tank maintains a negative pressure state for 60min~120min; step S34: turning off the vacuum pump to restore the interior of the impregnation tank to normal pressure.

[0041] Specifically, the negative pressure environment helps the silica gel solution to penetrate into the micropores of the substrate more quickly. By applying negative pressure, the gas in the porous material can be discharged, thereby forming a negative pressure state in the impregnation tank, allowing the impregnation liquid to quickly fill the material gaps.

[0042] Due to the negative pressure, the capillary force in the impregnation process is enhanced, thereby accelerating the impregnation speed and being able to penetrate into the internal structure of the material to achieve a more uniform and thorough impregnation effect, thereby promoting the contact between the first acidic silica sol or the second acidic silica sol and the surface of the carrier, enhancing the interaction force between molecules, and helping to improve the durability and stability of the final product. It effectively reduces the time required for the impregnation process and improves production efficiency. By adjusting the penetration depth and uniformity of the impregnation liquid into the material, the physical and chemical properties of the material are optimized. In addition, the negative pressure impregnation process is simpler and easier to implement than the traditional process.

[0043] In some embodiments, the metal wires are laid at a spacing of 2 mm to 4 mm to form a metal wire mesh, and the laying method is to lay a layer of metal wire mesh between every two layers of quartz fiber cloth to form a hybrid piece.

[0044] Specifically, through many experiments, it is known that when the spacing between the metal wires in the metal wire mesh is 2mm~4mm, while ensuring the compact structure of the first prefabricated braid, the first acidic silica sol or the second acidic silica sol can fully penetrate into the pores, and then can penetrate deeper into the internal structure of the first prefabricated braid, achieving a more uniform and thorough impregnation effect, thereby effectively ensuring the comprehensive performance of the final product. In addition, the setting of laying a layer of metal wire mesh between the two layers of quartz fiber cloth makes the mixing effect between the quartz fiber cloth and the metal wire mesh better, thereby providing a guarantee for the comprehensive performance of the final product.

[0045] In some embodiments, the material of the metal wire can be any one of TC4 titanium alloy wire and TC6 titanium alloy wire, and the tex value of the fiber yarn can be any one of 570, 190 and 195.

[0046] Specifically, TC4 titanium alloy wire has excellent specific strength and corrosion resistance as well as good weldability. TC4 titanium alloy wire is added to the quartz composite material to effectively improve the welding performance of the quartz composite material. In addition, fiber yarns of different thicknesses can be selected according to actual needs. After many experimental results, it can be known that for those with high requirements on durability and cost, fiber yarns with a tex value of 570 can be used, for those with high requirements on tensile properties and breathability, fiber yarns with a tex value of 190 can be used, and for those with high requirements on elastic properties and comprehensive properties, fiber yarns with a tex value of 195 can be used.

[0047] In some embodiments, the diameter of the metal wire is φ0.05 mm to 0.1 mm, the suturing method is a lock-through suturing process or a temporary suturing process, and the suturing needle distance of the suturing method is 4 mm to 5 mm.

[0048] Specifically, after many experiments, it is known that when the diameter of the metal wire is φ0.05mm~0.1mm, the mixture can react more fully under high temperature conditions and during the impregnation process, so that the final product can obtain better performance. In addition, by adopting a lock-type through-stitching process for stitching, the fibers can be stitched in the thickness direction, thereby increasing the bonding force between the layers of the quartz composite material, effectively preventing the occurrence of stratification, and thus improving the interlayer strength. At the same time, by increasing the adhesion between the layers, it helps to disperse and absorb impact energy, thereby enhancing impact resistance. By connecting each layer, the voids and gaps inside the material are reduced, the structural integrity of the composite material is improved, and the effect of optimizing the integrity of the structure is achieved. According to its specific stitching method and parameter adjustment, the tensile, compression and other properties of the quartz composite material can be significantly improved.

[0049] It should be pointed out that the stitching process can also be used for stitching, which can also achieve the effect of improving the tensile, compressive and bending properties of the quartz composite material.

