A method for preparing ultraviolet-resistant and aging-resistant thermoplastic vulcanized rubber

By synthesizing bisbenzophenone containing bis-DOPO and modified nanotitanium dioxide, combined with dynamic vulcanization technology, the problem of insufficient outdoor aging and flame retardant performance of thermoplastic vulcanized rubber is solved, and its ultraviolet resistance and flame retardant performance is achieved, satisfying the The actual demand for high-performance thermoplastic vulcanized rubbers.

CN118580587BActive Publication Date: 2024-11-01ANHUI XIONGYA PLASTIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411072689.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-01
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Traditional thermoplastic vulcanized rubber is prone to aging, deteriorating its performance in outdoor environments, and has poor flame retardant performance, which cannot meet actual needs.

Method used

By synthesizing bis-DOPO-containing bisbenzophenone intermediates and bis-DOPO-containing modified nanotitanium dioxide, combined with materials such as butyl rubber, sulfur, etc., dynamic vulcanization technology is used to prepare UV-resistant and aging-resistant thermoplastic vulcanized rubber to improve its UV and flame retardant properties, improving its UV resistance and flame retardant properties .

Benefits of technology

The prepared thermoplastic vulcanized rubber has excellent UV resistance to aging and flame retardant properties, the tensile strength maintenance rate can reach 92.5%, the limit oxygen index is increased to more than 128.9%, and the vertical combustion level reaches V-0.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of vulcanized rubbers, and discloses a method for preparing an anti-ultraviolet and anti-aging thermoplastic vulcanized rubber. The present invention uses 5-aminoisophthalic acid, DOPO, formaldehyde, etc. as raw materials to prepare intermediate 2, and reacts intermediate 2 with 2,4-dihydroxybenzophenone and amination nano titanium dioxide in sequence to obtain a bis-DOPO bisbenzophenone intermediate and a bis-DOPO modified nano titanium dioxide, and the two are uniformly mixed with butadiene rubber, sulfur, stearic acid, etc. to prepare a masterbatch, and melt-plasticized ethylene-vinyl acetate copolymer and high-density polyethylene are added thereto, vulcanized, and sliced ​​to obtain an anti-ultraviolet and anti-aging thermoplastic vulcanized rubber. The thermoplastic vulcanized rubber prepared by the present invention has excellent anti-ultraviolet and anti-aging properties and flame retardant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vulcanized rubber, in particular to a method for preparing ultraviolet-resistant and aging-resistant thermoplastic vulcanized rubber. Background Art

[0002] Thermoplastic vulcanizate, referred to as TPV, is a new type of thermoplastic elastomer prepared by dynamic vulcanization technology of rubber and plastic blends. It has excellent dimensional stability, fatigue resistance and other properties, and is widely used in the fields of automobiles, electrical appliances, building materials, etc. However, in outdoor environments, ultraviolet rays in sunlight can cause the vulcanized rubber to age, discolor, and even deteriorate in performance, affecting its service life. Therefore, traditional thermoplastic vulcanizate can no longer meet the demand, and it needs to be given anti-ultraviolet properties to meet actual needs. In addition, the flame retardant properties of thermoplastic vulcanizate are poor, so it also needs to improve its flame retardant properties.

[0003] Nano titanium dioxide not only has basic effects such as quantum size effect and surface effect, but also has good weather resistance and UV resistance, and is widely used in coatings, electronic materials, etc. Benzophenone anti-ultraviolet absorbers are a widely used anti-ultraviolet property, which is widely used in various fields.

[0004] For example, the patent with authorization announcement number CN 115232414 B discloses a PVC / SBR thermoplastic vulcanized rubber composition and a preparation method thereof. The thermoplastic vulcanized rubber prepared by the invention has good flame retardant properties, tensile properties, etc., but does not improve the anti-ultraviolet properties of the thermoplastic vulcanized rubber. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies of the prior art, the present invention provides a method for preparing an ultraviolet-resistant and aging-resistant thermoplastic vulcanized rubber. The prepared thermoplastic vulcanized rubber has good ultraviolet-resistant and aging-resistant properties and flame retardant properties.

