A flexible coking gas carbonyl sulfide hydrolysis catalyst and preparation method thereof
By using alumina-doped mesoporous carbon molecular sieves and sol-gel method to load metal oxides, the problems of pore clogging and active component shedding of microporous carbon molecular sieve catalysts were solved, and high stability and long-term stability of carbonyl sulfide hydrolysis catalysts were achieved. Highly active.
Patent Information
- Application Number
- CN202411072827.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-06
AI Technical Summary
As a carbonyl sulfide hydrolysis catalyst carrier, microporous carbon molecular sieves have problems such as easy clogging of the pore channels and shedding of active components, resulting in short-lived and unstable catalyst reaction activity.
Alumina-doped mesoporous carbon molecular sieves are used as carriers, and metal oxides are loaded through the sol-gel method to form a carbonyl sulfide hydrolysis catalyst with high stability.
It effectively solves the problems of pore blockage and active component shedding, improves the stability and service life of the catalyst, and enables the catalyst to maintain efficient activity under high temperature and high pressure conditions.
Smart Images

Figure CN118594598B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst and a preparation method thereof, and in particular to a flexible coking gas carbonyl sulfide hydrolysis catalyst and a preparation method thereof. Background Art
[0002] Carbonyl sulfide is a harmful component in industrial gases such as coking gas, and its removal is crucial for environmental protection and subsequent processes. Among the many removal methods, the hydrolysis method has attracted much attention due to its high efficiency and environmental protection. In the process of removing carbonyl sulfide by hydrolysis, the selection and use of catalysts are key. The catalyst carrier not only needs to be able to effectively support the active components, but also needs to provide good mass transfer performance to ensure the smooth progress of the catalytic reaction.
[0003] In the selection of carriers for carbonyl sulfide hydrolysis catalysts, activated carbon is often used as a traditional carrier due to its good adsorption performance and stability. However, with the continuous improvement of catalyst performance requirements, the limitations of activated carbon are gradually emerging. For this reason, carbon molecular sieves as a new type of porous material have begun to attract attention and have been tried as carriers for carbonyl sulfide hydrolysis catalysts.
[0004] However, when the applicant used microporous carbon molecular sieve as a carbonyl sulfide hydrolysis catalyst carrier and loaded transition metal oxide as an active ingredient, it was found that the high reaction activity of the above catalyst can only be maintained for a short time (1-2 hours). Therefore, the applicant found through research that the above technical solution has the following two problems:
[0005] First, the microporous carbon molecular sieve has small pores, and the sulfur generated during the reaction easily blocks the pores, causing the reaction activity of the catalyst to drop rapidly. Secondly, the active components (such as metal oxides) loaded on the carbon molecular sieve are prone to fall off under high temperature, high pressure or long reaction conditions, which further affects the stability and performance of the catalyst. The above two factors lead to the limitations of microporous carbon molecular sieves as carbonyl sulfide hydrolysis catalysts. Therefore, how to overcome the above problems is a technical problem that needs to be solved urgently. Summary of the invention
[0006] In view of the above problems, the present invention prepares an alumina-doped mesoporous carbon molecular sieve as a catalyst carrier, and uses a sol-gel method to load metal oxides as active ingredients, thereby preparing a carbonyl sulfide hydrolysis catalyst with high stability.
[0007] Specifically, the present invention provides a method for preparing a flexible coking gas carbonyl sulfide hydrolysis catalyst, comprising the following steps:
[0008] (a) mixing a carbon precursor, an aluminum oxide precursor and a template to form a uniform mixed solution, wherein the template is a mesoporous silicon template;
[0009] (b) drying and solidifying the mixed solution;
[0010] (c) performing carbonization treatment on the solidified sample to form a carbon molecular sieve;
[0011] (d) Activating the carbonized sample to remove the template and form a mesoporous structure;
[0012] (e) loading a metal oxide on the mesoporous carbon molecular sieve by a sol-gel method, wherein the metal oxide is a transition metal oxide;
[0013] (f) The loaded sample is dried and carbonized to obtain the catalyst.
