A pretreatment agent for silicon-containing VOCs and its preparation method and application

By using a pretreatment agent with a low silicon-aluminum ratio molecular sieve-supported transition metal in VOCs catalysts, the inactivation problem of precious metal catalysts caused by organic silicon is solved, extending the service life of the catalyst and reducing production costs.

CN118616110BActive Publication Date: 2024-11-15JIANGSU ZHONGCHUANG QINGYUAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410916351.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-15
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

When existing VOCs catalysts contain silicone, they are prone to generate silicon dioxide crystals to cover the catalytic surface, resulting in deactivation of precious metal catalysts, and the extrusion production process is high and the active ingredients cannot fully play a role, which affects the service life of the catalyst.

Method used

Using low silicon-aluminum-specific molecular sieve loaded transition metal, silicon-containing VOCs pretreatment agent is prepared by vacuum coating, so that the silicon element can form silicon dioxide crystals at the aluminum site in the pretreatment agent, reduce contact with noble metal catalysts, and prolong the catalyst. service life.

Benefits of technology

It reduces the deactivation rate of precious metal catalysts, extends its service life, reduces production costs, and improves catalytic activity, effectively captures and fixes silicon elements in exhaust gas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118616110B_ABST
    Figure CN118616110B_ABST
Patent Text Reader

Abstract

The present invention discloses a pretreatment agent for silicon-containing VOCs and a preparation method and application thereof, and belongs to the technical field of VOCs catalysts. The present invention adopts a silicon source and an aluminum source to prepare a low silicon-aluminum ratio molecular sieve with a silicon-aluminum ratio of 0.8-2; a transition metal precursor, a binder and the low silicon-aluminum ratio molecular sieve are mixed in water to obtain a mixed slurry; the mixed solution is coated on a carrier by a vacuum coating method, dried, and calcined to obtain a pretreatment agent for silicon-containing VOCs. The present invention adopts a transition metal-loaded low silicon-aluminum ratio molecular sieve, and the transition metal is evenly distributed on its surface, thereby avoiding the problem of transition metal being embedded. The low silicon-aluminum ratio molecular sieve catalyst has a large specific surface area, a high aluminum content, a uniform distribution of transition metals, and a high catalytic activity. It can effectively capture elemental silicon in the exhaust gas directly, and the remaining undecomposed small molecular silicon is catalytically decomposed, thereby achieving efficient capture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of VOCs catalysts, and in particular relates to a pretreatment agent for silicon-containing VOCs, and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Volatile organic compounds (VOCs) are one of the main air pollutants, which can directly cause photochemical smog and aggravate haze pollution, endangering human health. In practical applications, VOCs catalysts are mainly precious metal catalysts. Then when organic silicon is contained in the actual working conditions, silica crystals are often generated to cover the catalytic surface, block the pores, cover the silicon metal active sites, and accelerate the deactivation of the precious metal catalyst. In response to this phenomenon, there are a few coping methods, for example: Patent CN114100669 A discloses an extruded 400-mesh honeycomb silicon-containing VOCs pretreatment catalyst, including an aluminum-based carrier, an active component and other additives. Patent CN 115069277 A discloses an extruded spherical granular or spherical mesoporous through-granular VOCs pretreatment catalyst, including an aluminum-based carrier and an active component. Both of the above catalysts can protect the rear-end precious metal catalyst, but their extrusion production process and high mesh count characteristics greatly increase the production cost. In addition, due to the extrusion production, some active ingredients are coated in the aluminum-based carrier and cannot play a catalytic role, resulting in a large amount of active ingredients and high production costs. If the amount of active ingredients is reduced, its performance will be affected, the service life of the precious metal catalyst will be affected, and the effect of protecting the back-end precious metal catalyst will not be achieved.