[0050] In some embodiments, the quartz fiber cloth may be a quartz glass fiber satin cloth having a thickness of 0.1 mm to 0.3 mm.

[0051] Specifically, quartz glass fiber satin cloth is a high-performance special glass fiber fabric that can provide a high-quality performance foundation for quartz composite materials.

[0052] In some embodiments, the concentration of the first acidic silica sol is 45% to 50%; the concentration of the second acidic silica sol is 25% to 40%.

[0053] In some embodiments, the pressure of the negative pressure state is negative 0.095 MPa~0.1 MPa.

[0054] Specifically, after many experimental results, it can be known that when the pressure range of the negative pressure state is between negative 0.095MPa and 0.1Mpa, the acidic silica sol can better penetrate into the material without affecting the excellent performance of the material itself.

[0055] In some embodiments, the first prefabricated braid is in the shape of a flat plate, a rotating cone, or a special-shaped structure.

[0056] The present application also provides a quartz composite material, which is prepared by the preparation method of the quartz composite material of any of the above embodiments.

[0057] Specifically, the quartz composite material prepared by the preparation method provided in the present application has excellent comprehensive properties.

[0058] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments.

[0059] Example 1

[0060] A flat plate-shaped quartz composite material is prepared according to a target shape and a target size of the quartz composite material.

[0061] The preparation method of the quartz composite material comprises the following steps:

[0062] Step S1: preparing a first prefabricated braid: mixing quartz fiber cloth and metal wire in a layered manner, adopting a quartz fiber yarn puncture and suturing process to prepare a first prefabricated braid with a flat structure, and sequentially treating the first prefabricated braid in the following manner to obtain a preform; wherein the process parameters of the suturing method are shown in Table 1 below;

[0063]

[0064] Step S2: pre-treating the first prefabricated braided fabric: placing the first prefabricated braided fabric in a high temperature furnace, heating the high temperature furnace to 475° C., so that the first prefabricated braided fabric is treated in a high temperature oxygen environment for 3 hours;

[0065] Step S3: Impregnation treatment: take out the first prefabricated woven fabric after the high-temperature aerobic treatment from the high-temperature furnace and place it in the impregnation tank, then seal the tank cover of the impregnation tank, and use a vacuum pump to evacuate the inside of the impregnation tank to a negative pressure of negative 0.1Mpa, and maintain the negative pressure condition for 10 minutes; using the negative pressure environment in the impregnation tank, suck the acidic silica sol with a concentration of 50% into the impregnation tank through the preset extraction pipeline on the impregnation tank, and immerse the first prefabricated woven fabric in the acidic silica sol. Braided fabric, and keep the negative pressure state in the impregnation tank unchanged during the process of inhaling acidic silica sol; close the valve of the extraction pipeline, continue to keep the vacuum pump to evacuate the impregnation tank, so that the pressure of the impregnation tank in the negative pressure state is maintained at negative 0.1Mpa, and turn off the vacuum pump after 120 minutes to restore the impregnation tank to normal pressure; open the cover of the impregnation tank, place the impregnation tank in the oven, set the temperature in the oven to 50℃ and maintain it until the acidic silica sol completely turns into a solid state;

[0066] Step S4: taking out the first prefabricated braided fabric after the dipping treatment from the dipping tank, first removing the attachments on the surface of the first prefabricated braided fabric, and then placing the treated first prefabricated braided fabric in a high-temperature furnace, heating it to 450° C., and treating it under aerobic conditions for 3 hours;

