A kind of adsorption resin with porous structure and preparation method thereof

The adsorption resin with a porous structure is generated through copolymerization and cross-linking reactions, which solves the problems of low adsorption performance and poor repeatability of existing resins, and achieves efficient adsorption and improved stability of heavy metal ions.

CN118580405BActive Publication Date: 2024-10-11JIANGSU JINSHAN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068909.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-11
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Existing heavy metal ion adsorption resins have low adsorption performance and poor repeatability, and cannot effectively treat wastewater containing heavy metals.

Method used

Through the copolymerization of styrene, methyl cyanoacrylate and 4,4'-divinyl-1,1'-biphenyl, a terpolymer is formed, and a double cross-linked structure is generated through chlorination and cross-linking reactions. Hydroxylamine hydrochloride reacts to form an adsorption resin with a porous structure.

Benefits of technology

It improves the heavy metal adsorption performance and repeatability of the adsorption resin, achieves efficient adsorption and stability of heavy metal ions such as Cu2+ and Pb2+, and maintains a removal rate of more than 88% after 10 adsorption-desorption times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the field of adsorption separation technology, and in particular to an adsorption resin with a porous structure and a preparation method thereof. The present invention forms a terpolymer by copolymerizing styrene, methyl cyanoacrylate and 4,4'-divinyl-1,1'-biphenyl, and then chlorinating the terpolymer by chloromethyl methyl ether, and then cross-linking is generated inside the chlorinated terpolymer by Friedel-Crafts alkylation to generate a double cross-linked structure, and then hydroxylamine hydrochloride is used to react with the ester group and cyano group inside the cross-linked terpolymer to obtain an adsorption resin with a porous structure. The adsorption resin with a porous structure prepared by the present invention has excellent adsorption performance and reproducibility, and is expected to become a new adsorption material for treating heavy metal wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adsorption separation, and in particular to an adsorption resin with a porous structure and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of industry, electroplating, mining, smelting, leather making and other industries have produced a large amount of wastewater containing heavy metal ions. Heavy metal wastewater is highly toxic, easy to accumulate, non-degradable and highly concealed. Once discharged into the water body, it will seriously damage the ecosystem. Therefore, the development of heavy metal wastewater treatment technology is of great practical significance for protecting the ecological environment.

[0003] Patent technology document CN202211130660.2 discloses a modified chelating resin for heavy metal ion adsorption, which is prepared by the following steps: 1) preparing poly(glycidyl methacrylate) resin; 2) performing aminoguanidine functional modification on the resin prepared in step 1); 3) using carbon dots as modifiers to perform adsorption enhancement modification on the resin prepared in step 2) to obtain the modified chelating resin. This invention significantly improves the adsorption performance of the resin for heavy metal ions by introducing a large number of amino groups. However, poly(glycidyl methacrylate) resin is a macroporous cross-linked resin, and its larger pores make its specific surface area lower, so that the adsorption amount is limited, and the repeatability of the cross-linked resin with a macroporous structure is poor. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide an adsorption resin with a porous structure and a preparation method thereof, so as to solve the problems of low adsorption performance and poor repeatability of existing heavy metal ion adsorption resins.

[0005] Based on the above purpose, the present invention provides a method for preparing an adsorption resin with a porous structure, comprising the following steps:

[0006] (1) In a nitrogen atmosphere, styrene, methyl cyanoacrylate and azobisisobutyronitrile are added to ethanol, and then dichloroethane is added, and the temperature is raised to 70-75°C, and the reaction is stirred for 2-3 hours, and then 4,4'-divinyl-1,1'-biphenyl is added, and the reaction is continued by stirring for 20-30 hours. After cooling, purification is performed to obtain a terpolymer;

[0007] (2) At room temperature, the terpolymer is added to dichloroethane and swelled for 5-10 hours, then chloromethyl methyl ether is added and stirred for 10-20 minutes, then anhydrous zinc chloride is added, the temperature is raised to 50-60°C, stirred and reacted for 6-8 hours, cooled, purified, and chlorinated to obtain the terpolymer;

[0008] (3) adding the chlorinated terpolymer to dichloroethane at room temperature, swelling for 5-10 hours, then adding anhydrous ferric chloride, heating to 75-80°C, stirring and reacting for 20-24 hours, cooling, and purifying to obtain a cross-linked terpolymer;

[0009] (4) At room temperature, the cross-linked terpolymer is added to n-butanol and swelled for 4-6 hours. Then, hydroxylamine hydrochloride and sodium hydroxide are added. The temperature is raised to 60-65°C and stirred for reaction for 6-8 hours. After cooling, the mixture is washed with deionized water, and sulfuric acid solution is added to neutralize the sodium hydroxide. Finally, the mixture is purified to obtain an adsorption resin with a porous structure.