[0007] (II) Technical solution

[0008] The present invention is achieved through the following technical solutions:

[0009] A method for preparing ultraviolet-resistant and aging-resistant thermoplastic vulcanized rubber, the preparation method is as follows:

[0010] Step (1), add 5-aminoisophthalic acid, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and formaldehyde into a flask filled with N,N-dimethylformamide solvent, stir and disperse, heat to 55-70°C, react for 5-10 hours, cool to room temperature after the reaction, add methanol to precipitate at 0-5°C, filter, wash with methanol, and dry to obtain intermediate 1, whose reaction formula is: .

[0011] Step (2), add intermediate 1 and thionyl chloride into a flask, stir and disperse, heat to 80-90°C, react for 2-5h, and after the reaction, evaporate the thionyl chloride under reduced pressure and dry to obtain intermediate 2, the reaction formula of which is: .

[0012] Step (3), add 2,4-dihydroxybenzophenone and triethylamine to a flask containing N,N-dimethylformamide solvent, stir and disperse, add intermediate 2 at 0-5°C, react for 4-8h, precipitate after the reaction, wash with saturated sodium carbonate, filter, and dry to obtain a bis-DOPO bisbenzophenone intermediate, the reaction formula of which is: .

[0013] Step (4), under nitrogen conditions, add intermediate 2, amino nano-titanium dioxide, and triethylamine into a flask containing N,N-dimethylformamide solvent, stir and disperse, react at 40-55°C for 10-20h, and after the reaction is completed, distill under reduced pressure, wash with saturated brine, and dry to obtain nano-titanium dioxide modified with double DOPO, the reaction formula of which is: .

[0014] Step (5), adding butadiene rubber, bisbenzophenone intermediate containing bis-DOPO, modified nano titanium dioxide containing bis-DOPO, sulfur, accelerator CZ, accelerator TS, and stearic acid to a low-temperature double-roll rubber mixer and mixing evenly to prepare a masterbatch.

[0015] Step (6), placing ethylene-vinyl acetate copolymer and high-density polyethylene in a high-temperature double-roll open mill at 160° C., melting and plasticizing, adding the masterbatch thereto, vulcanizing at 160° C. for 10 minutes, sheeting, and then placing it in a flat vulcanizer, preheating at 180° C. for 5 minutes, exhausting 3-5 times, maintaining pressure for 10 minutes, cold pressing for 10 minutes, and sheeting to obtain UV-resistant and aging-resistant thermoplastic vulcanized rubber.

[0016] Preferably, in step (1), the molar ratio of 5-aminoisophthalic acid, DOPO and formaldehyde is 1:2-3:2-3.

[0017] Preferably, in step (3), the molar ratio of 2,4-dihydroxybenzophenone, triethylamine and intermediate 2 is 2-2.5:2-3:1.

[0018] Preferably, in step (4), the molar ratio of intermediate 2, amino-modified nano-titanium dioxide and triethylamine is 1:2-2.5:2-3.

[0019] Preferably, in step (5), the mass ratio of styrene-butadiene rubber, bisbenzophenone intermediate containing bis-DOPO, nano-titanium dioxide modified containing bis-DOPO, sulfur, accelerator CZ, accelerator TS, and stearic acid is 100:1-5:2-8:0.5-1.5:1-2:0.1-0.4:1-1.5.

[0020] Preferably, in step (6), the mass ratio of ethylene-vinyl acetate copolymer, high-density polyethylene and masterbatch is 20-35:15-25:100.

