Injection molding process for automatic molding of plastic parts
By combining polymer polymer with modified nanofillers in the injection molding process, and melting and cooling and solidifying under magnetic field conditions, the problem of poor thermal conductivity of injection molded plastic parts is solved, and the improvement of high thermal conductivity and mechanical properties is achieved. In a variety of electronic product shells.
Patent Information
- Application Number
- CN202411088278.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Injection-molded plastic parts have poor thermal conductivity, resulting in overheating, failure or degradation of functions of electronic devices during long-term use. The existing technology has failed to effectively solve the problem of how to obtain high thermal conductivity plastic parts.
Using an injection molding process for automatic molding of plastic parts, the thermal conductivity and mechanical properties of injection molding are adjusted by combining polymer polymers and modified nanofillers, and the thermal conductivity and mechanical properties of injection molding are suitable for mobile phone covers, TV case and other scenes.
The preparation of plastic parts with high thermal conductivity is achieved. By adjusting the raw material ratio and magnetic field conditions, the thermal conductivity, flexibility and wear resistance of plastic parts are improved, and it is suitable for a variety of electronic product shells.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of injection molding, and in particular to an injection molding process for automatic molding of plastic parts. Background Art
[0002] Injection molded plastic parts are often used in electronic product housings. Plastic parts have poor thermal conductivity, and electronic devices will overheat under long-term operating conditions, causing electronic components to fail or function to decline. Therefore, during the injection molding process of plastic parts, how to ensure that the plastic parts have good thermal conductivity and dimensional stability is a long-term technical challenge faced by the industry.
[0003] The existing technology focuses more on the heat dissipation of the mold, such as CN112757597A and CN108858962B, and pays less attention to injection molded parts. Although the academic community has a certain degree of enthusiasm for the study of thermal conductivity of polymers, there is no relevant research on how to use the injection molding process to obtain plastic parts with high thermal conductivity. Summary of the invention
[0004] In order to solve the above problems, the present invention proposes an injection molding process for automatic molding of plastic parts, which can produce high thermal conductivity and adjust the mechanical properties of injection molded parts by raw material ratio, and is suitable for various scenarios such as mobile phone cases and TV casings.
[0005] To achieve the above object, the technical solution of the present invention is:
[0006] An injection molding process for automatic molding of plastic parts comprises the following steps:
[0007] Step (1), pre-treating the raw material to obtain the pre-treated raw material: comprising the following steps:
[0008] 1-a: Weigh polymer A, modified nanofiller and common filler in a ratio of 1:0-0.1:0-0.1;
[0009] 1-b: Heat and melt the polymer A, add the modified nano filler, common filler and dispersant, stir evenly, and then cool and granulate to obtain the pretreated raw material;
[0010] Step (2), after the pre-treated raw material is melted, it is uniformly mixed with the high molecular polymer B at a mass ratio of 1:0-0.1, and then added into an injection device to obtain an injection material;
[0011] Step (3), injecting the injection material into the mold through the injection device, heating it to 220°C-250°C under 500-1000Gs magnetic field conditions, keeping it warm for 10-20s, and then cooling and shaping it under 2000-3000Gs magnetic field conditions, solidifying it, and demolding it to obtain a plastic part.
[0012] Preferably, the modified nanofiller in step (1) is modified soft magnetic nanoparticles, which are prepared by the following steps:
[0013] 1-a-1: Dispersing soft magnetic nanoparticles in an alcohol solvent at a mass ratio of 1:1-1.5 to obtain a suspension C;
[0014] 1-a-2: Add 0.03-0.1% of the mass of the soft magnetic nanoparticles to the suspension C, then ball-mill for 0.5-3h at 20-40°C, and obtain modified soft magnetic nanoparticles after separation.
[0015] Preferably, the modified soft magnetic nanoparticles in step 1-a-1 are MnZn ferrite; and the alcohol solvent is ethanol or propanol.
[0016] Preferably, the modifying reagent in step 1-a-2 is one of ethanolamine, acetic acid, acrylic acid, and carbonate.
