Construction method of pollution resistance strength model of coral concrete doped with nano-TiO2
By using the synergistic effect of nano-TiO2, fly ash and slag in coral concrete, a pollution resistance strength model was established, which solved the problem of insufficient prediction of the mechanical properties and durability of coral concrete in the existing technology, and achieved high-accuracy mechanics. Performance and durability improvements.
Patent Information
- Application Number
- CN202411087867.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing pollution resistance strength model is mainly based on traditional gravel concrete and cannot be effectively applied to coral concrete, resulting in insufficient accuracy in predicting the mechanical properties and durability of coral concrete in marine engineering, especially in the environment where sewage and wastewater corrode the performance.
A model of corrosion resistance strength of coral concrete doped with nano-TiO2 was designed. By preparing specimens, conducting sewage erosion tests and establishing statistical mathematical models, including the evolution model of coral concrete cube compressive strength and prism flexural strength, nanometer The synergistic effect of TiO2, fly ash and slag improves concrete compactness and performance.
It achieves the accuracy of predicting the mechanical properties and durability of coral concrete in sewage and wastewater environments, improves the compressive strength and flexural strength of coral concrete, extends the service life of the structure, and obtains the results through nonlinear fitting technology. Highly accurate and applicable models.
Smart Images

Figure CN118609735B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of concrete, and in particular to a method for constructing a pollution resistance strength model of coral concrete doped with nano-TiO2. Background Art
[0002] In the construction of marine engineering, crushed stone aggregate and fresh water are often difficult to obtain, so coral concrete, which is made from local materials, is widely used. Coral aggregate has low strength and high porosity, so the strength and durability of coral concrete are lower than those of traditional concrete. Especially in some sewage treatment facilities, due to the erosion of sewage and wastewater, the service performance of coral concrete decreases significantly as the service cycle increases, seriously affecting the service life of the structure.
[0003] At present, in order to improve the physical properties of coral concrete, nano-TiO2 is usually added to coral concrete. The current stain resistance strength model is basically established on the basis of traditional crushed stone concrete, which is not suitable for coral concrete. It has the defects of poor applicability to coral concrete and insufficient prediction accuracy. Summary of the invention
[0004] In order to overcome the above problems, the purpose of the present invention is to provide a method for constructing a pollution resistance strength model of coral concrete doped with nano-TiO2, which can accurately predict the mechanical properties and durability of coral concrete components in marine engineering.
[0005] To achieve the above object, the method for constructing the stain resistance strength model of coral concrete designed by the present invention is characterized by comprising the steps of:
[0006] Step 1: Prepare coral concrete specimens:
[0007] First, weigh the raw materials according to weight: 750-780 parts of cement, 135-150 parts of slag, 55-70 parts of fly ash, 0-60 parts of nano-TiO2, 300 parts of coral aggregate, 700 parts of coral sand, 250 parts of seawater, and 20 parts of water reducer; then mix the raw materials evenly to obtain concrete slurry; finally, introduce the concrete slurry into a mold, and obtain a coral concrete specimen after demoulding and curing;
[0008] Step 2, conducting sewage erosion tests on each coral concrete specimen to test the compressive strength of the coral concrete cube and the flexural strength of the prism;
[0009] Extracted data set A in the sewage erosion resistance test: the composition ratio of coral concrete specimens, nano-TiO2 dosage, corrosion time and concrete cube compressive strength data; extracted data set B: the composition ratio of coral concrete specimens, nano-TiO2 dosage, corrosion time and prism flexural strength;
[0010] Step 3: Based on the statistical mathematical model shown in formula (1) and data set A, a coral concrete cube compressive strength evolution model shown in formula (2) is obtained; based on the statistical mathematical model shown in formula (1) and data set B, a coral concrete prism flexural compressive strength evolution model shown in formula (3) is obtained;
[0011]
[0012] Among them, f is the cube compressive strength or prism flexural strength of coral concrete, MPa; w is the mass percentage of nano-TiO2; d is the service time in sewage environment, d; a, b, c are sewage medium corrosion parameters; e, g, h, i, j are material physical and mechanical property parameters;
[0013]
[0014] In formula (2), f cp is the cubic compressive strength of high-performance coral concrete, MPa; w is the mass percentage of nano-TiO2; d is the service time in sewage and wastewater environment, d;
[0015]
[0016] In formula (3), f f is the prism flexural strength of high-performance coral concrete, MPa, w is the mass percentage of nano-TiO2; d is the service time in sewage and wastewater environment, d.