[0067] Step S5: Take out the first prefabricated braided fabric that has been subjected to high-temperature aerobic treatment from the high-temperature furnace, and place it in an impregnation tank, and evacuate the impregnation tank by means of a vacuum pump until the inside of the impregnation tank is evacuated, so that the inside of the impregnation tank is in a negative pressure state, the pressure of the negative pressure state is negative 0.1Mpa, and the negative pressure state is maintained for 10 minutes; thereby, the acidic silica sol with a concentration value of 30% can be sucked into the impregnation tank through a preset extraction pipeline on the impregnation tank by means of the negative pressure state in the impregnation tank, until the acidic silica sol immerses the first prefabricated braided fabric, and the negative pressure state in the impregnation tank is always maintained unchanged during the process of absorbing the acidic silica sol; close the extraction pipeline valve, continue to maintain the vacuum pump to evacuate the impregnation tank, so that the inside of the impregnation tank is maintained in a negative pressure state of negative 0.1Mpa, and after 60 minutes, turn off the vacuum pump to restore the inside of the impregnation tank to a normal pressure state; open the impregnation tank cover and take out the first prefabricated braided fabric;

[0068] Step S6: placing the treated first prefabricated braid into an oven, setting the oven temperature to 80°C, and maintaining the environment at 80°C for 3 hours; then transferring the first prefabricated braid into a high-temperature furnace, heating it to 450°C, and continuously treating it under aerobic conditions for 3 hours;

[0069] Step S7: repeating step S5 and step S6 twice in sequence to obtain a preform;

[0070] Step S8: Take out the preform, clean the attachments on the surface of the preform, control the high-temperature furnace to heat up to 800°C at 2°C / min, and place the preform in an environment of 800°C for 3 hours, then cool the high-temperature furnace to room temperature, and then take out the preform to obtain the quartz composite material.

[0071] Example 2

[0072] A flat plate-shaped quartz composite material is prepared according to a target shape and a target size of the quartz composite material.

[0073] The preparation method of the quartz composite material comprises the following steps:

[0074] Step S1: preparing a first prefabricated braid: mixing quartz fiber cloth and metal wire in a layered manner, adopting a quartz fiber yarn puncture and suturing process to prepare a first prefabricated braid with a flat structure, and sequentially treating the first prefabricated braid in the following manner to obtain a preform; wherein the process parameters of the suturing method are shown in Table 2 below;

[0075]

[0076] Step S2: pre-treating the first prefabricated braided fabric: placing the first prefabricated braided fabric in a high-temperature furnace, heating the high-temperature furnace to 490° C., so that the first prefabricated braided fabric is treated in a high-temperature oxygen environment for 3 hours;

[0077] Step S3: Impregnation treatment: Take out the first prefabricated woven fabric after the high-temperature aerobic treatment from the high-temperature furnace and place it in the impregnation tank, then seal the tank cover of the impregnation tank, and use a vacuum pump to evacuate the inside of the impregnation tank to a negative pressure of 0.098Mpa, and maintain the negative pressure condition for 15 minutes; using the negative pressure environment in the impregnation tank, suck the acidic silica sol with a concentration of 50% into the impregnation tank through the preset extraction pipeline on the impregnation tank, and immerse the first prefabricated woven fabric in the acidic silica sol. Braided fabric, and keep the negative pressure state in the impregnation tank unchanged during the process of inhaling the acidic silica sol; close the valve of the extraction pipeline, continue to keep the vacuum pump to evacuate the impregnation tank, so that the pressure of the impregnation tank in the negative pressure state is maintained at negative 0.098Mpa, and turn off the vacuum pump after 120 minutes to restore the impregnation tank to normal pressure; open the cover of the impregnation tank, place the impregnation tank in the oven, set the temperature in the oven to 50℃ and maintain it until the acidic silica sol completely turns into a solid state;

[0078] Step S4: taking out the first prefabricated braided fabric after the dipping treatment from the dipping tank, first removing the attachments on the surface of the first prefabricated braided fabric, and then placing the treated first prefabricated braided fabric in a high-temperature furnace, heating it to 450° C., and treating it under aerobic conditions for 3 hours;