[0010] Preferably, in step (1), the weight ratio of styrene, methyl cyanoacrylate, azobisisobutyronitrile, ethanol, ethylene dichloride and 4,4'-divinyl-1,1'-biphenyl is 2-3:0.5-1:0.06-0.08:10-14:0.5-0.7:0.08-0.12.

[0011] Preferably, the purification step in step (1) is: washing with ethanol and then vacuum drying at 60° C. for 48 hours.

[0012] Preferably, in step (2), the weight ratio of the terpolymer, ethylene dichloride, chloromethyl methyl ether and anhydrous zinc chloride is 2-4:30-60:1.5-4.5:2.5-5.2.

[0013] Preferably, the purification step in step (2) is: washing with ethanol and dichloromethane, then Soxhlet extraction with ethanol for 48 hours, and then vacuum drying at 60° C. for 48 hours.

[0014] Preferably, in step (3), the weight ratio of the chlorinated terpolymer, ethylene dichloride and anhydrous ferric chloride is 2-4:30-60:8-15.

[0015] Preferably, the purification step in step (3) is: washing with ethanol and dichloromethane, then Soxhlet extraction with ethanol for 48 hours, and then vacuum drying at 60° C. for 48 hours.

[0016] Preferably, in step (4), the weight ratio of the cross-linked terpolymer, n-butanol, hydroxylamine hydrochloride and sodium hydroxide is 2-4:20-40:0.8-1.6:0.5-1.2.

[0017] Preferably, the purification step in step (4) is: washing with deionized water and ethanol, and then vacuum drying at 60° C. for 48 hours.

[0018] Furthermore, the present invention also provides an adsorption resin with a porous structure, which is obtained according to the preparation method of the adsorption resin with a porous structure.

[0019] Beneficial effects of the present invention:

[0020] The present invention prepares a terpolymer by copolymerizing styrene, methyl cyanoacrylate and 4,4'-divinyl-1,1'-biphenyl, and then chlorinates the terpolymer by chloromethyl methyl ether, and then generates crosslinks inside the chlorinated terpolymer by Friedel-Crafts alkylation to generate a double crosslinking structure, and then utilizes hydroxylamine hydrochloride to react with the ester group and the cyano group inside the crosslinked terpolymer to generate hydroxamic acid with excellent adsorption effect, thereby giving the adsorption resin abundant pores and a large number of adsorption sites, so that the prepared adsorption resin with a porous structure has excellent heavy metal adsorption performance and repeatability.

[0021] The 4,4'-divinyl-1,1'-biphenyl used in the present invention has certain steric hindrance and rotation performance, which helps to prevent excessive cross-linking in the second cross-linking, thereby increasing the grafting rate of hydroxamic acid and further improving the adsorption performance.

[0022] The methyl cyanoacrylate used in the present invention has both an ester group and a cyano group capable of reacting with hydroxylamine hydrochloride, which helps to increase the adsorption sites inside the adsorption resin, thereby improving the adsorption performance, and similar hydroxamic acids can synergistically improve the adsorption stability. DETAILED DESCRIPTION

[0023] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0024] Embodiment 1:

[0025] (1) Under nitrogen atmosphere, 2 g of styrene, 0.5 g of methyl cyanoacrylate and 0.06 g of azobisisobutyronitrile were added to 10 g of ethanol, and then 0.5 g of ethylene dichloride was added. The temperature was raised to 70°C and stirred for reaction for 2 h. Then 0.08 g of 4,4'-divinyl-1,1'-biphenyl was added and the stirring reaction was continued for 20 h. After cooling, the mixture was washed with ethanol and then vacuum dried at 60°C for 48 h to obtain a terpolymer.