[0017] As a preferred embodiment, the particle size of the nano-TiO2 is 10 to 20 nm. There is a significant synergistic effect between nano-TiO2, fly ash and slag. The addition of nano-TiO2 accelerates the hydration reaction of cement, so that cement hydration products are generated earlier and react with the active ingredients in fly ash and slag to generate more beneficial products such as CSH gel and calcium aluminate. Slag and fly ash can fill part of the voids in the cement matrix, and smaller-sized nano-TiO2 can fill smaller voids to make the matrix more compact. The synergistic effect of nano-TiO2, fly ash and slag can significantly improve the performance of concrete.
[0018] As a preferred solution, the coral sand has a fineness modulus of 2.87 and a zone II grading, and is medium sand.
[0019] As a preferred solution, the coral aggregate is a coarse aggregate with a continuous grade of 5 to 8 mm.
[0020] As a preferred solution, the cement is silicate cement, the slag is S95 grade slag, and the fly ash is grade I fly ash.
[0021] As a preferred embodiment, each raw material mixing method is: firstly, nano-TiO2, water reducing agent and seawater are stirred and mixed to obtain a mixed suspension, the mixed suspension is divided into two mixed suspensions of the same volume, half of the mixed suspension is stirred and mixed with coral aggregate and coral sand, cement, slag, fly ash and the remaining other half of the mixed suspension are added successively, and the coral concrete slurry is obtained by continuing to stir and mix. Since nano-TiO2 has a smaller density, it is easily driven and scattered by airflow, so when dispersing nano-TiO2, it is necessary to carry out in a windless room. Meanwhile, due to its extremely fine particle size, different concrete mixers and even mortar mixer dry mixing cannot be evenly dispersed, and observations show that dry mixing can cause nano-TiO2 to "stick to the wall", causing the nano-TiO2 dosage in the final cement-based material to reduce, and it is impossible to ensure that nano-TiO2 fully plays a role. Therefore, the dispersion method of nano-TiO2 in the present invention is to first weigh the water and water reducer required by the group ratio, stir the two for 1 minute, and then add the nano-TiO2 into the mixed solution of water and high-efficiency water reducer while stirring in a windless room. After all the nano-TiO2 is dissolved, stir for another 3 minutes to make a mixed suspension.
[0022] As a preferred embodiment, in step 2, the wastewater in the sewage erosion test is obtained by fermenting sewage sludge and organic solution in an erosion barrel.
[0023] As a preferred embodiment, in step 2, the test of the compressive strength of the coral concrete cube is specifically to conduct a cube compressive test on the coral concrete using a 100t electro-hydraulic servo universal testing machine with a loading rate of 500N / s; the test of the flexural strength of the coral concrete prism is specifically to conduct a four-point bending test on the coral concrete using a 10t electronic universal material testing machine with a loading rate of 80N / s.
[0024] A method for constructing a pollution resistance strength model of coral concrete, characterized in that the pollution resistance strength model of coral concrete is applied to the prediction of mechanical properties and durability performance of sewage and wastewater discharge structural components in marine engineering.
[0025] As a preferred solution, the mass percentage of nano-TiO2 in the stain resistance strength model of coral concrete is set to 3% to 4%.
[0026] The advantages of the present invention are: the construction method of the stain resistance strength model of coral concrete of the present invention uses nonlinear fitting technology to obtain two models that jointly characterize the stain resistance strength of coral concrete: a coral concrete cube compressive strength evolution model and a coral concrete prism flexural compressive strength evolution model; the two models have the characteristics of high accuracy and strong applicability. In addition, the stain resistance strength model of coral concrete of the present invention can be used to design the content ratio of nano-TiO2 in coral concrete according to different target stain resistance performances to obtain the best service performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The compressive strength curve of coral concrete with corrosion time when the nano-TiO2 content is 0%, 2%, 4% and 6% respectively;
[0028] Figure 2 This is a curve of the flexural strength of coral concrete changing with corrosion time when the nano-TiO2 dosage is 0%, 2%, 4% and 6%. DETAILED DESCRIPTION
[0029] In order to better understand the present invention, the present invention will be described in detail below with reference to the accompanying drawings and specific examples.