[0079] Step S5: Take out the first prefabricated braided fabric that has been subjected to high-temperature aerobic treatment from the high-temperature furnace, and place it in an impregnation tank, and evacuate the impregnation tank by means of a vacuum pump until the inside of the impregnation tank is evacuated, so that the inside of the impregnation tank is in a negative pressure state, the pressure of the negative pressure state is -0.098Mpa, and the negative pressure state is maintained for 10 minutes; thereby, the acidic silica sol with a concentration value of 25% can be sucked into the impregnation tank through a preset extraction pipeline on the impregnation tank by means of the negative pressure state in the impregnation tank, until the acidic silica sol immerses the first prefabricated braided fabric, and the negative pressure state in the impregnation tank is always maintained unchanged during the process of absorbing the acidic silica sol; close the extraction pipeline valve, continue to maintain the vacuum pump to evacuate the impregnation tank, so that the inside of the impregnation tank is maintained in a negative pressure state of 0.098Mpa, and after 60 minutes, turn off the vacuum pump to restore the inside of the impregnation tank to a normal pressure state; open the impregnation tank cover and take out the first prefabricated braided fabric;

[0080] Step S6: placing the treated first prefabricated braid into an oven, setting the oven temperature to 80°C, and maintaining the environment at 80°C for 3 hours; then transferring the first prefabricated braid into a high-temperature furnace, heating it to 450°C, and continuously treating it under aerobic conditions for 3 hours;

[0081] Step S7: repeating step S5 and step S6 twice in sequence to obtain a preform;

[0082] Step S8: Take out the preform, clean the attachments on the surface of the preform, control the high-temperature furnace to heat up to 750°C at 3°C / min, and place the preform in an environment of 750°C for 3h, then cool the high-temperature furnace to room temperature, and then take out the preform to obtain the quartz composite material.

[0083] Example 3

[0084] A quartz composite material in the shape of a rotational cone is prepared according to a target shape and a target size of the quartz composite material.

[0085] The preparation method of the quartz composite material comprises the following steps:

[0086] Step S1: preparing a first prefabricated braid: mixing quartz fiber cloth and metal wire in a layered manner, adopting a quartz fiber yarn puncture and suturing process to prepare a first prefabricated braid with a flat structure, and sequentially treating the first prefabricated braid in the following manner to obtain a preform; wherein the process parameters of the suturing method are shown in Table 3 below;

[0087]

[0088] Step S2: pre-treating the first prefabricated braided fabric: placing the first prefabricated braided fabric in a high-temperature furnace, heating the high-temperature furnace to 500° C., so that the first prefabricated braided fabric is treated in a high-temperature oxygen environment for 3 hours;

[0089] Step S3: Impregnation treatment: take out the first prefabricated woven fabric after the high-temperature aerobic treatment from the high-temperature furnace and place it in the impregnation tank, then seal the tank cover of the impregnation tank, and use a vacuum pump to evacuate the inside of the impregnation tank to a negative pressure of negative 0.1Mpa, and maintain the negative pressure condition for 20 minutes; using the negative pressure environment in the impregnation tank, suck the acidic silica sol with a concentration of 50% into the impregnation tank through the preset extraction pipeline on the impregnation tank, and immerse the first prefabricated woven fabric in the acidic silica sol. Braided fabric, and keep the negative pressure state in the impregnation tank unchanged during the process of inhaling acidic silica sol; close the valve of the extraction pipeline, continue to keep the vacuum pump to evacuate the impregnation tank, so that the pressure of the impregnation tank in the negative pressure state is maintained at negative 0.1Mpa, and turn off the vacuum pump after 120 minutes to restore the impregnation tank to normal pressure; open the cover of the impregnation tank, place the impregnation tank in the oven, set the temperature in the oven to 50℃ and maintain it until the acidic silica sol completely turns into a solid state;

[0090] Step S4: taking out the first prefabricated braided fabric after the dipping treatment from the dipping tank, first removing the attachments on the surface of the first prefabricated braided fabric, and then placing the treated first prefabricated braided fabric in a high-temperature furnace, heating it to 500° C., and treating it under aerobic conditions for 3 hours;