[0017] Preferably, the particle size of the pre-processed raw material particles is 0.3-1.5 cm. The particle size of the processed raw material particles is related to the melting temperature of the subsequent processed raw material particles. This solution sets it to 0.3-1.5 cm. Too large particles may cause incomplete melting and blockage, while too small particles may increase processing costs.
[0018] Preferably, the high molecular polymer A is a thermoplastic, including one or more of PC, nylon and PET.
[0019] Preferably, the high molecular polymer B is a thermosetting plastic, one or more of epoxy resin, polyurethane, polyimide and PVDF.
[0020] When high molecular polymers are solidified in a magnetic field, they will have a certain orientation, but the orientation strength is not obvious. This scheme assists the solidification of high molecular polymers by adding modified nanofillers, thereby adjusting the thermal conductivity. This scheme preferably uses modified soft magnetic nanoparticles. The modified soft magnetic nanoparticles have strong magnetism. This scheme enables the modified soft magnetic nanoparticles to participate in the high molecular polymer solidification reaction by grafting simple functional groups on the modified soft magnetic nanoparticles. At the same time, under the action of the magnetic field, the modified soft magnetic nanoparticles rotate and drive the carbon chain, so that the main chain structure of the carbon chain is in the same direction as the magnetic field, and at the same time improves the regularity of the molecular chain arrangement, improves the crystallinity, and improves the thermal conductivity.
[0021] The polymer A in this scheme is mainly for thermoplastic injection molding, but in step (2) of this scheme, it is mentioned that a certain proportion of thermosetting plastic, that is, polymer B, can be added to achieve rigidity adjustment. Since thermosetting plastics will solidify at high temperatures (about 220°C), in order to fully fuse the two plastics, the temperature of the pretreated raw material in step (2) is controlled at 180°C-200°C, and the mixing temperature with polymer B is 180-210°C. This temperature ensures that the pretreated raw material and polymer B are both in liquid state and can be fully miscible. At the same time, the modified nanofiller and ordinary filler are uniformly added. In step (3), the temperature is raised to 220°C, and polymer B solidifies. In this process, if the thermosetting raw material polymer B is an epoxy resin, the molecular carbon main chain will turn to the direction of the magnetic field during solidification. Under the action of the modified soft magnetic nanoparticles, the arrangement orientation is more obvious. Since polymer B is uniformly dispersed, it cannot form a long-range continuous solid phase, and acts as a non-uniform nucleation carrier for the thermoplastic component during the cooling process. And because the functional groups of the modified soft magnetic nanoparticles are involved in the curing reaction of the thermoplastic raw materials, the molecular chains are pulled by the modified soft magnetic nanoparticles during the curing of thermoplastic injection molding, which can make the molecular chains more orderly and enhance the flexibility of the injection molded parts. After curing, the modified soft magnetic nanoparticles can serve as carbon chain pinning points to improve wear resistance.
[0022] Preferably, the common filler is at least three of nano-silicon dioxide, nano-carbon tubes, graphene, calcium carbonate and kaolin.
[0023] Ordinary fillers are used to change color, increase mechanical strength, wear resistance, etc., so conventional fillers are selected.
[0024] Preferably, the melting temperature of the pretreated raw material in step (2) is 180-200°C.
[0025] Preferably, the heating rate in step (3) is 3-5°C / s, and the cooling rate for cooling and setting is 3-5°C / s.
[0026] Since the modified soft magnetic nanoparticles will move in a directional manner in the magnetic field and cause segregation, the magnetic field should not be too large, especially when the thermosetting plastic is solidified and crystallized, the magnetic field only provides one orientation, so the heating rate should be fast and the insulation time should be short. Since the injection material itself has a high viscosity, the movement of the modified soft magnetic nanoparticles under the action of the magnetic field designed in this scheme encounters a large resistance, and the entire injection molding process takes only 34-120s, and the modified soft magnetic nanoparticles will not have a large segregation.
[0027] Preferably, the magnetic field in step (3) is provided by a coil. In order to make the magnitude of the magnetic field controllable, this solution chooses to use a Helmholtz coil to provide the magnetic field.
[0028] Compared with the prior art, the present invention achieves the following beneficial effects:
[0029] 1. It has high thermal conductivity and can adjust the rigidity of plastic parts by adjusting the proportion of thermosetting plastics.