[0021] 3. Beneficial technical effects

[0022] The invention uses 5-aminoisophthalic acid, DOPO and formaldehyde as raw materials, synthesizes an intermediate 1 through a one-pot method, and then chlorinates the intermediate 1 to obtain an intermediate 2. The intermediate 2 is reacted with 2,4-dihydroxybenzophenone and amino nano-titanium dioxide in sequence to obtain a bis-DOPO-containing bis-benzophenone intermediate and a bis-DOPO-modified nano-titanium dioxide. The intermediates are uniformly mixed with butadiene rubber, sulfur, stearic acid and the like to prepare a masterbatch, and melt-plasticized ethylene-vinyl acetate copolymer and high-density polyethylene are added thereto, vulcanized, and sheeted to obtain a UV-resistant and aging-resistant thermoplastic vulcanized rubber.

[0023] The present invention prepares intermediate 2 through a series of reactions and uses it twice to react with 2,4-dihydroxybenzophenone and amino-modified nano-titanium dioxide in sequence to obtain a bisbenzophenone intermediate containing bis-DOPO and a modified nano-titanium dioxide containing bis-DOPO. The preparation method is simple and the structure is novel.

[0024] The bis-DOPO bis-benzophenone intermediate and the amino nano-titanium dioxide prepared by the present invention contain a benzophenone structure and a nano-titanium dioxide structure, both of which are good anti-ultraviolet structures and have good anti-ultraviolet effects. When added to thermoplastic vulcanized rubber, the anti-ultraviolet and anti-aging properties of the thermoplastic vulcanized rubber can be improved. In addition, nano-titanium dioxide itself is easy to agglomerate, and the present invention makes it organic, reduces the agglomeration degree of nano-titanium dioxide, increases its compatibility with thermoplastic vulcanized rubber, and then evenly distributes it in the thermoplastic vulcanized rubber to better exert its anti-ultraviolet effect.

[0025] In addition, the intermediate 2 prepared by the present invention contains a DOPO structure, which is a typical phosphorus-containing flame retardant structure with good flame retardant effect. The present invention adds it to the thermoplastic vulcanized rubber to improve the flame retardant performance of the thermoplastic vulcanized rubber. The thermoplastic vulcanized rubber prepared by the present invention has excellent UV resistance, aging resistance and flame retardant properties. DETAILED DESCRIPTION

[0026] The flame retardant thermoplastic composition, preparation method and application of the present invention are further described below in conjunction with some specific embodiments. The specific embodiments are for further illustrating the present invention in detail, but do not limit the protection scope of the present invention.

[0027] 20 g of nano titanium dioxide was added to 200 g of ethanol solvent, and ultrasonically dispersed for 1 hour. Then 1.6 g of aminopropyltriethoxysilane was added thereto, and refluxed and stirred at 80°C for 2 hours. After the reaction was completed, the mixture was filtered, washed with ethanol, and dried to obtain amino nano titanium dioxide. Embodiment 1

[0028] (1) Add 20 mmol of 5-aminoisophthalic acid, 40 mmol of DOPO and 50 mmol of formaldehyde into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, heat to 60°C, react for 8 h. After the reaction is completed, cool to room temperature, add methanol to precipitate at 0°C, filter, wash with methanol and dry to obtain intermediate 1.

[0029] (2) Add 20 mmol of intermediate 1 and 25 mL of dichlorothionyl into a flask, stir and disperse, heat to 85°C, and react for 5 h. After the reaction is completed, evaporate the dichlorothionyl under reduced pressure and dry to obtain intermediate 2.

[0030] (3) Add 45 mmol of 2,4-dihydroxybenzophenone and 50 mmol of triethylamine into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, add 20 mmol of intermediate 2 at 0°C, and react for 6 h. After the reaction is completed, precipitate, wash with saturated sodium carbonate, filter, and dry to obtain a bis-DOPO-containing bisbenzophenone intermediate.

[0031] (4) Under nitrogen conditions, 30 mmol of intermediate 2, 65 mmol of amino-modified nano-titanium dioxide, and 60 mmol of triethylamine were added to a flask containing 100 mL of N,N-dimethylformamide solvent, stirred and dispersed, and reacted at 45°C for 10 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with saturated brine, and dried to obtain nano-titanium dioxide modified with double DOPO.