[0026] (2) At room temperature, 2 g of the terpolymer was added to 30 g of dichloroethane and swollen for 5 h, then 1.5 g of chloromethyl methyl ether was added and stirred for 10 min, then 2.5 g of anhydrous zinc chloride was added, the temperature was raised to 50 °C, stirred and reacted for 6 h, cooled, washed with ethanol and dichloromethane, and then extracted with ethanol Soxhlet for 48 h to chlorinate the terpolymer;

[0027] (3) At room temperature, 2 g of the chlorinated terpolymer was added to 30 g of dichloroethane and swelled for 5 h, then 8 g of anhydrous ferric chloride was added, the temperature was raised to 75 °C, and the mixture was stirred for reaction for 20 h. After cooling, the mixture was washed with ethanol and dichloromethane, and then extracted with ethanol Soxhlet for 48 h, and then vacuum dried at 60 °C for 48 h to obtain a cross-linked terpolymer;

[0028] (4) At room temperature, 2 g of the cross-linked terpolymer was added to 20 g of n-butanol and allowed to swell for 4 h. Then, 0.8 g of hydroxylamine hydrochloride and 0.5 g of sodium hydroxide were added. The temperature was raised to 60 °C and stirred for reaction for 6 h. After cooling, the mixture was washed with deionized water and sulfuric acid solution was added to neutralize the sodium hydroxide. Finally, the mixture was washed with deionized water and ethanol and vacuum dried at 60 °C for 48 h to obtain an adsorption resin with a porous structure.

[0029] Embodiment 2:

[0030] (1) Under nitrogen atmosphere, 2.5 g of styrene, 0.8 g of methyl cyanoacrylate and 0.07 g of azobisisobutyronitrile were added to 12 g of ethanol, and then 0.6 g of ethylene dichloride was added. The temperature was raised to 75°C and stirred for reaction for 2.5 h. Then 0.1 g of 4,4'-divinyl-1,1'-biphenyl was added and the stirring reaction was continued for 25 h. After cooling, the mixture was washed with ethanol and then vacuum dried at 60°C for 48 h to obtain a terpolymer.

[0031] (2) At room temperature, 3 g of the terpolymer was added to 45 g of dichloroethane and swollen for 8 h, then 3 g of chloromethyl methyl ether was added and stirred for 20 min, then 4 g of anhydrous zinc chloride was added, the temperature was raised to 55 °C, stirred and reacted for 8 h, after cooling, washed with ethanol and dichloromethane, and then extracted with ethanol Soxhlet for 48 h to chlorinate the terpolymer;

[0032] (3) At room temperature, 3 g of the chlorinated terpolymer was added to 45 g of dichloroethane and swelled for 8 h, then 12 g of anhydrous ferric chloride was added, the temperature was raised to 80 °C, and the mixture was stirred for reaction for 24 h. After cooling, the mixture was washed with ethanol and dichloromethane, and then extracted with ethanol Soxhlet for 48 h, and then vacuum dried at 60 °C for 48 h to obtain a cross-linked terpolymer;

[0033] (4) At room temperature, 3 g of the cross-linked terpolymer was added to 30 g of n-butanol and allowed to swell for 5 h. Then, 1.2 g of hydroxylamine hydrochloride and 0.9 g of sodium hydroxide were added and the temperature was raised to 65 °C. The mixture was stirred and reacted for 8 h. After cooling, the mixture was washed with deionized water and sulfuric acid solution was added to neutralize the sodium hydroxide. Finally, the mixture was washed with deionized water and ethanol and vacuum dried at 60 °C for 48 h to obtain an adsorption resin with a porous structure.

[0034] Embodiment 3:

[0035] (1) Under nitrogen atmosphere, 3 g of styrene, 1 g of methyl cyanoacrylate and 0.08 g of azobisisobutyronitrile were added to 14 g of ethanol, and then 0.7 g of ethylene dichloride was added. The temperature was raised to 75°C and stirred for reaction for 3 h. Then 0.12 g of 4,4'-divinyl-1,1'-biphenyl was added and the stirring reaction was continued for 30 h. After cooling, the mixture was washed with ethanol and then vacuum dried at 60°C for 48 h to obtain a terpolymer.

[0036] (2) At room temperature, 4 g of the terpolymer was added to 60 g of dichloroethane and allowed to swell for 10 h. Then, 4.5 g of chloromethyl methyl ether was added and stirred for 20 min. Then, 5.2 g of anhydrous zinc chloride was added and the temperature was raised to 60 °C. The mixture was stirred for 8 h. After cooling, the terpolymer was washed with ethanol and dichloromethane and then extracted with ethanol Soxhlet for 48 h to chlorinate the terpolymer.