[0091] Step S5: Take out the first prefabricated braided fabric that has been subjected to high-temperature aerobic treatment from the high-temperature furnace, and place it in an impregnation tank, and evacuate the impregnation tank by means of a vacuum pump until the inside of the impregnation tank is evacuated, so that the inside of the impregnation tank is in a negative pressure state, the pressure of the negative pressure state is negative 0.1Mpa, and the negative pressure state is maintained for 20 minutes; thereby, the acidic silica sol with a concentration value of 30% can be sucked into the impregnation tank through a preset extraction pipeline on the impregnation tank by means of the negative pressure state in the impregnation tank, until the acidic silica sol immerses the first prefabricated braided fabric, and the negative pressure state in the impregnation tank is always maintained unchanged during the process of absorbing the acidic silica sol; close the extraction pipeline valve, continue to maintain the vacuum pump to evacuate the impregnation tank, so that the inside of the impregnation tank is maintained in a negative pressure state of negative 0.1Mpa, and after 120 minutes, turn off the vacuum pump to restore the inside of the impregnation tank to a normal pressure state; open the impregnation tank cover and take out the first prefabricated braided fabric;

[0092] Step S6: placing the treated first prefabricated braid into an oven, setting the oven temperature to 100°C, and maintaining the environment at 100°C for 3 hours; then transferring the first prefabricated braid into a high-temperature furnace, heating it to 500°C, and continuously treating it under aerobic conditions for 3 hours;

[0093] Step S7: repeating step S5 and step S6 twice in sequence to obtain a preform;

[0094] Step S8: Take out the preform, clean the attachments on the surface of the preform, control the high-temperature furnace to heat up to 800°C at 3°C / min, and place the preform in an environment of 800°C for 3 hours, then cool the high-temperature furnace to room temperature, and then take out the preform to obtain the quartz composite material.

[0095] Comparative Example 1

[0096] A flat plate-shaped quartz composite material is prepared according to a target shape and a target size of the quartz composite material.

[0097] The preparation method of the quartz composite material comprises the following steps:

[0098] Step S1: preparing a first prefabricated braided fabric: stacking quartz fiber cloth in a layered manner, adopting a quartz fiber yarn puncture and stitching process to prepare a first prefabricated braided fabric with a flat structure, and sequentially treating the first prefabricated braided fabric in the following manner to obtain a preform; wherein the process parameters of the stitching method are shown in Table 4 below;

[0099]

[0100] Step S2: pre-treating the first prefabricated braided fabric: placing the first prefabricated braided fabric in a high-temperature furnace, heating the high-temperature furnace to 500° C., so that the first prefabricated braided fabric is treated in a high-temperature oxygen environment for 3 hours;

[0101] Step S3: Impregnation treatment: take out the first prefabricated woven fabric after the high-temperature aerobic treatment from the high-temperature furnace and place it in the impregnation tank, then seal the tank cover of the impregnation tank, and use a vacuum pump to evacuate the inside of the impregnation tank to a negative pressure of negative 0.1Mpa, and maintain the negative pressure condition for 20 minutes; using the negative pressure environment in the impregnation tank, suck the acidic silica sol with a concentration of 50% into the impregnation tank through the preset extraction pipeline on the impregnation tank, and immerse the first prefabricated woven fabric in the acidic silica sol. Braided fabric, and keep the negative pressure state in the impregnation tank unchanged during the process of inhaling acidic silica sol; close the valve of the extraction pipeline, continue to keep the vacuum pump to evacuate the impregnation tank, so that the pressure of the impregnation tank in the negative pressure state is maintained at negative 0.1Mpa, and turn off the vacuum pump after 120 minutes to restore the impregnation tank to normal pressure; open the cover of the impregnation tank, place the impregnation tank in the oven, set the temperature in the oven to 50℃ and maintain it until the acidic silica sol completely turns into a solid state;

[0102] Step S4: taking out the first prefabricated braided fabric after the dipping treatment from the dipping tank, first removing the attachments on the surface of the first prefabricated braided fabric, and then placing the treated first prefabricated braided fabric in a high-temperature furnace, heating it to 500° C., and treating it under aerobic conditions for 3 hours;