[0004] Therefore, there is an urgent need to develop a pretreatment catalyst that can efficiently capture silicone while reducing the amount of active ingredients. Summary of the invention

[0005] In order to address the deficiencies of the prior art, the purpose of the present invention is to provide a silicon-containing VOCs pretreatment agent and a preparation method and application thereof. The silicon-containing VOCs pretreatment agent provided by the present invention can capture the silicon element in VOCs on the aluminum site in the pretreatment agent to generate silicon dioxide crystals, so that the silicon element remains on the pretreatment agent, thereby reducing its contact with the precious metal catalyst and extending the service life of the precious metal catalyst.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] The first aspect of the present invention provides a method for preparing a silicon-containing VOCs pretreatment agent, comprising the following steps:

[0008] A low silicon-aluminum ratio molecular sieve with a silicon-aluminum ratio of 0.8-2 is prepared by using a silicon source and an aluminum source;

[0009] Mixing a transition metal precursor, a binder and the low silicon-aluminum ratio molecular sieve in water, and grinding to obtain a mixed slurry; the transition metal is at least one of cerium, manganese, cobalt and copper;

[0010] The mixed slurry is coated on a carrier by a vacuum coating method, and then dried and calcined to obtain a pretreatment agent for silicon-containing VOCs.

[0011] Molecular sieves have great application prospects in the field of adsorption catalysis due to their rich pore structure and large specific surface area. A large number of studies have shown that loading transition metals on molecular sieves can not only make the metal elements more evenly distributed, but also improve the overall catalytic activity of the catalyst, which can make the organic silicon captured on the surface of the pretreatment agent and not decomposed be catalytically decomposed into small molecular silicon, making it easier to generate silicon dioxide crystals and be intercepted. Since silicon has an affinity for aluminum, traditional molecular sieves have a very high silicon-aluminum ratio, which is not conducive to the fixation of silicon.

[0012] The present invention provides a method for preparing a silicon-containing VOCs pretreatment agent, wherein a low silicon-aluminum ratio molecular sieve (which is a low silicon-aluminum ratio MCM-41 molecular sieve) with a silicon-aluminum ratio of 0.8-2 is prepared by a simple process, a transition metal is loaded thereon by an impregnation method, and a binder is added to prepare a required slurry, and finally the slurry is coated on a porous carrier by a vacuum coating technology to prepare an integral pretreatment catalyst. In actual working conditions, the pretreatment agent is placed at the front end of a noble metal catalyst, and the silicon element in the VOCs adsorbed on the surface of the pretreatment agent is preferentially captured by the aluminum site in the pretreatment agent, and the remaining small molecular organic silicon that has not been decomposed is catalytically decomposed to finally generate silicon dioxide crystals at the aluminum site, which stay on the pretreatment agent, reduce its contact with the rear-end noble metal catalyst, and extend the service life of the noble metal catalyst.

[0013] In some embodiments of the present invention, the method for preparing the low silicon-aluminum ratio molecular sieve comprises the following steps:

[0014] Prepare a water glass solution as solution A;

[0015] Sodium oxide and aluminum oxide are mixed in a molar ratio of 2.4-2.6:1 and added into water to obtain solution B after reaction; a surfactant is added into solution B and the pH is adjusted to 9-11;

[0016] The solution A is added dropwise to the solution B with adjusted pH, and the ratio of silicon in solution A to aluminum in solution B is controlled to be 0.8-2; after the addition is completed, the solution is heated in a water bath, crystallized, cooled, washed and dried to obtain a molecular sieve with a low silicon-aluminum ratio.

[0017] The water bath temperature is 28-32°C for 3-5 h; the crystallization temperature is 88-92°C for 5-8 h.

[0018] In some embodiments of the present invention, the solid content of the mixed slurry is 30%-40%, and the solid composition of the mixed solution is: based on the mass percentage of each raw material, the transition metal precursor is 35%-45%, the low silicon-aluminum ratio molecular sieve is 20%-27%, and the rest is a binder.

[0019] In some embodiments of the present invention, the transition metal is a mixture of cerium, manganese, cobalt and copper, and the molar ratio of manganese, cobalt, cerium and copper is (175-180):(290-293):(138:142):(185-190).

[0020] The transition metal precursor is a transition metal salt.

[0021] Preferably, the cerium precursor is at least one of cerium nitrate and cerium sulfate.

[0022] Preferably, the manganese precursor is at least one of manganese acetate and manganese nitrate.

[0023] Preferably, the cobalt precursor is at least one of cobalt nitrate and cobalt hydroxide.