[0032] (5) 100 g of butadiene rubber, 1 g of bis(2-DOPO)-containing bis(2-benzophenone) intermediate, 2 g of bis(2-DOPO)-modified nano-titanium dioxide, 1.5 g of sulfur, 2 g of accelerator CZ, 0.2 g of accelerator TS, and 1.5 g of stearic acid were added to a low-temperature double-roll rubber mixer and mixed evenly to prepare a masterbatch.

[0033] (6) 35 g of ethylene-vinyl acetate copolymer and 25 g of high-density polyethylene were placed in a high-temperature twin-roll mill at 160°C for melting and plasticization, and then 100 g of masterbatch was added thereto and vulcanized at 160°C for 10 min. The mixture was sheeted and then placed in a flat-plate vulcanizer at 180°C for preheating for 5 min, venting 4 times, maintaining pressure for 10 min, cold pressing for 10 min, and sheeting to obtain UV-resistant and aging-resistant thermoplastic vulcanized rubber. Embodiment 2

[0034] (1) Add 20 mmol of 5-aminoisophthalic acid, 60 mmol of DOPO and 60 mmol of formaldehyde into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, heat to 70°C, react for 5 h. After the reaction is completed, cool to room temperature, add methanol to precipitate at 5°C, filter, wash with methanol, and dry to obtain intermediate 1.

[0035] (2) Add 20 mmol of intermediate 1 and 25 mL of dichlorothionyl into a flask, stir and disperse, heat to 90°C, and react for 2 h. After the reaction is completed, evaporate the dichlorothionyl under reduced pressure and dry to obtain intermediate 2.

[0036] (3) Add 45 mmol of 2,4-dihydroxybenzophenone and 60 mmol of triethylamine into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, add 20 mmol of intermediate 2 at 0°C, and react for 6 h. After the reaction is completed, precipitate, wash with saturated sodium carbonate, filter, and dry to obtain a bis-DOPO-containing bisbenzophenone intermediate.

[0037] (4) Under nitrogen conditions, 30 mmol of intermediate 2, 60 mmol of amino-modified nano-titanium dioxide, and 90 mmol of triethylamine were added to a flask containing 100 mL of N,N-dimethylformamide solvent, stirred and dispersed, and reacted at 40°C for 20 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with saturated brine, and dried to obtain nano-titanium dioxide modified with double DOPO.

[0038] (5) 100 g of butadiene rubber, 2 g of bis(2-DOPO)-containing bis(2-benzophenone) intermediate, 4 g of bis(2-DOPO)-modified nano-titanium dioxide, 0.5 g of sulfur, 1 g of accelerator CZ, 0.1 g of accelerator TS, and 1 g of stearic acid were added to a low-temperature double-roll rubber mixer and mixed evenly to prepare a masterbatch.

[0039] (6) 30 g of ethylene-vinyl acetate copolymer and 18 g of high-density polyethylene were placed in a high-temperature twin-roll mill at 160°C for melting and plasticization, and then 100 g of masterbatch was added thereto and vulcanized at 160°C for 10 min. The mixture was sheeted and then placed in a flat-plate vulcanizer at 180°C for preheating for 5 min, venting 5 times, maintaining pressure for 10 min, cold pressing for 10 min, and sheeting to obtain UV-resistant and aging-resistant thermoplastic vulcanized rubber. Embodiment 3

[0040] (1) Add 20 mmol of 5-aminoisophthalic acid, 50 mmol of DOPO and 40 mmol of formaldehyde into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, heat to 55°C, react for 10 h. After the reaction is completed, cool to room temperature, add methanol to precipitate at 0°C, filter, wash with methanol, and dry to obtain intermediate 1.

[0041] (2) Add 20 mmol of intermediate 1 and 25 mL of dichlorothionyl into a flask, stir and disperse, heat to 80°C, and react for 5 h. After the reaction is completed, evaporate the dichlorothionyl under reduced pressure and dry to obtain intermediate 2.