[0103] Step S5: Take out the first prefabricated braided fabric that has been subjected to high-temperature aerobic treatment from the high-temperature furnace, and place it in an impregnation tank, and evacuate the impregnation tank by means of a vacuum pump until the inside of the impregnation tank is evacuated, so that the inside of the impregnation tank is in a negative pressure state, the pressure of the negative pressure state is negative 0.1Mpa, and the negative pressure state is maintained for 20 minutes; thereby, the acidic silica sol with a concentration value of 30% can be sucked into the impregnation tank through a preset extraction pipeline on the impregnation tank by means of the negative pressure state in the impregnation tank, until the acidic silica sol immerses the first prefabricated braided fabric, and the negative pressure state in the impregnation tank is always maintained unchanged during the process of absorbing the acidic silica sol; close the extraction pipeline valve, continue to maintain the vacuum pump to evacuate the impregnation tank, so that the inside of the impregnation tank is maintained in a negative pressure state of negative 0.1Mpa, and after 120 minutes, turn off the vacuum pump to restore the inside of the impregnation tank to a normal pressure state; open the impregnation tank cover and take out the first prefabricated braided fabric;

[0104] Step S6: placing the treated first prefabricated braid into an oven, setting the oven temperature to 100°C, and maintaining the environment at 100°C for 3 hours; then transferring the first prefabricated braid into a high-temperature furnace, heating it to 500°C, and continuously treating it under aerobic conditions for 3 hours;

[0105] Step S7: repeating step S5 and step S6 twice in sequence to obtain a preform;

[0106] Step S8: Take out the preform, clean the attachments on the surface of the preform, control the high-temperature furnace to heat up to 800°C at 3°C / min, and place the preform in an environment of 800°C for 3 hours, then cool the high-temperature furnace to room temperature, and then take out the preform to obtain the quartz composite material.

[0107] The performance tests were carried out on the three embodiments and one comparative example obtained above, and the results are shown in Table 5 below.

[0108]

[0109] First, the performance of each sample obtained was tested according to the "Fine Ceramics Bending Strength Test Method" (GB / T 6569-2006), "Fine Ceramics Room Temperature Tensile Strength Test Method" (GB / T 23805-2009), "Fiber Reinforced Plastic Compression Performance Test Method" (GB / T 1448-2005) and "Fiber Reinforced Plastic Interlaminar Shear Strength Test Method" (GB / T 1450.1-2005). It can be seen from Table 5 that the quartz composite material prepared by the preparation method of the quartz composite material provided by the present invention has tensile properties equivalent to those of Comparative Example 1. In addition, according to the "Welded Joint Tensile Test Method" (GB / T The above-obtained samples were tested by the performance testing method of welding tensile strength according to ASTM D 2651-2008. It was found that the welding tensile strength of Comparative Example 1 shown in Table 5 was 0 MPa, while the welding tensile strength of the quartz composite materials prepared in the present application was above 18 MPa. This was mainly because the quartz composite materials in Comparative Example 1 could not achieve a good welding connection with the titanium alloy, while the quartz composite materials prepared in the present application had excellent welding strength. Therefore, the quartz composite materials prepared in the present application could achieve a tight connection with other metal parts and meet the mechanical, thermal and other performance requirements under special working conditions.

[0110] Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and modifications of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and modifications.