[0024] Preferably, the copper precursor is at least one of copper sulfate and copper nitrate.

[0025] The transition metal exists in the low silicon-aluminum ratio molecular sieve catalyst in the form of oxides, namely, cerium oxide (CeO2), manganese oxide (MnO2), cobalt oxide (CoO2), and copper oxide (CuO).

[0026] In some embodiments of the present invention, the binder is silica sol or alumina sol.

[0027] In some embodiments of the present invention, the transition metal precursor, the binder and the low silicon-aluminum ratio molecular sieve are mixed in water, and the mixture is fully mixed and then ground to obtain the desired slurry. A horizontal grinder can be used for grinding. Specifically, the grinding temperature of the mixed solution is 5°C-20°C, the grinding speed is 300 r / min-1500 r / min, the grinding time is 0.5 h-5h, and the particle size D90 of the slurry obtained after grinding is 1 μm-5 μm, and the viscosity is 10 mPa·S-200 mPa·S.

[0028] In some embodiments of the present invention, the carrier is a cordierite honeycomb ceramic carrier. The cordierite honeycomb ceramic carrier is mainly composed of more than 90% cordierite crystals, has excellent compressive strength, thermal shock resistance and low thermal expansion coefficient, and can meet the application of industrial VOCs catalytic combustion process.

[0029] Preferably, the number of openings in the cross section of the cordierite honeycomb ceramic carrier is 100-600 meshes. In addition, in order to meet the requirements of the space design of engineering equipment during use, the cordierite honeycomb ceramic carrier structure is a cuboid, a cube or a cylinder. Specifically, when the carrier is a cuboid or a cube, its length, width and height can be 100 mm-200 mm, 100 mm-200 mm, 40 mm-200 mm, for example: the length, width and height are 100 mm, 100 mm, 50 mm, etc.; when the cordierite honeycomb ceramic carrier is a cylinder, its diameter and height are 100 mm-330 mm, 100 mm-200 mm, for example, the diameter and height are 330 mm and 150 mm, respectively.

[0030] In some embodiments of the present invention, a bottom-feeding vacuum coating device is used to coat the mixed solution on the surface of the cordierite honeycomb ceramic carrier.

[0031] Wherein, the vacuum degree of the lower feeding vacuum coating is 0.1 MPa-0.5 MPa, and the number of vacuum coating times is 1 time-3 times.

[0032] In some embodiments of the present invention, the drying temperature is 80° C.-120° C. and the time is 0.1 h-0.5 h.

[0033] In some embodiments of the present invention, the calcination temperature is 450° C.-600° C. and the time is 1 h-5 h.

[0034] The second aspect of the present invention provides a pretreatment agent for silicon-containing VOCs, which is prepared by the above-mentioned preparation method.

[0035] The third aspect of the present invention provides a use of the above-mentioned silicon-containing VOCs pretreatment agent in VOCs treatment;

[0036] The application is as follows: the pretreatment agent for silicon-containing VOCs is placed in front of a precious metal catalyst, the silicon element in the VOCs adsorbed on the surface of the pretreatment agent is preferentially captured by the aluminum site in the pretreatment agent, and the remaining small molecular silicone that has not been decomposed is catalytically decomposed to eventually generate silicon dioxide crystals on the aluminum site, which stay on the pretreatment agent, thereby reducing the contact probability between the silicone in the silicon-containing VOCs gas and the precious metal catalyst.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] The present invention uses a low silicon-aluminum ratio molecular sieve to load the transition metal, and the transition metal is evenly distributed on the surface of the low silicon-aluminum ratio molecular sieve, avoiding the fact that the transition metal is embedded in the matrix and cannot play a catalytic role, thereby increasing the production cost. It has been verified that the silicon-containing VOCs pretreatment agent prepared by the present invention can still reduce the probability of contact between the organosilicon and the rear-end precious metal catalyst in the working condition under the condition of low active ingredient addition, and significantly prolong the service life of the precious metal catalyst.