[0042] (3) Add 40 mmol of 2,4-dihydroxybenzophenone and 50 mmol of triethylamine into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, add 20 mmol of intermediate 2 at 0°C, and react for 4 h. After the reaction is completed, precipitate, wash with saturated sodium carbonate, filter, and dry to obtain a bis-DOPO-containing bisbenzophenone intermediate.

[0043] (4) Under nitrogen conditions, 30 mmol of intermediate 2, 75 mmol of amino-modified nano-titanium dioxide, and 80 mmol of triethylamine were added to a flask containing 100 mL of N,N-dimethylformamide solvent, stirred and dispersed, and reacted at 55 °C for 12 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with saturated brine, and dried to obtain nano-titanium dioxide modified with double DOPO.

[0044] (5) 100 g of butadiene rubber, 3 g of bis(2-DOPO)-containing bis(2-benzophenone) intermediate, 5 g of bis(2-DOPO)-modified nano-titanium dioxide, 1 g of sulfur, 1.5 g of accelerator CZ, 0.4 g of accelerator TS, and 1.2 g of stearic acid were added to a low-temperature twin-roll rubber mixer and mixed evenly to prepare a masterbatch.

[0045] (6) Place 25 g of ethylene-vinyl acetate copolymer and 20 g of high-density polyethylene in a high-temperature double-roll open mill at 160°C for melting and plasticization, add 100 g of masterbatch and vulcanize at 160°C for 10 min, and then sheet it. Then place it in a flat-plate vulcanizer at 180°C, preheat for 5 min, vent 5 times, maintain pressure for 10 min, cold press for 10 min, and sheet it to obtain UV-resistant and aging-resistant thermoplastic vulcanized rubber. Embodiment 4

[0046] (1) Add 20 mmol of 5-aminoisophthalic acid, 60 mmol of DOPO and 60 mmol of formaldehyde into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, heat to 60°C, react for 8 h. After the reaction is completed, cool to room temperature, add methanol to precipitate at 0°C, filter, wash with methanol, and dry to obtain intermediate 1.

[0047] (2) Add 20 mmol of intermediate 1 and 25 mL of dichlorothionyl into a flask, stir and disperse, heat to 85°C, and react for 2 h. After the reaction is completed, evaporate the dichlorothionyl under reduced pressure and dry to obtain intermediate 2.

[0048] (3) Add 45 mmol of 2,4-dihydroxybenzophenone and 60 mmol of triethylamine into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, add 20 mmol of intermediate 2 at 0°C, and react for 6 h. After the reaction is completed, precipitate, wash with saturated sodium carbonate, filter, and dry to obtain a bis-DOPO-containing bisbenzophenone intermediate.

[0049] (4) Under nitrogen conditions, 30 mmol of intermediate 2, 70 mmol of amino-modified nano-titanium dioxide, and 80 mmol of triethylamine were added to a flask containing 100 mL of N,N-dimethylformamide solvent, stirred and dispersed, and reacted at 50°C for 15 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with saturated brine, and dried to obtain nano-titanium dioxide modified with double DOPO.

[0050] (5) 100 g of butadiene rubber, 4 g of bis(2-DOPO)-containing bis(2-benzophenone) intermediate, 6 g of bis(2-DOPO)-modified nano-titanium dioxide, 0.8 g of sulfur, 2 g of accelerator CZ, 0.1 g of accelerator TS, and 1.2 g of stearic acid were added to a low-temperature double-roll rubber mixer and mixed evenly to prepare a masterbatch.