Claims

1. A method for preparing a quartz composite material, It is characterized in that The following steps are involved: Step S1: quartz fiber cloth and metal wire mesh are mixed in a layering manner to obtain a mixed component, and the mixed component is made into a first prefabricated braid by using fiber yarn in a suturing manner, and the first prefabricated braid is processed in sequence in the following manners to obtain a preform, wherein the metal wire mesh is formed by laying metal wires in a manner of a spacing of 2 mm to 4 mm, the layering manner is to lay a layer of the metal wire mesh between every two layers of the quartz fiber cloth to form the mixed component, the material of the metal wire is any one of TC4 titanium alloy wire and TC6 titanium alloy wire, the diameter of the metal wire is φ0.05 mm to 0.1 mm, the suturing manner is a lock-through suturing process or a temporary suturing process, and the suturing needle distance of the suturing method is 4 mm to 5 mm; Step S2: placing the first prefabricated braid in a high temperature furnace, heating the high temperature furnace to 450° C. to 500° C. and maintaining the temperature for 2 h to 4 h, so that the first prefabricated braid is treated under aerobic high temperature conditions for 2 h to 4 h; Step S3: taking the first prefabricated braid out of the high-temperature furnace and placing it in an impregnation tank, and impregnating the first prefabricated braid with a first acidic silica sol, wherein the concentration of the first acidic silica sol is 45% to 50%; Step S4: placing the impregnation tank in an oven, setting the oven temperature at 40° C. to 60° C. and maintaining the temperature until the first acidic silica sol completely turns into a solid state; Step S5: taking the first prefabricated braid out of the impregnation tank and placing it in the high-temperature furnace, heating the high-temperature furnace to 400° C. to 500° C., so that the first prefabricated braid is treated under aerobic high-temperature conditions for 2 to 4 hours; Step S6: taking the first prefabricated braid out of the high-temperature furnace and placing it in an impregnation tank, and impregnating the first prefabricated braid with a second acidic silica sol, wherein the concentration of the second acidic silica sol is 25% to 40%; Step S7: placing the first prefabricated braid in an oven, setting the temperature of the oven to 70°C to 100°C, and keeping the first prefabricated braid at 70°C to 100°C for 2h to 4h; then transferring the first prefabricated braid into the high-temperature furnace, heating the high-temperature furnace to 400°C to 500°C and maintaining it for 2h to 4h, so that the first prefabricated braid is treated under aerobic high-temperature conditions for 2h to 4h; Step S8: repeating the step S6 and the step S7 at least twice to obtain the preform; Step S9: Take out the preform and place it in the high temperature furnace, control the high temperature furnace to heat up to 700°C to 800°C at 2 to 4°C / min, and place the preform in an environment of 700°C to 800°C for 3h to 4h, then cool the high temperature furnace to room temperature, and then take out the preform to obtain a quartz composite material.

2. The method for preparing the quartz composite material according to claim 1, It is characterized in that The impregnation tank is provided with a pumping pipeline for sucking the first acidic silica sol or the second acidic silica sol into the impregnation tank; In addition, step S3 further comprises the following steps: Step S31: evacuating the interior of the impregnation tank by a vacuum pump to make the interior of the impregnation tank a negative pressure state, and maintaining the negative pressure state for 10 minutes to 20 minutes; Step S32: sucking the first acidic silica sol into the immersion tank through the extraction pipeline, and immersing the first prefabricated braided fabric in the first acidic silica sol, and maintaining the negative pressure state in the immersion tank unchanged during the process of sucking the first acidic silica sol; Step S33: closing the extraction pipeline, and continuing to maintain the vacuum pump to continuously evacuate the impregnation tank, so that the impregnation tank maintains a negative pressure state for 60 minutes to 120 minutes; Step S34: Turn off the vacuum pump to restore the interior of the impregnation tank to normal pressure.

3. The method for preparing the quartz composite material according to claim 1 or 2, It is characterized in that The tex value of the fiber yarn is any one of 570, 190 and 195.

4. The method for preparing the quartz composite material according to claim 3, It is characterized in that The quartz fiber cloth is a quartz glass fiber satin cloth with a thickness of 0.1 mm to 0.3 mm.

5. The method for preparing the quartz composite material according to claim 2, It is characterized in that The pressure of the negative pressure state is negative 0.095MPa to 0.1Mpa.

6. The method for preparing the quartz composite material according to claim 5, It is characterized in that The first prefabricated braid is in the shape of a flat plate, a rotating cone or a special-shaped structure.

7. A quartz composite material, It is characterized in that The quartz composite material is prepared by the preparation method of any one of claims 1 to 6, and the quartz composite material is used for welding and fixing metal parts to the outside.