[0039] The silicon-containing VOCs pretreatment agent prepared by the present invention has a simple production process, low production cost, large catalyst specific surface area, high aluminum content, uniform distribution of transition metals, high catalytic activity, and can effectively capture and fix silicon in exhaust gas, effectively solving the problem of deactivation of precious metal catalysts caused by organic silicon in VOCs treatment. The low silicon-aluminum ratio molecular sieve prepared by the present invention has a large specific surface area and uniform and continuous pore distribution, which can make the metal active sites evenly distributed. The present invention introduces transition metals into the low silicon-aluminum ratio molecular sieve, which can catalytically decompose some of the undecomposed small molecule organic silicon in VOCs, and finally is captured by a large number of aluminum sites in the molecular sieve to generate silicon dioxide crystals, reduce the contact between organic silicon and the back-end VOCs precious metal catalyst, and extend the service life of the VOCs precious metal catalyst.

[0040] When the silicon-containing VOCs pretreatment agent provided by the present invention is placed in front of the VOCs precious metal catalyst during actual use, the probability of contact between the organic silicon and the VOCs precious metal catalyst in the working condition can be effectively reduced, the service life of the precious metal catalyst can be significantly extended, the frequency of catalyst replacement can be reduced, and costs can be saved. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0042] Figure 1 The activity decay diagram of the VOCs noble metal catalyst when the silicon-containing VOCs pretreatment agent prepared in Examples 1-8 of the present invention is used in combination with the VOCs noble metal catalyst;

[0043] Figure 2 The activity decay diagram of the VOCs noble metal catalyst when the silicon-containing VOCs pretreatment agent prepared in Examples 1, 9, 10 and Comparative Examples of the present invention is used in combination with the VOCs noble metal catalyst;

[0044] Figure 3 This is the XRD spectrum of the surface coating of the pretreatment agent after the activity decay test of Example 10 of the present invention. DETAILED DESCRIPTION

[0045] Glossary:

[0046] Solid content: The solid content in the present invention is defined as the ratio of the mass of the solid obtained after the mixed slurry is calcined to the mass of the mixed slurry. The calculation formula is as follows:

[0047] Solid content = (m a +m b +m c ×C) / (m a +m c +m d +m e )×100%

[0048] Among them, the mass of the low silicon-aluminum ratio molecular sieve is recorded as m a ; The total mass of the transition metal oxide is denoted as m b ; The mass of silica sol or aluminum sol (binder) is recorded as m c , the concentration of silica sol or aluminum sol (binder) is denoted as C; the total mass of the transition metal precursor is denoted as m d ; The mass of water is recorded as m e .

[0049] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0050] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are explanations of the present invention rather than limitations. In the embodiments, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0051] In the following examples, the concentrations of silica sol and alumina sol are both 30%.

[0052] Example 1

[0053] A method for preparing a silicon-containing VOCs pretreatment agent comprises the following steps:

[0054] Step 1: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution A. Prepare solution B by mixing aluminum oxide, sodium oxide and a certain amount of deionized water according to n (Na2O) / n (Al2O3) = 2.5. Mix hexadecyltrimethylammonium bromide and solution B in deionized water while stirring, adjust the pH value to 10, add solution A dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution A to aluminum in solution B to be 0.9. Place the resulting mixed solution in a water bath, age at 30°C for 3 h, and crystallize at 90°C for 5 h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.9).

[0055] Step 2: 1690 g of manganese nitrate tetrahydrate, 5310 g of molecular sieve raw powder (silicon-aluminum ratio of 0.9), and 450 g of aluminum sol are placed in 12549 g of deionized water and stirred to obtain a mixed solution with a solid content of 30%.

[0056] Step 3: The mixed solution obtained in step 2 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 15°C. The obtained grinding slurry had a particle size D90 of 2 μm-4 μm and a viscosity of 85.1 mPa·S.

[0057] Step 4: The slurry obtained in step 3 is coated on a 200 mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively through a bottom feeding vacuum coating device, the coating vacuum degree is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100°C for 0.5 h and calcined at 500°C for 3 h to prepare a pretreatment agent for silicon-containing VOCs.