[0014] Preferably, the carbon precursor is selected from phenolic resin or sucrose, the alumina precursor is selected from alumina sol or nanoparticles, and the particle size of the alumina sol and the nanoparticles ranges from 5 to 30 nm.
[0015] Preferably, in the mixed solution in step (a), the mass ratio of the carbon precursor to the aluminum oxide precursor is 5:1 to 20:1, and the mass of the template accounts for 1% to 10% of the total mass of the mixed solution.
[0016] Preferably, the drying and curing treatment in step (b) comprises drying at room temperature for 12 to 48 hours, and then further drying at 50 to 150° C. for 2 to 8 hours.
[0017] Preferably, the carbonization treatment in step (c) comprises heating the temperature to 400 to 600°C at a heating rate of 2 to 10°C / min under nitrogen protection, keeping the temperature for 1 to 4 hours, and then heating the temperature to 600 to 900°C at a heating rate of 1 to 5°C / min, and keeping the temperature for 2 to 6 hours.
[0018] Preferably, the activation treatment in step (d) comprises soaking in a hydrofluoric acid (HF) solution or a sodium hydroxide (NaOH) solution for 2 to 12 hours, and then washing with deionized water until the washing solution is neutral.
[0019] Preferably, the sol-gel method in step (e) includes immersing the carbonized sample in a solution containing a metal salt and a sol-gelling agent for 6 to 24 hours, wherein the metal salt is a nitrate of Fe3+, Co2+, Ni2+, Cu2+, or Zn2+, and the sol-gelling agent is citric acid or ethylene glycol.
[0020] Preferably, the concentration of the metal salt solution is 0.01 to 0.5 mol / L, and the mass of the sol-gelling agent accounts for 5% to 30% of the total mass of the solution.
[0021] Preferably, the drying and carbonization treatment in step (f) comprises drying at room temperature for 6 to 24 hours, then heating to 400 to 700° C. at a heating rate of 2 to 10° C. / min under nitrogen protection, and keeping the temperature for 1 to 5 hours.
[0022] The present invention also provides a flexible coking gas carbonyl sulfide hydrolysis catalyst, which includes a carrier and an active component loaded on the carrier, wherein the active component is a transition metal oxide, and the carrier is an alumina-doped mesoporous carbon molecular sieve.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] First, by designing alumina-doped mesoporous carbon molecular sieves, the problem of easy clogging of microporous carbon molecular sieve channels in the prior art was effectively solved. The doping of alumina not only improves the binding force between the carbon molecular sieve and the active components, but also enhances the strength of the catalyst, making the catalyst more stable under high temperature, high pressure or long-term reaction conditions.
[0025] Secondly, the addition of alumina promotes the formation of mesoporous structure, which is less prone to clogging than microporous structure, thereby extending the reaction activity time of the catalyst and increasing the service life of the catalyst.
[0026] In addition, the sol-gel method is used to load the active components of metal oxides, so that chemical bonding or physical adsorption may occur between the metal oxides and the carbon molecular sieve. This interaction further enhances the loading strength, improves the stability and performance of the catalyst, and enables the catalyst to maintain efficient catalytic activity under more severe reaction conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a SEM characterization image of the catalyst prepared in Example 2 of the present application;
[0028] Figure 2 These are the activity test results of the catalyst samples prepared in the examples and comparative examples of the present application. DETAILED DESCRIPTION
[0029] Example 1: Raw material selection:
[0030] Carbon Precursor: Phenolic Resin
[0031] Alumina precursor: Alumina sol with a particle size of 10nm
[0032] Template: MCM-41 mesoporous silica template
[0033] Metal salt: ferric nitrate
[0034] Sol-gelling reagent: citric acid.
[0035] Preparation steps:
[0036] (a) Preparation of mixed solution:
[0037] - Phenolic resin, alumina sol and MCM-41 mesoporous silica template were mixed in a mass ratio of 10:2:1 and stirred to form a uniform mixed solution.
[0038] (b) Drying and curing:
[0039] - Dry the mixed solution at room temperature for 24 hours and then further dry at 80°C for 4 hours to solidify the solution.