[0030] 2. The grafted functional groups of the modified soft magnetic nanoparticles participate in the curing reaction of the thermoplastic raw materials, so that the molecular chains are pulled by the modified soft magnetic nanoparticles during the curing of the thermoplastic injection molding, which can make the molecular chains more orderly and enhance the flexibility of the injection molded parts. The modified soft magnetic nanoparticles can be used as carbon chain pinning points to improve wear resistance. DETAILED DESCRIPTION
[0031] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0032] Embodiment 1, an injection molding process for automatic molding of plastic parts, comprising the following steps:
[0033] Step (1), raw material pretreatment: comprising the following steps:
[0034] 1-a: Weigh polymer A, modified nanofiller and common filler in a ratio of 1:0.1:0.1;
[0035] 1-b: Heat and melt the polymer A, add the modified nanofiller, common filler and dispersant, stir evenly, and then cool and granulate to obtain a pretreated raw material with a diameter of 1 cm;
[0036] Step (2): After the pretreated raw material is melted at 180° C., it is uniformly mixed with the high molecular polymer B at a mass ratio of 1:0.1, and then added into an injection device to obtain an injection material;
[0037] Step (3): injecting the injection material into the mold through an injection device, heating it to 200°C under a 500Gs magnetic field at a heating rate of 5°C / s, keeping it warm for 10s, then cooling it under a 2000Gs magnetic field at a cooling rate of 5°C / s, solidifying it, and demolding it to obtain a plastic part;
[0038] The polymer A is nylon, and the polymer B is polyamic acid;
[0039] The modified nanofiller in step (1) is a modified soft magnetic nanoparticle, which is prepared by the following steps:
[0040] 1-a-1: Disperse the soft magnetic nanoparticles in ethanol at a mass ratio of 1:1 to obtain a suspension C;
[0041] 1-a-2: Add ethanolamine to the suspension C, the mass of ethanolamine is 0.03 of the mass of the soft magnetic nanoparticles, ball mill for 0.5h at 20℃, and obtain modified soft magnetic nanoparticles after separation.
[0042] The common filler is a combination of nano silicon dioxide, calcium carbonate and kaolin in a ratio of 1:1:1.
[0043] Embodiment 2, an injection molding process for automatic molding of plastic parts, comprising the following steps:
[0044] Step (1), raw material pretreatment: comprising the following steps:
[0045] 1-a: Weigh polymer A, modified nanofiller and common filler in a ratio of 1:0.05:0.05;
[0046] 1-b: Heat and melt the polymer A, add the modified nanofiller, common filler and dispersant, stir evenly, and then cool and granulate to obtain a pretreated raw material with a diameter of 1 cm;
[0047] Step (2), after the pretreated raw material is melted at 180° C., it is uniformly mixed with the high molecular polymer B at a mass ratio of 1:0.1, and then added into an injection device to obtain an injection material;
[0048] Step (3), injecting the injection material into the mold through the injection device, heating to 200°C under 500Gs magnetic field conditions, heating rate of 5°C / s, keeping warm for 10s, then cooling and shaping under 2000Gs magnetic field conditions, cooling rate of 5°C / s, solidifying, and demolding to obtain a plastic part;
[0049] The polymer A is nylon, and the polymer B is polyamic acid;
[0050] The modified nanofiller in step (1) is a modified soft magnetic nanoparticle, which is prepared by the following steps:
[0051] 1-a-1: Disperse the soft magnetic nanoparticles in ethanol at a mass ratio of 1:1 to obtain a suspension C;
[0052] 1-a-2: Add ethanolamine to the suspension C, the mass of ethanolamine is 0.03 of the mass of the soft magnetic nanoparticles, ball mill for 0.5h at 20℃, and obtain modified soft magnetic nanoparticles after separation.
[0053] The common filler is a combination of nano silicon dioxide, calcium carbonate and kaolin in a ratio of 1:1:1.