[0058] Example 2

[0059] A method for preparing a silicon-containing VOCs pretreatment agent, which differs from Example 1 in that, in step 1, the ratio of silicon in solution A to aluminum in solution B is controlled to be 0.8, the silicon-aluminum ratio of the obtained molecular sieve raw powder is 0.8, and the remaining steps are consistent with Example 1.

[0060] Example 3

[0061] A method for preparing a silicon-containing VOCs pretreatment agent, which differs from Example 1 in that, in step 1, the ratio of silicon in solution A to aluminum in solution B is controlled to be 2, and the silicon-aluminum ratio of the obtained molecular sieve raw powder is 2, and the remaining steps are consistent with Example 1.

[0062] Example 4

[0063] A method for preparing a silicon-containing VOCs pretreatment agent, which differs from Example 1 in that, in step 1, the ratio of silicon in solution A to aluminum in solution B is controlled to be 3, and the silicon-aluminum ratio of the obtained molecular sieve raw powder is 3, and the remaining steps are consistent with Example 1.

[0064] Example 5

[0065] A method for preparing a silicon-containing VOCs pretreatment agent, which differs from Example 1 in that, in step 1, the ratio of silicon in solution A to aluminum in solution B is controlled to be 5, and the silicon-aluminum ratio of the obtained molecular sieve raw powder is 5, and the remaining steps are consistent with Example 1.

[0066] Example 6

[0067] A method for preparing a silicon-containing VOCs pretreatment agent, which differs from Example 1 in that, in step 1, the ratio of silicon in solution A to aluminum in solution B is controlled to be 6, and the silicon-aluminum ratio of the obtained molecular sieve raw powder is 6, and the remaining steps are consistent with Example 1.

[0068] Example 7

[0069] A method for preparing a silicon-containing VOCs pretreatment agent, which differs from Example 1 in that, in step 1, the ratio of silicon in solution A to aluminum in solution B is controlled to be 8, and the silicon-aluminum ratio of the obtained molecular sieve raw powder is 8, and the remaining steps are consistent with Example 1.

[0070] Example 8

[0071] A method for preparing a silicon-containing VOCs pretreatment agent, which differs from Example 1 in that, in step 1, the ratio of silicon in solution A to aluminum in solution B is controlled to be 9, and the silicon-aluminum ratio of the obtained molecular sieve raw powder is 9, and the remaining steps are consistent with Example 1.

[0072] Example 9

[0073] A method for preparing a silicon-containing VOCs pretreatment agent comprises the following steps:

[0074] Step 1: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution A. Prepare solution B by mixing aluminum oxide, sodium oxide and a certain amount of deionized water according to n (Na2O) / n (Al2O3) = 2.5. Mix hexadecyl trimethylammonium bromide and solution B in deionized water while stirring, adjust the pH value to 11, add solution A dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution A to aluminum in solution B to be 0.8. Place the resulting mixed solution in a water bath, age at 30°C for 4 h, and crystallize at 90°C for 7 h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).

[0075] Step 2: 1690 g of manganese nitrate tetrahydrate, 1088 g of cobalt nitrate hexahydrate, 454 g of cerium nitrate hexahydrate, 4830 g of low silicon-aluminum ratio molecular sieve, and 450 g of aluminum sol are placed in 11487 g of deionized water and stirred to obtain a mixed solution with a solid content of 30%.

[0076] Step 3: The mixed solution obtained in step 2 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 15°C. The obtained grinding slurry had a particle size D90 of 2 μm-4 μm and a viscosity of 85.1 mPa·S.

[0077] Step 4: The mixed solution obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively through a bottom feeding vacuum coating device, the coating vacuum degree is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100°C for 0.5 h and calcined at 500°C for 3 h to prepare a pretreatment agent for silicon-containing VOCs.

[0078] Example 10

[0079] A method for preparing a silicon-containing VOCs pretreatment agent comprises the following steps:

[0080] Step 1: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution A. Prepare solution B by mixing aluminum oxide, sodium oxide and a certain amount of deionized water according to n (Na2O) / n (Al2O3) = 2.5. Mix hexadecyl trimethylammonium bromide and solution B in deionized water while stirring, adjust the pH value to 11, add solution A dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution A to aluminum in solution B to be 0.8. Place the resulting mixed solution in a water bath, age at 30°C for 4 h, and crystallize at 90°C for 7 h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).