[0037] (3) At room temperature, 4 g of the chlorinated terpolymer was added to 60 g of dichloroethane and swelled for 10 h, then 15 g of anhydrous ferric chloride was added, the temperature was raised to 80 °C, and the mixture was stirred for reaction for 24 h. After cooling, the mixture was washed with ethanol and dichloromethane, and then extracted with ethanol Soxhlet for 48 h, and then vacuum dried at 60 °C for 48 h to obtain a cross-linked terpolymer;

[0038] (4) At room temperature, 4 g of the cross-linked terpolymer was added to 40 g of n-butanol and allowed to swell for 6 h. Then, 1.6 g of hydroxylamine hydrochloride and 1.2 g of sodium hydroxide were added and the temperature was raised to 65 °C. The mixture was stirred and reacted for 8 h. After cooling, the mixture was washed with deionized water and sulfuric acid solution was added to neutralize the sodium hydroxide. Finally, the mixture was washed with deionized water and ethanol and vacuum dried at 60 °C for 48 h to obtain an adsorption resin with a porous structure.

[0039] Comparative Example 1:

[0040] (1) Under nitrogen atmosphere, 2.5 g of styrene, 0.8 g of methyl cyanoacrylate and 0.07 g of azobisisobutyronitrile were added to 12 g of ethanol, and then 0.6 g of ethylene dichloride was added. The temperature was raised to 75°C and stirred for reaction for 2.5 h. Then 0.01 g of p-divinylbenzene was added and the stirring reaction was continued for 25 h. After cooling, the mixture was washed with ethanol and then vacuum dried at 60°C for 48 h to obtain a terpolymer.

[0041] (2) At room temperature, 3 g of the terpolymer was added to 45 g of dichloroethane and swollen for 8 h, then 3 g of chloromethyl methyl ether was added and stirred for 20 min, then 4 g of anhydrous zinc chloride was added, the temperature was raised to 55 °C, stirred and reacted for 8 h, after cooling, washed with ethanol and dichloromethane, and then extracted with ethanol Soxhlet for 48 h to chlorinate the terpolymer;

[0042] (3) At room temperature, 3 g of the chlorinated terpolymer was added to 45 g of dichloroethane and swelled for 8 h, then 12 g of anhydrous ferric chloride was added, the temperature was raised to 80 °C, and the mixture was stirred for reaction for 24 h. After cooling, the mixture was washed with ethanol and dichloromethane, and then extracted with ethanol Soxhlet for 48 h, and then vacuum dried at 60 °C for 48 h to obtain a cross-linked terpolymer;

[0043] (4) At room temperature, 3 g of the cross-linked terpolymer was added to 30 g of n-butanol and swelled for 5 h. Then, 1.2 g of hydroxylamine hydrochloride and 0.9 g of sodium hydroxide were added, the temperature was raised to 65 ° C, and the reaction was stirred for 8 h. After cooling, the mixture was washed with deionized water, and sulfuric acid solution was added to neutralize the sodium hydroxide. Finally, the mixture was washed with deionized water and ethanol, and vacuum dried at 60 ° C for 48 h to obtain an adsorption resin.

[0044] The difference between Comparative Example 1 and Example 2 is that the 4,4'-divinyl-1,1'-biphenyl in step (1) is replaced by p-divinylbenzene.

[0045] Comparative Example 2:

[0046] (1) Under nitrogen atmosphere, 2.5 g of styrene, 0.8 g of methyl methacrylate and 0.07 g of azobisisobutyronitrile were added to 12 g of ethanol, and then 0.6 g of ethylene dichloride was added. The temperature was raised to 75°C and stirred for reaction for 2.5 h. Then 0.1 g of 4,4'-divinyl-1,1'-biphenyl was added and the stirring reaction was continued for 25 h. After cooling, the mixture was washed with ethanol and then vacuum dried at 60°C for 48 h to obtain a terpolymer.

[0047] (2) At room temperature, 3 g of the terpolymer was added to 45 g of dichloroethane and swollen for 8 h, then 3 g of chloromethyl methyl ether was added and stirred for 20 min, then 4 g of anhydrous zinc chloride was added, the temperature was raised to 55 °C, stirred and reacted for 8 h, after cooling, washed with ethanol and dichloromethane, and then extracted with ethanol Soxhlet for 48 h to chlorinate the terpolymer;

[0048] (3) At room temperature, 3 g of the chlorinated terpolymer was added to 45 g of dichloroethane and swelled for 8 h, then 12 g of anhydrous ferric chloride was added, the temperature was raised to 80 °C, and the mixture was stirred for reaction for 24 h. After cooling, the mixture was washed with ethanol and dichloromethane, and then extracted with ethanol Soxhlet for 48 h, and then vacuum dried at 60 °C for 48 h to obtain a cross-linked terpolymer;

[0049] (4) At room temperature, 3 g of the cross-linked terpolymer was added to 30 g of n-butanol and swelled for 5 h. Then, 1.2 g of hydroxylamine hydrochloride and 0.9 g of sodium hydroxide were added, the temperature was raised to 65 °C, and the reaction was stirred for 8 h. After cooling, the mixture was washed with deionized water, and sulfuric acid solution was added to neutralize the sodium hydroxide. Finally, the mixture was washed with deionized water and ethanol, and vacuum dried at 60 °C for 48 h to obtain an adsorption resin with a porous structure.