[0030] A method for constructing a pollution resistance strength model of coral concrete doped with nano-TiO2 comprises the following steps:
[0031] Step 1: Prepare coral concrete specimens:
[0032] (1.1) As shown in Table 1, by weight, cement is 750-780 parts, slag is 135-150 parts, fly ash is 55-70 parts, nano-TiO2 is 0-60 parts, coral aggregate is 300 parts, coral sand is 700 parts, seawater is 250 parts, and water reducer is 20 parts; the particle size of nano-TiO2 is 15nm, the fineness modulus of coral sand is 2.87, the gradation of zone II is medium sand, the coral aggregate is a coarse aggregate with continuous grading of 5-8mm, the cement is silicate cement, the slag is S95 grade slag, and the fly ash is grade I fly ash.
[0033] (1.2) Mixing nano-TiO2, a water reducing agent and seawater to obtain a mixed suspension, dividing the mixed suspension into two mixed suspensions of equal volume, taking half of the mixed suspension and mixing them evenly with coral aggregate and coral sand, and then adding cement, slag, fly ash and the remaining half of the mixed suspension in sequence, and continuing to stir and mix evenly to obtain coral concrete slurry;
[0034] (1.3) The coral concrete slurry was introduced into the mold coated with the release agent, and vibrated and compacted on a vibrator. After 24 hours, the slurry was demoulded and placed in a standard curing room for 28 days. The curing conditions were an ambient temperature of 20±2℃ and a relative humidity of more than 95%, and the coral concrete specimens were obtained.
[0035] Table 1 Composition ratio of some specimens
[0036]
[0037] Step 2, conducting sewage erosion tests on each coral concrete specimen to test the compressive strength of the coral concrete cube and the flexural strength of the prism;
[0038] Each concrete specimen was subjected to sewage erosion test. The sewage was obtained by fermenting sewage sludge and organic matter solution in an erosion barrel. The test sewage environment simulated the sewage discharged from the ocean. The concrete cube compressive strength and prism flexural strength were tested according to the "Standard for Test Methods of Physical and Mechanical Properties of Ordinary Concrete" (GB / T50081-2019); the experimental data set A of the composition ratio, nano-TiO2 dosage and corrosion time of coral concrete specimens and the experimental data set B of the composition ratio, nano-TiO2, corrosion time and prism flexural strength of coral concrete specimens were extracted, and the data of some data sets A and B shown in Tables 2 and 3 were combined.
[0039] Table 2 Compressive strength of some coral concrete specimens Dataset A
[0040]
[0041] Table 3 Flexural strength of some coral concrete specimens Data set B
[0042]
[0043] Combining Table 1, Table 2 and Table 3, it can be seen that the 28d cubic compressive strength of specimens 1 to 7 is 70.96-83.83Mpa, which is 1.5%-19.9% higher than the 28d cubic compressive strength of specimen 8; the 28d flexural strength of specimens 1 to 7 is 8.66MPa-10.55Mpa, which is 2.1%-24.4% higher than the 28d cubic compressive strength of specimen 8; after 90 days of sewage erosion, the cubic compressive strength of specimens 1 to 7 lost 2.14-3.81MPa , compared with specimen 8, it was reduced by 3.3%-45.7%, the prism flexural strength of specimens 1 to 7 lost 0.4-0.64MPa, compared with specimen 8, it was reduced by 5.9%-41.2%, after 180 days of sewage erosion, the cube compressive strength of specimens 1 to 7 lost 5.03-7.27MPa, compared with specimen 8, it was reduced by 13.3%-40%, and the prism flexural strength of specimens 1 to 7 lost 0.95-1.39MPa, compared with specimen 8, it was reduced by 4.1%-34.5%. It shows that the coral concrete doped with nano-TiO2 prepared by the present invention has higher strength and better durability.