[0040] (c) Carbonization treatment:
[0041] - Under nitrogen protection, the cured sample was heated to 500°C at a heating rate of 5°C / min and kept at this temperature for 2 hours, and then heated to 800°C at a heating rate of 3°C / min and kept at this temperature for 4 hours to form a carbon molecular sieve.
[0042] (d) Activation treatment:
[0043] - Soak the carbonized sample in hydrofluoric acid (HF) solution for 6 hours, then wash with deionized water until the washing solution is neutral, remove the MCM-41 mesoporous silicon template, and form a mesoporous structure. The specific surface area of the carbon molecular sieve is 1340m 2 / g, average pore diameter of 5.0nm, pore volume of 1.95cm 3 / g, and the compressive strength is 102N / pc.
[0044] (e) Metal oxide loading:
[0045] - Using the sol-gel method, the carbonized sample was immersed in a solution containing 0.1 mol / L ferric nitrate and 15% mass fraction of citric acid for 12 hours to load the metal oxide on the mesoporous carbon molecular sieve.
[0046] (f) Drying and carbonization:
[0047] - The loaded sample was dried at room temperature for 12 hours, and then heated to 600°C at a rate of 5°C / min under nitrogen protection and kept at this temperature for 3 hours to obtain the catalyst.
[0048] Embodiment 2: Raw material selection:
[0049] Carbon Precursor: Phenolic Resin
[0050] Alumina precursor: Alumina sol with a particle size of 10nm
[0051] Template: MCM-41 mesoporous silica template
[0052] Metal salt: copper nitrate
[0053] Sol-gelling reagent: citric acid.
[0054] Preparation steps:
[0055] (a) Preparation of mixed solution:
[0056] - Phenolic resin, alumina sol and MCM-41 mesoporous silica template were mixed in a mass ratio of 10:2:1 and stirred to form a uniform mixed solution.
[0057] (b) Drying and curing:
[0058] - Dry the mixed solution at room temperature for 24 hours and then further dry at 80°C for 4 hours to solidify the solution.
[0059] (c) Carbonization treatment:
[0060] - Under nitrogen protection, the cured sample was heated to 500°C at a heating rate of 5°C / min and kept at this temperature for 2 hours, and then heated to 800°C at a heating rate of 3°C / min and kept at this temperature for 4 hours to form a carbon molecular sieve.
[0061] (d) Activation treatment:
[0062] - The carbonized sample was immersed in hydrofluoric acid (HF) solution for 6 hours and then washed with deionized water until the washing solution was neutral to remove the MCM-41 mesoporous silica template and form a mesoporous structure.
[0063] (e) Metal oxide loading:
[0064] - Using the sol-gel method, the carbonized sample was immersed in a solution containing 0.1 mol / L copper nitrate and 15% mass fraction of citric acid for 12 hours to load the metal oxide on the mesoporous carbon molecular sieve.
[0065] (f) Drying and carbonization:
[0066] - The loaded sample was dried at room temperature for 12 hours, and then heated to 600°C at a rate of 5°C / min under nitrogen protection and kept at this temperature for 3 hours to obtain the catalyst (see SEM characterization for details). Figure 1 ).
[0067] Comparative Example 1: Raw material selection:
[0068] Carbon Precursor: Phenolic Resin
[0069] Alumina precursor: Alumina sol with a particle size of 10nm
[0070] Template: Activated carbon (as a microporous template to replace the MCM-41 mesoporous silica template)
[0071] Metal salt: copper nitrate
[0072] Sol-gelling reagent: citric acid.
[0073] Preparation steps:
[0074] (a) Preparation of mixed solution:
[0075] - Mix phenolic resin, alumina sol and activated carbon template in a mass ratio of 10:2:2 and stir to form a uniform mixed solution.
[0076] (b) Drying and curing:
[0077] - Dry the mixed solution at room temperature for 24 hours and then further dry at 80°C for 4 hours to solidify the solution.
[0078] (c) Carbonization treatment:
[0079] - Under nitrogen protection, the cured sample was heated to 500°C at a heating rate of 5°C / min, kept at this temperature for 2 hours, and then heated to 700°C at a heating rate of 3°C / min (relatively low temperature to retain the microporous structure), kept at this temperature for 4 hours to form a microporous carbon molecular sieve.