[0050] The difference between Comparative Example 2 and Example 2 is that the methyl cyanoacrylate in step (1) is replaced by methyl methacrylate.

[0051] Comparative Example 3:

[0052] (1) Under nitrogen atmosphere, 2.5 g of styrene, 0.8 g of methyl cyanoacrylate and 0.07 g of azobisisobutyronitrile were added to 12 g of ethanol, and then 0.6 g of ethylene dichloride was added. The temperature was raised to 75°C and stirred for reaction for 2.5 h. Then 0.1 g of 4,4'-divinyl-1,1'-biphenyl was added and the stirring reaction was continued for 25 h. After cooling, the mixture was washed with ethanol and then vacuum dried at 60°C for 48 h to obtain a terpolymer.

[0053] (2) At room temperature, 3 g of the terpolymer was added to 30 g of n-butanol and swelled for 5 h. Then, 1.2 g of hydroxylamine hydrochloride and 0.9 g of sodium hydroxide were added, the temperature was raised to 65 ° C, and the reaction was stirred for 8 h. After cooling, it was washed with deionized water, and then sulfuric acid solution was added to neutralize the sodium hydroxide. Finally, it was washed with deionized water and ethanol, and vacuum dried at 60 ° C for 48 h to obtain an adsorption resin with a porous structure;

[0054] The difference between Comparative Example 3 and Example 2 is that the terpolymer is not chlorinated and cross-linked, but is directly reacted with hydroxylamine hydrochloride.

[0055] Performance Test:

[0056] Specific surface area: The specific surface area of ​​the adsorption resins prepared in the examples and comparative examples was tested by a fully automatic BET specific surface (area) analysis tester. The results are shown in Table 1.

[0057] Static adsorption test: Static adsorption was used to determine the adsorption performance of the resins prepared in the examples and comparative examples for heavy metal ions under different conditions. At room temperature, 0.1 g of the resin was placed in 50 mL of 200 mg·L -1 Heavy metal ion Cu 2+ , Pb 2+ The solution was placed in a conical flask and shaken at 150 rpm. The adsorption capacity of the resin was recorded after 8 hours. The results are shown in Table 1. The adsorption capacity of the resin was calculated according to the following formula:

[0058]

[0059] In the formula, q e is the equilibrium adsorption capacity, mg·g –1 ; C 0 and C e are the initial concentration of metal ions in the solution and the concentration when they reach equilibrium, mg·L –1 ; m is the mass of the adsorbent, g.

[0060] Static desorption test: The resin after static adsorption test was repeatedly washed with a large amount of distilled water until the distilled water became colorless, and then the washed resin was placed in 50 mL of 0.1 mol·L –1 The desorption temperature was 45 °C and the desorption time was 20 min. The above steps were repeated 10 times and the Pb content in the solution after repeated cycles was determined. 2+ ion concentration, respectively calculate the resin prepared in the embodiment and the comparative example to Pb 2+ The removal rate of Pb 2+ The ion removal rate is calculated as follows:

[0061]

[0062] In the formula, C 0 and C e are the initial concentration of the solution and the concentration of the solution at adsorption equilibrium, mg·L –1 ; R e is the cyclic removal rate of heavy metal ions in the solution, %.

[0063] Table 1 Performance test results

[0064]

[0065] Data Analysis:

[0066] It can be seen from the data of Examples 1-3 that the adsorption resin prepared by the present invention has a high specific surface area, presents a porous structure, and has a high specific surface area. 2+ , Pb 2+ The heavy metal ions have excellent adsorption performance, and after 10 cycles of adsorption-desorption, the adsorption of Pb 2+ The removal rate of heavy metal ions can still be maintained above 88%, with good repeatability, and is expected to become a new adsorption material for treating heavy metal wastewater.