[0051] (6) 30 g of ethylene-vinyl acetate copolymer and 22 g of high-density polyethylene were placed in a high-temperature twin-roll mill at 160°C for melting and plasticization, and then 100 g of masterbatch was added thereto and vulcanized at 160°C for 10 min. The mixture was sheeted and then placed in a flat-plate vulcanizer at 180°C for preheating for 5 min, venting 3 times, maintaining pressure for 10 min, cold pressing for 10 min, and sheeting to obtain UV-resistant and aging-resistant thermoplastic vulcanized rubber. Embodiment 5

[0052] (1) Add 20 mmol of 5-aminoisophthalic acid, 55 mmol of DOPO and 50 mmol of formaldehyde into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, heat to 60°C, react for 8 h. After the reaction is completed, cool to room temperature, add methanol to precipitate at 0°C, filter, wash with methanol and dry to obtain intermediate 1.

[0053] (2) Add 20 mmol of intermediate 1 and 25 mL of dichlorothionyl into a flask, stir and disperse, heat to 90°C, and react for 4 h. After the reaction is completed, evaporate the dichlorothionyl under reduced pressure and dry to obtain intermediate 2.

[0054] (3) Add 50 mmol of 2,4-dihydroxybenzophenone and 40 mmol of triethylamine into a flask containing 100 mL of N,N-dimethylformamide solvent, stir and disperse, add 20 mmol of intermediate 2 at 5°C, and react for 8 h. After the reaction is completed, precipitate, wash with saturated sodium carbonate, filter, and dry to obtain a bis-DOPO-containing bisbenzophenone intermediate.

[0055] (4) Under nitrogen conditions, 30 mmol of intermediate 2, 65 mmol of amino-modified nano-titanium dioxide, and 80 mmol of triethylamine were added to a flask containing 100 mL of N,N-dimethylformamide solvent, stirred and dispersed, and reacted at 50°C for 15 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with saturated brine, and dried to obtain nano-titanium dioxide modified with double DOPO.

[0056] (5) 100 g of butadiene rubber, 5 g of bis(2-DOPO)-containing bis(2-benzophenone) intermediate, 8 g of bis(2-DOPO)-modified nano-titanium dioxide, 1 g of sulfur, 1.5 g of accelerator CZ, 0.3 g of accelerator TS, and 1.2 g of stearic acid were added to a low-temperature double-roll rubber mixer and mixed evenly to prepare a masterbatch.

[0057] (6) Place 20 g of ethylene-vinyl acetate copolymer and 15 g of high-density polyethylene in a high-temperature double-roll open mill at 160°C for melting and plasticization, add 100 g of masterbatch and vulcanize at 160°C for 10 min, and then sheet it. Then place it in a flat-plate vulcanizer at 180°C, preheat for 5 min, vent 5 times, maintain pressure for 10 min, cold press for 10 min, and sheet it to obtain UV-resistant and aging-resistant thermoplastic vulcanized rubber.

[0058] Comparative Example 1

[0059] The difference between this comparative example and Example 1 is that in step (5), no bis-DOPO bis-benzophenone intermediate is contained.

[0060] Comparative Example 2

[0061] The difference between this comparative example and Example 1 is that in step (5), no double-DOPO-modified nano titanium dioxide is contained.

[0062] Referring to GB / T2406-2009, the limiting oxygen index of thermoplastic vulcanizate was tested using a limiting oxygen index analyzer, and the sample size was 120 mm × 6.5 mm × 3.2 mm.

[0063] Referring to GB / T2408-2008, the vertical burning grade of thermoplastic vulcanizate was tested using a horizontal vertical burning tester, and the sample size was 125mm×13mm×1.6mm.

[0064] Table 1: Flame retardant performance test results of various embodiments and comparative examples

[0065] Limiting oxygen index / % Vertical burning level Example 1 28.9 V-0 Example 2 30.6 V-0 Example 3 32.0 V-0 Example 4 32.8 V-0 Example 5 33.4 V-0 Comparative Example 1 26.4 V-1 Comparative Example 2 25.5 V-1

[0066] It can be seen from the table that the thermoplastic vulcanized rubber prepared by the present invention has good flame retardant properties.