[0044] Step 3: Use statistical laws to reflect the nonlinear and time-varying random distribution of coral concrete and establish a statistical mathematical model as shown in formula (1):
[0045]
[0046] Wherein, f is the cube compressive strength or prism flexural strength of coral concrete, MPa; w is the mass percentage of nano-TiO2; d is the service time in sewage environment, d; a, b, c are sewage medium corrosion parameters; e, g, h, i, j are material physical and mechanical property parameters,
[0047] Substitute the experimental data set A into the statistical strength mathematical model to solve the sewage medium corrosion parameters and material physical and mechanical property parameters, and then obtain the coral concrete cube compressive strength model under sewage as shown in formula (2):
[0048]
[0049] In formula (2), f cp is the cube compressive strength of high performance coral concrete, MPa; w is the mass fraction of nano-TiO2; d is the service time in sewage environment, d.
[0050] Substituting the experimental data set B into the statistical strength mathematical model to solve the sewage medium corrosion parameters and material physical and mechanical property parameters, the flexural and compressive strength model of coral concrete prisms under sewage is obtained as shown in formula (3):
[0051]
[0052] In formula (3), f f is the prism flexural strength of high-performance coral concrete, MPa, w is the mass fraction of nano-TiO2; d is the service time in sewage and wastewater environment, d.
[0053] Combination Figure 1 and Figure 2 As shown in the figure, using the coral concrete cube compressive strength evolution model and prism flexural compressive strength evolution model, the compressive strength and flexural compressive strength curves of coral concrete with corrosion time are predicted when the nano-TiO2 content is 0%, 2%, 4% and 6%. Figure 1 and Figure 2 It can be seen that the average deviation of the coral concrete cube compressive strength model and the prism flexural compressive strength model is about 2.89%, and the error value is within an acceptable range, indicating that the coral concrete cube compressive strength evolution model and the prism flexural compressive strength evolution model of the present invention are highly accurate and can well predict the coral concrete cube compressive strength and flexural compressive strength.
[0054] Moreover, using the coral concrete cube compressive strength evolution model and the prism flexural compressive strength evolution model, it is found that the mechanical properties (including compressive strength and flexural strength) of high-performance coral concrete will show an upward and then downward trend with the increase of nano-TiO2 content. When the mass fraction of nano-TiO2 is less than 4%, the mechanical properties (including compressive strength and flexural strength) of high-performance coral concrete are enhanced with the increase of nano-TiO2 content. Under this condition, nano-TiO2 gives full play to its size benefit and nucleation effect, which has significant benefits for the mechanical properties (including compressive strength and flexural strength) of high-performance coral concrete. When the mass fraction of nano-TiO2 is greater than 4%, the mechanical properties (including compressive strength and flexural strength) of high-performance coral concrete are weakened with the increase of nano-TiO2 content. Under this condition, excessive nano-TiO2 agglomerates in the cement matrix and cannot play a good role, and the strengthening effect on the mechanical properties (including compressive strength and flexural strength) of high-performance coral concrete is weakened. When using this model to design the mix ratio of high-performance coral concrete, the mass fraction of nano-TiO2 should be controlled below 4% to obtain the best service performance, and then the mix ratio design should be carried out according to the target pollution resistance performance.
[0055] Step 4: Apply the coral concrete cube compressive strength evolution model and the coral concrete prism flexural compressive strength evolution model to marine sewage discharge concrete facilities, design mix proportions of coral concrete with different target pollution resistance, and predict the changes in its mechanical properties with the increase of service time. No additional testing is required, which is convenient for engineers to estimate the service life and maintenance cycle of the structure and reduce the operating costs of the enterprise.