[0080] (d) Activation treatment:
[0081] - Use oxygen The carbonized sample was activated at 400°C for 2 hours to remove the activated carbon template and further enhance the microporous structure. The specific surface area of the carbon molecular sieve was tested to be 1510 m 2 / g, average pore diameter of 1.1nm, pore volume of 1.45cm 3 / g.
[0082] (e) Metal oxide loading:
[0083] - Using the sol-gel method, the activated sample was immersed in a solution containing 0.1 mol / L copper nitrate and 15% mass fraction of citric acid for 12 hours to load the metal oxide on the microporous carbon molecular sieve.
[0084] (f) Drying and carbonization:
[0085] - The loaded sample was dried at room temperature for 12 hours, and then heated to 500°C at a rate of 5°C / min under nitrogen protection and kept at this temperature for 3 hours to obtain the catalyst.
[0086] Comparative Example 2: Raw material selection:
[0087] Carbon Precursor: Phenolic Resin
[0088] Template: MCM-41 mesoporous silica template
[0089] Metal salt: copper nitrate
[0090] Sol-gelling reagent: citric acid.
[0091] Preparation steps:
[0092] (a) Preparation of mixed solution:
[0093] The phenolic resin and the MCM-41 mesoporous silica template were mixed at a mass ratio of 10:1 and stirred to form a uniform mixed solution. Note that no alumina sol was added in this step.
[0094] (b) Drying and curing:
[0095] The mixed solution was dried at room temperature for 24 h and then further dried at 80 °C for 4 h to solidify the solution.
[0096] (c) Carbonization treatment:
[0097] Under nitrogen protection, the cured sample was heated to 500°C at a heating rate of 5°C / min and kept at that temperature for 2 hours, and then heated to 800°C at a heating rate of 3°C / min and kept at that temperature for 4 hours to form a carbon molecular sieve.
[0098] (d) Activation treatment:
[0099] The carbonized sample was soaked in hydrofluoric acid (HF) solution for 6 hours, and then washed with deionized water until the washing solution was neutral to remove the MCM-41 mesoporous silicon template and form a mesoporous structure. The specific surface area of the carbon molecular sieve was 1320m 2 / g, average pore diameter of 3.9nm, pore volume of 1.67cm 3 / g.
[0100] (e) Metal oxide loading:
[0101] The carbonized sample was immersed in a solution containing 0.1 mol / L copper nitrate and 15% mass fraction of citric acid by the sol-gel method for 12 hours to load the metal oxide on the mesoporous carbon molecular sieve.
[0102] (f) Drying and carbonization:
[0103] The loaded sample was dried at room temperature for 12 hours, and then heated to 600°C at a heating rate of 5°C / min under nitrogen protection and kept at this temperature for 3 hours to obtain a catalyst.
[0104] Comparative Example 3: Raw material selection:
[0105] Carbon Precursor: Phenolic Resin
[0106] Alumina precursor: Alumina sol with a particle size of 10nm
[0107] Template: MCM-41 mesoporous silica template
[0108] Metal salt: copper nitrate .
[0109] Preparation steps:
[0110] (a) Preparation of mixed solution:
[0111] Phenolic resin, alumina sol and MCM-41 mesoporous silica template were mixed in a mass ratio of 10:2:1 and stirred to form a uniform mixed solution.
[0112] (b) Drying and curing:
[0113] The mixed solution was dried at room temperature for 24 h and then further dried at 80 °C for 4 h to solidify the solution.
[0114] (c) Carbonization treatment:
[0115] Under nitrogen protection, the cured sample was heated to 500°C at a heating rate of 5°C / min and kept at that temperature for 2 hours, and then heated to 800°C at a heating rate of 3°C / min and kept at that temperature for 4 hours to form a carbon molecular sieve.
[0116] (d) Activation treatment:
[0117] The carbonized sample was immersed in a hydrofluoric acid (HF) solution for 6 hours and then washed with deionized water until the washing solution was neutral to remove the MCM-41 mesoporous silicon template and form a mesoporous structure.
[0118] (e) Metal oxide loading:
[0119] The carbonized and activated sample was immersed in a 0.1 mol / L copper nitrate solution for 12 hours to load the metal oxide on the mesoporous carbon molecular sieve.