[0054] Embodiment 3, an injection molding process for automatic molding of plastic parts, comprising the following steps:
[0055] Step (1), raw material pretreatment: comprising the following steps:
[0056] 1-a: Weigh polymer A, modified nanofiller and common filler in a ratio of 1:0.1:0.1;
[0057] 1-b: Heat and melt the polymer A, add the modified nanofiller, common filler and dispersant, stir evenly, and then cool and granulate to obtain a pretreated raw material with a diameter of 1 cm;
[0058] Step (2), after the pretreated raw material is melted at 180° C., it is uniformly mixed with the high molecular polymer B at a mass ratio of 1:0.05, and then added into an injection device to obtain an injection material;
[0059] Step (3), injecting the injection material into the mold through the injection device, heating to 200°C under 500Gs magnetic field conditions, heating rate of 5°C / s, keeping warm for 10s, then cooling and shaping under 2000Gs magnetic field conditions, cooling rate of 5°C / s, solidifying, and demolding to obtain a plastic part;
[0060] The polymer A is nylon, and the polymer B is polyamic acid;
[0061] The modified nanofiller in step (1) is a modified soft magnetic nanoparticle, which is prepared by the following steps:
[0062] 1-a-1: Disperse the soft magnetic nanoparticles in ethanol at a mass ratio of 1:1 to obtain a suspension C;
[0063] 1-a-2: Add ethanolamine to the suspension C, the mass of ethanolamine is 0.03 of the mass of the soft magnetic nanoparticles, ball mill for 0.5h at 20℃, and obtain modified soft magnetic nanoparticles after separation.
[0064] The common filler is a combination of nano silicon dioxide, calcium carbonate and kaolin in a ratio of 1:1:1.
[0065] Embodiment 4, an injection molding process for automatic molding of plastic parts, comprising the following steps:
[0066] Step (1), raw material pretreatment: comprising the following steps:
[0067] 1-a: Weigh polymer A, modified nanofiller and common filler in a ratio of 1:0.1:0.1;
[0068] 1-b: Heat and melt the polymer A, add the modified nanofiller, common filler and dispersant, stir evenly, and then cool and granulate to obtain a pretreated raw material with a diameter of 1 cm;
[0069] Step (2), after the pretreated raw material is melted at 180° C., it is uniformly mixed with the high molecular polymer B at a mass ratio of 1:0.1, and then added into an injection device to obtain an injection material;
[0070] Step (3), injecting the injection material into the mold through the injection device, heating to 200°C under 1000Gs magnetic field conditions at a heating rate of 5°C / s, keeping warm for 10s, then cooling and shaping under 3000Gs magnetic field conditions at a cooling rate of 5°C / s, solidifying, and demolding to obtain a plastic part;
[0071] The polymer A is nylon, and the polymer B is polyamic acid;
[0072] The modified nanofiller in step (1) is a modified soft magnetic nanoparticle, which is prepared by the following steps:
[0073] 1-a-1: Disperse the soft magnetic nanoparticles in ethanol at a mass ratio of 1:1 to obtain a suspension C;
[0074] 1-a-2: Add ethanolamine to the suspension C, the mass of ethanolamine is 0.03 of the mass of the soft magnetic nanoparticles, ball mill for 0.5h at 20℃, and obtain modified soft magnetic nanoparticles after separation.
[0075] The common filler is a combination of nano silicon dioxide, calcium carbonate and kaolin in a ratio of 1:1:1.
[0076] Embodiment 5, an injection molding process for automatic molding of plastic parts, comprising the following steps:
[0077] Step (1), raw material pretreatment: comprising the following steps:
[0078] 1-a: Weigh polymer A, modified nanofiller and common filler in a ratio of 1:0.1:0.1;
[0079] 1-b: Heat and melt the polymer A, add the modified nanofiller, common filler and dispersant, stir evenly, and then cool and granulate to obtain a pretreated raw material with a diameter of 1 cm;
[0080] Step (2): After the pretreated raw material is melted at 180° C., it is uniformly mixed with the high molecular polymer B at a mass ratio of 1:0.1, and then added into an injection device to obtain an injection material;
[0081] Step (3): injecting the injection material into the mold through an injection device, heating it to 200°C under a 500Gs magnetic field at a heating rate of 3°C / s, keeping it warm for 10s, then cooling it under a 2000Gs magnetic field at a cooling rate of 3°C / s, solidifying it, and demolding it to obtain a plastic part;
[0082] The polymer A is nylon, and the polymer B is polyamic acid;
[0083] The modified nanofiller in step (1) is a modified soft magnetic nanoparticle, which is prepared by the following steps:
[0084] 1-a-1: Disperse the soft magnetic nanoparticles in ethanol at a mass ratio of 1:1 to obtain a suspension C;
[0085] 1-a-2: Add ethanolamine to the suspension C, the mass of ethanolamine is 0.03 of the mass of the soft magnetic nanoparticles, ball mill for 0.5h at 20℃, and obtain modified soft magnetic nanoparticles after separation.