[0056] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for constructing a pollution resistance strength model of coral concrete doped with nano-TiO2, characterized in that: Includes steps: Step 1: Prepare coral concrete specimens: First, weigh the raw materials according to weight: 750-780 parts of cement, 135-150 parts of slag, 55-70 parts of fly ash, 0-60 parts of nano-TiO2, 300 parts of coral aggregate, 700 parts of coral sand, 250 parts of seawater, and 20 parts of water reducer; then mix the raw materials evenly to obtain concrete slurry; finally, introduce the concrete slurry into a mold, and obtain a coral concrete specimen after demoulding and curing; Step 2, conducting sewage erosion resistance tests on each coral concrete specimen, and testing the compressive strength of the coral concrete cube and the flexural strength of the prism; Extracted data set A in the sewage erosion resistance test: the composition ratio of coral concrete specimens, nano-TiO2 dosage, corrosion time and concrete cube compressive strength data; extracted data set B: the composition ratio of coral concrete specimens, nano-TiO2 dosage, corrosion time and prism flexural strength; Step 3: Based on the statistical mathematical model shown in formula (1) and data set A, a coral concrete cube compressive strength evolution model shown in formula (2) is obtained; based on the statistical mathematical model shown in formula (1) and data set B, a coral concrete prism flexural compressive strength evolution model shown in formula (3) is obtained; Wherein, f is the cube compressive strength or prism flexural strength of coral concrete, MPa; w is the mass percentage of nano-TiO2; d is the service time in sewage environment; a, b, c are sewage medium corrosion parameters; e, g, h, i, j are material physical and mechanical property parameters; In formula (2), f cp is the cubic compressive strength of high-performance coral concrete, MPa; w is the mass percentage of nano-TiO2; d is the service time in sewage and wastewater environment; In formula (3), f f is the prism flexural strength of high-performance coral concrete, MPa, w is the mass percentage of nano-TiO2; d is the service time in sewage and wastewater environment.
2. The method for constructing the pollution resistance strength model of coral concrete doped with nano-TiO2 according to claim 1 is characterized in that: The particle size of the nano-TiO2 is 10-20 nm.
3. The method for constructing the pollution resistance strength model of coral concrete doped with nano-TiO2 according to claim 1 is characterized in that: The coral sand has a fineness modulus of 2.87 and a zone II grading, and is medium sand.
4. The method for constructing the pollution resistance strength model of coral concrete doped with nano-TiO2 according to claim 1 is characterized in that: The coral aggregate is a coarse aggregate with a continuous grade of 5 to 8 mm.
5. The method for constructing the pollution resistance strength model of coral concrete doped with nano-TiO2 according to claim 1 is characterized in that: The cement is silicate cement, the slag is S95 grade slag, and the fly ash is grade I fly ash.
6. The method for constructing the pollution resistance strength model of coral concrete doped with nano-TiO2 according to claim 1 is characterized in that: The mixing method of the raw materials is as follows: first, nano-TiO2, water reducing agent and seawater are stirred and mixed to obtain a mixed suspension, the mixed suspension is divided into two mixed suspensions of equal volume, half of the mixed suspension is taken and stirred and mixed with coral aggregate and coral sand, and then cement, slag, fly ash and the remaining half of the mixed suspension are added in sequence, and the stirring and mixing is continued to obtain coral concrete slurry.
7. The method for constructing the pollution resistance strength model of coral concrete doped with nano-TiO2 according to claim 1 is characterized in that: In step 2, the wastewater in the sewage erosion resistance test is obtained by fermenting sewage sludge and organic matter solution in an erosion barrel.
8. The method for constructing the pollution resistance strength model of coral concrete doped with nano-TiO2 according to claim 1 is characterized in that: In the step 2, the test of the compressive strength of the coral concrete cube is specifically to carry out a cube compressive test on the coral concrete using a 100t electro-hydraulic servo universal testing machine with a loading rate of 500N / s; the test of the flexural strength of the coral concrete prism is specifically to carry out a four-point bending test on the coral concrete using a 10t electronic universal material testing machine with a loading rate of 80N / s.
9. The method for constructing the pollution resistance strength model of coral concrete doped with nano-TiO2 according to claim 1 is characterized in that: The anti-fouling strength model of coral concrete is applied to the prediction of mechanical properties and durability of sewage and wastewater discharge structural components in marine engineering.
10. The method for constructing the pollution resistance strength model of coral concrete doped with nano-TiO2 according to claim 1 is characterized in that: The mass percentage of nano-TiO2 in the stain resistance strength model of coral concrete is set to 3% to 4%.
Citation Information
Patent Citations
Preparation method for high-strength coral concrete
CN110372298A
Basalt-polyethylene fiber concrete dynamic damage constitutive model establishing method
CN116705208A