[0067] With reference to GB / T16585-1996, an accelerated aging test was carried out using an ultraviolet lamp weather resistance test chamber. The irradiation wavelength was 310nm, the illumination temperature was 40°C, the condensation temperature was 45°C, the illumination cycle was 8h / 4h (illumination time / no-illumination condensation time), and the aging cycle was 0h and 48h. After the test, the specimens were taken out and the tensile strength was tested using an electronic tensile testing machine. The tensile strength maintenance rate (%) = 48h tensile strength (MPa) / 0h tensile strength (MPa), and the tensile rate was 500mm / min.

[0068] Tensile strength maintenance rate (%) Example 1 82.3 Example 2 84.0 Example 3 87.1 Example 4 90.2 Example 5 92.5 Comparative Example 1 77.0 Comparative Example 2 75.4

[0069] It can be seen from the table that the thermoplastic vulcanized rubber prepared in the present invention has good UV resistance and aging resistance, and the maximum tensile strength maintenance rate can reach 92.5%.

[0070] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a UV-resistant and aging-resistant thermoplastic vulcanized rubber, characterized in that: The preparation method is as follows: Step (1), adding 5-aminoisophthalic acid, DOPO and formaldehyde into a flask filled with N,N-dimethylformamide solvent, stirring and dispersing, heating to 55-70°C, reacting for 5-10 hours, cooling to room temperature after the reaction, adding methanol to precipitate at 0-5°C, filtering, washing with methanol, and drying to obtain intermediate 1, wherein the molar ratio of 5-aminoisophthalic acid, DOPO and formaldehyde is 1:2-3:2-3; Step (2), add intermediate 1 and thionyl chloride into a flask, stir and disperse, heat to 80-90°C, react for 2-5h, and after the reaction is completed, evaporate the thionyl chloride under reduced pressure and dry to obtain intermediate 2; Step (3), adding 2,4-dihydroxybenzophenone and triethylamine to a flask containing N,N-dimethylformamide solvent, stirring and dispersing, adding intermediate 2 thereto at 0-5° C., reacting for 4-8 hours, and after the reaction is completed, precipitating, washing with saturated sodium carbonate, filtering, and drying to obtain a bis-DOPO bisbenzophenone intermediate, wherein the molar ratio of 2,4-dihydroxybenzophenone, triethylamine, and intermediate 2 is 2-2.5:2-3:1; Step (4), under nitrogen conditions, adding intermediate 2, aminated nano titanium dioxide, and triethylamine to a flask filled with N,N-dimethylformamide solvent, stirring and dispersing, reacting at 40-55° C. for 10-20 hours, and after the reaction is completed, distilling under reduced pressure, washing with saturated brine, and drying to obtain nano titanium dioxide modified with bis-DOPO, wherein the molar ratio of intermediate 2, aminated nano titanium dioxide, and triethylamine is 1:2-2.5:2-3; Step (5), adding butadiene rubber, bis-DOPO bis-benzophenone intermediate, bis-DOPO modified nano-titanium dioxide, sulfur, accelerator CZ, accelerator TS, and stearic acid to a low-temperature double-roll rubber mixer and mixing evenly to prepare a masterbatch, wherein the mass ratio of the butadiene rubber, bis-DOPO bis-benzophenone intermediate, bis-DOPO modified nano-titanium dioxide, sulfur, accelerator CZ, accelerator TS, and stearic acid is 100:1-5:2-8:0.5-1.5:1-2:0.1-0.4:1-1.5; Step (6), placing ethylene-vinyl acetate copolymer and high-density polyethylene in a high-temperature double-roll open mill at 160° C., melting and plasticizing, adding a masterbatch thereto, vulcanizing at 160° C. for 10 minutes, sheeting, and then placing it in a flat vulcanizer, preheating at 180° C. for 5 minutes, exhausting 3-5 times, maintaining pressure for 10 minutes, cold pressing for 10 minutes, and sheeting to obtain an anti-ultraviolet and aging-resistant thermoplastic vulcanized rubber, wherein the mass ratio of the ethylene-vinyl acetate copolymer, the high-density polyethylene, and the masterbatch is 20-35:15-25:100.