[0086] The common filler is a combination of nano silicon dioxide, calcium carbonate and kaolin in a ratio of 1:1:1.
[0087] Embodiment 6, an injection molding process for automatic molding of plastic parts, comprising the following steps:
[0088] Step (1), raw material pretreatment: comprising the following steps:
[0089] 1-a: Weigh polymer A, modified nanofiller and common filler in a ratio of 1:0.1:0.1;
[0090] 1-b: Heat and melt the polymer A, add the modified nanofiller, common filler and dispersant, stir evenly, and then cool and granulate to obtain a pretreated raw material with a diameter of 1 cm;
[0091] Step (2): After the pretreated raw material is melted at 180° C., it is uniformly mixed with the high molecular polymer B at a mass ratio of 1:0.1, and then added into an injection device to obtain an injection material;
[0092] Step (3): injecting the injection material into the mold through an injection device, heating it to 200°C under a 500Gs magnetic field at a heating rate of 5°C / s, keeping it warm for 10s, then cooling it under a 2000Gs magnetic field at a cooling rate of 5°C / s, solidifying it, and demolding it to obtain a plastic part;
[0093] The polymer A is nylon, and the polymer B is polyamic acid;
[0094] The modified nanofiller in step (1) is a modified soft magnetic nanoparticle, which is prepared by the following steps:
[0095] 1-a-1: Disperse the soft magnetic nanoparticles in ethanol at a mass ratio of 1:1 to obtain a suspension C;
[0096] 1-a-2: Add ethanolamine to the suspension C, the mass of ethanolamine is 0.03 of the mass of the soft magnetic nanoparticles, ball mill for 3 hours at 20°C, and obtain modified soft magnetic nanoparticles after separation.
[0097] The common filler is a combination of nano silicon dioxide, calcium carbonate and kaolin in a ratio of 1:1:1.
[0098] Comparative Example 1 is different from Example 1 in that the plastic part is prepared by conventional nylon injection molding process.
[0099] Comparative Example 2 is different from Example 1 in that the plastic part is prepared by conventional polyamic acid injection molding process in Comparative Example 1.
[0100] Comparative Example 3 is different from Example 1 in that the soft magnetic nanoparticles are not modified.
[0101] Comparative Example 4 is different from Example 1 in that the curing is not performed under a magnetic field.
[0102] Comparative Example 5 is different from Example 1 in that the pretreated raw material is melted at 180° C. and then mixed with high molecular polymer B (polyamic acid) at a mass ratio of 1:0.2.
[0103] Comparative Example 6 is different from Example 1 in that, in step (3), the injection material is injected into the mold through the injection device, heated to 200°C under 2000Gs magnetic field conditions at a heating rate of 5°C / s, and kept warm for 10s, then cooled and shaped under 4000Gs magnetic field conditions at a cooling rate of 5°C / s, solidified, and demolded to obtain a plastic part.
[0104] Detection parameters:
[0105] Thermal conductivity: tested according to ISO 22007-2:2015 method;
[0106] Wear resistance coefficient: tested according to ASTM D4060 method;
[0107] Flexural modulus: tested according to GB / T 9341-2008 method;
[0108] Tensile strength: tested according to ASTM D256-10 method.
[0109] The test results are shown in Table 1.