[0067] It can be seen from the data of Example 2 and Comparative Example 1 that the use of 4,4'-divinyl-1,1'-biphenyl will lead to a decrease in the specific surface area of ​​the adsorption resin, but it will help to increase the adsorption capacity and repeatability of the adsorption resin for heavy metal ions. This is mainly because 4,4'-divinyl-1,1'-biphenyl has a large steric hindrance, which reduces the cross-linking density within the resin, thereby increasing the grafting rate of hydroxamic acid within the resin, thereby increasing the adsorption capacity, and 4,4'-divinyl-1,1'-biphenyl is rotatable, which may help desorb heavy metal ions, thereby improving repeatability.

[0068] It can be seen from the data of Example 2 and Comparative Example 2 that methyl cyanoacrylate is more helpful in improving the adsorption amount and repeatability of the adsorption resin for heavy metal ions than traditional methyl methacrylate. This is mainly because methyl cyanoacrylate has both an ester group and a cyano group that can react with hydroxylamine hydrochloride, thereby increasing the adsorption sites in the adsorption resin.

[0069] It can be seen from the data of Example 2 and Comparative Example 3 that chlorination and cross-linking of the terpolymer can greatly increase the specific surface area of ​​the adsorption resin, and the increase in the specific surface area has a significant promoting effect on the adsorption performance of the adsorption resin.

[0070] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A method for preparing an adsorption resin having a porous structure, characterized in that: The following steps are involved: (1) In a nitrogen atmosphere, styrene, methyl cyanoacrylate and azobisisobutyronitrile are added to ethanol, and then dichloroethane is added, and the temperature is raised to 70-75°C, and the reaction is stirred for 2-3 hours, and then 4,4'-divinyl-1,1'-biphenyl is added, and the reaction is continued by stirring for 20-30 hours. After cooling, purification is performed to obtain a terpolymer; (2) At room temperature, the terpolymer is added to dichloroethane and swelled for 5-10 hours, then chloromethyl methyl ether is added and stirred for 10-20 minutes, then anhydrous zinc chloride is added, the temperature is raised to 50-60°C, stirred and reacted for 6-8 hours, cooled, purified, and chlorinated to obtain the terpolymer; (3) adding the chlorinated terpolymer to dichloroethane at room temperature, swelling for 5-10 hours, then adding anhydrous ferric chloride, heating to 75-80°C, stirring and reacting for 20-24 hours, cooling, and purifying to obtain a cross-linked terpolymer; (4) Add the cross-linked terpolymer to n-butanol at room temperature and swell for 4-6 hours, then add hydroxylamine hydrochloride and sodium hydroxide, raise the temperature to 60-65°C, stir and react for 6-8 hours, cool, wash with deionized water, add sulfuric acid solution to neutralize the sodium hydroxide, and finally purify to obtain an adsorption resin with a porous structure; In the step (1), the weight ratio of styrene, methyl cyanoacrylate, azobisisobutyronitrile, ethanol, ethylene dichloride and 4,4'-divinyl-1,1'-biphenyl is 2-3:0.5-1:0.06-0.08:10-14:0.5-0.7:0.08-0.12; In the step (2), the weight ratio of the terpolymer, ethylene dichloride, chloromethyl methyl ether and anhydrous zinc chloride is 2-4:30-60:1.5-4.5:2.5-5.2; In the step (3), the weight ratio of the chlorinated terpolymer, ethylene dichloride and anhydrous ferric chloride is 2-4:30-60:8-15; In the step (4), the weight ratio of the cross-linked terpolymer, n-butanol, hydroxylamine hydrochloride and sodium hydroxide is 2-4:20-40:0.8-1.6:0.5-1.

2.

2. The method for preparing an adsorption resin having a porous structure according to claim 1, characterized in that: The purification step in step (1) is: washing with ethanol and then vacuum drying at 60° C. for 48 hours.

3. The method for preparing an adsorption resin having a porous structure according to claim 1, characterized in that: The purification steps in step (2) are: washing with ethanol and dichloromethane, then Soxhlet extraction with ethanol for 48 hours, and then vacuum drying at 60° C. for 48 hours.

4. The method for preparing an adsorption resin having a porous structure according to claim 1, characterized in that: The purification steps in step (3) are: washing with ethanol and dichloromethane, then Soxhlet extraction with ethanol for 48 hours, and then vacuum drying at 60° C. for 48 hours.

5. The method for preparing an adsorption resin having a porous structure according to claim 1, characterized in that: The purification step in step (4) is: washing with deionized water and ethanol, and then vacuum drying at 60° C. for 48 hours.

6. An adsorption resin having a porous structure, characterized in that: The method for preparing the adsorption resin with a porous structure according to any one of claims 1 to 5 is obtained.