[0120] (f) Drying and carbonization:
[0121] The loaded sample was dried at room temperature for 12 hours, and then heated to 600°C at a heating rate of 5°C / min under nitrogen protection and kept at this temperature for 3 hours to obtain a catalyst.
[0122] Catalyst activity test: The catalyst performance was tested with a carbonyl sulfide concentration of 500×10-6 as the reaction gas, a space velocity of 1200h-1, and a reaction temperature of 80°C. The results are as follows: Figure 1 As shown. Figure 2 It can be seen that the carbonyl sulfide hydrolysis catalyst prepared in Examples 1-2 of the present application has high stability.
[0123] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a flexible coking gas carbonyl sulfide hydrolysis catalyst, comprising the following steps: (a) mixing a carbon precursor, an aluminum oxide precursor and a template to form a uniform mixed solution; the template is a mesoporous silicon template; (b) drying and solidifying the mixed solution; (c) performing carbonization treatment on the solidified sample to form a carbon molecular sieve; (d) Activating the carbonized sample to remove the template and form a mesoporous structure; (e) loading a metal oxide on the mesoporous carbon molecular sieve by a sol-gel method, wherein the metal oxide is a transition metal oxide; (f) The loaded sample is dried and carbonized to obtain the catalyst.
2. The method according to claim 1, characterized in that The carbon precursor is selected from phenolic resin or sucrose, the aluminum oxide precursor is selected from aluminum oxide sol or nanoparticles, and the particle size range of the aluminum oxide sol and the nanoparticles is 5-30nm.
3. The method according to claim 1, characterized in that In the mixed solution of step (a), the mass ratio of the carbon precursor to the aluminum oxide precursor is 5:1 to 20:1, and the mass of the template accounts for 1% to 10% of the total mass of the mixed solution.
4. The method according to claim 1, characterized in that The drying and curing treatment in step (b) comprises drying at room temperature for 12 to 48 hours and then further drying at 50 to 150° C. for 2 to 8 hours.
5. The method according to claim 1, characterized in that The carbonization treatment in step (c) includes heating to 400 to 600°C at a heating rate of 2 to 10°C / min under nitrogen protection, keeping the temperature for 1 to 4 hours, and then heating to 600 to 900°C at a heating rate of 1 to 5°C / min, and keeping the temperature for 2 to 6 hours.
6. The method according to claim 1, characterized in that The activation treatment in step (d) comprises soaking in a hydrofluoric acid solution or a sodium hydroxide solution for 2 to 12 hours, and then washing with deionized water until the washing solution is neutral.
7. The method according to claim 1, characterized in that The sol-gel method in step (e) comprises immersing the carbonized sample in a solution containing a metal salt and a sol-gelling agent for 6 to 24 hours, wherein the metal salt is Fe 3+ 、Co 2+ 、Ni 2+ , Cu 2+ 、 Zn 2+ The sol-gelling agent is citric acid or ethylene glycol.
8. The method according to claim 7, characterized in that The concentration of the metal salt solution is 0.01 to 0.5 mol / L, and the mass of the sol-gelling agent accounts for 5% to 30% of the total mass of the solution.
9. The method according to claim 1, characterized in that: The drying and carbonization treatment in step (f) comprises drying at room temperature for 6 to 24 hours, then heating to 400 to 700° C. at a heating rate of 2 to 10° C. / min under nitrogen protection, and keeping the temperature for 1 to 5 hours.
10. A flexible coking gas carbonyl sulfide hydrolysis catalyst prepared according to any one of claims 1 to 9, characterized in that The catalyst comprises a carrier and an active component loaded on the carrier, wherein the active component is a transition metal oxide, and the carrier is an aluminum oxide-doped mesoporous carbon molecular sieve.
Citation Information
Patent Citations
MOLECULAR sieve CONTAINING CARBON AND SUITABLE FOR SEPARATE GASES WITH SMALL MOLECULES FROM THE MIXTURES CONTAINING THEM
BE769800A
Resin hydrogenation catalyst and preparation method and application of resin hydrogenation catalyst
CN107866231A