[0110] Table 1
[0111]
[0112] As can be seen from the data in Table 1, by comparing the data of different embodiments and comparative examples, it can be clearly seen that the use of a specific ratio of modified nanofillers, high molecular polymers and injection molding process under magnetic field curing conditions can significantly improve the performance of plastic parts. In particular, the thermal conductivity, wear resistance, bending modulus and tensile strength of Examples 1 to 6 are significantly better than those of the comparative examples. This proves the importance of the selection of modified nanofillers, high molecular polymers and magnetic field curing conditions in the injection molding process of this solution.
[0113] Comparative Examples 1 and 2 are injection molded parts obtained by conventional technical means, and their thermal conductivity is two orders of magnitude lower than that of this embodiment. In Comparative Example 3, the soft magnetic nanoparticles were not modified, and its performance was significantly worse, which illustrates the key role of modified nanofillers in improving the performance of plastic parts. Through modification, the nanofiller can be made more compatible with the polymer, so as to give full play to its reinforcing effect. In Example 4, the performance is obviously poor because it is not cured under the magnetic field. This further proves the importance of magnetic field curing conditions in improving the performance of plastic parts. Under the action of the magnetic field, the polymer chains will be arranged in an orderly manner to form a more compact structure, thereby improving the performance of the plastic parts. In Example 5, the excessive amount of thermosetting plastic will nucleate in large quantities during the heating process of step (3). Excessive nucleation will hinder the curing reaction of the thermoplastic plastic, resulting in a decrease in performance, especially a decrease in tensile strength. Cracks may be generated from the junction between the two polymers. In Example 6, the excessive magnetic field causes the modified soft magnetic particles to move faster, resulting in one-sided segregation, affecting the uniformity of the overall structure, and further affecting the thermal conductivity and tensile strength.
[0114] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An injection molding process for automatic molding of plastic parts, characterized in that: The following steps are involved: Step (1), pre-treating the raw material to obtain the pre-treated raw material, comprises the following steps: 1-a: Weigh polymer A, modified nanofiller and common filler in a ratio of 1:0-0.1:0-0.1; 1-b: Heat and melt the polymer A, add the modified nano filler, common filler and dispersant, stir evenly, and then cool and granulate to obtain the pretreated raw material; Step (2), after the pre-treated raw material is melted, it is uniformly mixed with the high molecular polymer B at a mass ratio of 1:0-0.1, and then added into an injection device to obtain an injection material; Step (3), injecting the injection material into the mold through the injection device, heating it to 220°C-250°C under the condition of 500-1000Gs magnetic field, keeping it warm for 10-20s, then cooling and shaping it under the condition of 2000-3000Gs magnetic field, solidifying it, and demolding it to obtain a plastic part; The modified nanofiller in step (1) is a modified soft magnetic nanoparticle, which is prepared by the following steps: 1-a-1: Dispersing soft magnetic nanoparticles in an alcohol solvent at a mass ratio of 1:1-1.5 to obtain a suspension C; the soft magnetic nanoparticles are MnZn ferrite; the alcohol solvent is ethanol or propanol; 1-a-2: Add 0.03-0.1 of the mass of the soft magnetic nanoparticles to the suspension C, then ball-mill for 0.5-3h at 20-40°C, and obtain modified soft magnetic nanoparticles after separation; the modifying agent is one of ethanolamine, acetic acid, acrylic acid or carbonate; The melting temperature of the pretreated raw material in step (2) is 180-200°C; The heating rate in step (3) is 3-5°C / s, and the cooling rate for cooling and setting is 3-5°C / s.
2. The injection molding process for automatic molding of plastic parts as claimed in claim 1, characterized in that: The particle size of the pretreated raw material particles in step (1) is 0.3-1.5 cm.
3. The injection molding process for automatic molding of plastic parts as claimed in claim 1, characterized in that: The high molecular polymer A is one or more of PC, nylon, and PET; the high molecular polymer B is one or more of epoxy resin, polyurethane, polyimide, and PVDF.
4. The injection molding process for automatic molding of plastic parts as claimed in claim 1, characterized in that: The common filler in step (1) is at least three of nano-silicon dioxide, nano-carbon tubes, graphene, calcium carbonate and kaolin.
5. The injection molding process for automatic molding of plastic parts as claimed in claim 1, characterized in that: The magnetic field in step (3) is provided by a coil.