[0081] Step 2: 1690 g of manganese nitrate tetrahydrate, 1088 g of cobalt nitrate hexahydrate, 378 g of cerium nitrate hexahydrate, 546 g of copper sulfate pentahydrate, 4650 g of low silicon-aluminum ratio molecular sieve, and 450 g of aluminum sol are placed in 11120 g of deionized water and stirred to obtain a mixed solution with a solid content of 30%.

[0082] Step 3: The mixed solution obtained in step 2 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 15°C. The obtained grinding slurry had a particle size D90 of 2 μm-4 μm and a viscosity of 85.1 mPa·S.

[0083] Step 4: The mixed solution obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively through a bottom feeding vacuum coating device, the coating vacuum degree is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100°C for 0.5 h and calcined at 500°C for 3 h to prepare a pretreatment agent for silicon-containing VOCs.

[0084] Comparative Example 1

[0085] A method for preparing a silicon-containing VOCs pretreatment agent comprises the following steps:

[0086] Step 1: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution A. Prepare solution B by mixing aluminum oxide, sodium oxide and a certain amount of deionized water according to n (Na2O) / n (Al2O3) = 2.5. Mix hexadecyl trimethylammonium bromide and solution B in deionized water while stirring, adjust the pH value to 11, add solution A dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution A to aluminum in solution B to be 0.8. Place the resulting mixed solution in a water bath, age at 30°C for 4 h, and crystallize at 90°C for 7 h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).

[0087] Step 2: 1690 g of manganese nitrate tetrahydrate, 1088 g of cobalt nitrate hexahydrate, 378 g of cerium nitrate hexahydrate, 546 g of copper sulfate pentahydrate, 909 g of ferric nitrate nonahydrate, 4830 g of low silicon-aluminum ratio molecular sieve, and 450 g of aluminum sol are placed in 11487 g of deionized water and stirred to obtain a mixed solution with a solid content of 30%.

[0088] Step 3: The mixed solution obtained in step 2 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 15°C. The obtained grinding slurry had a particle size D90 of 2 μm-4 μm and a viscosity of 85.1 mPa·S.

[0089] Step 4: The mixed solution obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively through a bottom feeding vacuum coating device, the coating vacuum degree is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100°C for 0.5 h and calcined at 500°C for 3 h to prepare a pretreatment agent for silicon-containing VOCs.

[0090] Comparative Example 2

[0091] A method for preparing a silicon-containing VOCs pretreatment agent comprises the following steps:

[0092] Step 1: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution A. Prepare solution B by mixing aluminum oxide, sodium oxide and a certain amount of deionized water according to n (Na2O) / n (Al2O3) = 2.5. Mix hexadecyl trimethylammonium bromide and solution B in deionized water while stirring, adjust the pH value to 11, add solution A dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution A to aluminum in solution B to be 0.8. Place the resulting mixed solution in a water bath, age at 30°C for 4 h, and crystallize at 90°C for 7 h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).

[0093] Step 2: 1690 g of manganese nitrate tetrahydrate, 1088 g of cobalt nitrate hexahydrate, 546 g of copper sulfate pentahydrate, 4830 g of low silicon-aluminum ratio molecular sieve, and 450 g of aluminum sol are placed in 11487 g of deionized water and stirred to obtain a mixed solution with a solid content of 30%.

[0094] Step 3: The mixed solution obtained in step 2 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 15°C. The obtained grinding slurry had a particle size D90 of 2 μm-4 μm and a viscosity of 85.1 mPa·S.

[0095] Step 4: The mixed solution obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively through a bottom feeding vacuum coating device, the coating vacuum degree is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100°C for 0.5 h and calcined at 500°C for 3 h to prepare a pretreatment agent for silicon-containing VOCs.

[0096] Comparative Example 3

[0097] A method for preparing a silicon-containing VOCs pretreatment agent comprises the following steps:

[0098] Step 1: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution A. Prepare solution B by mixing aluminum oxide, sodium oxide and a certain amount of deionized water according to n (Na2O) / n (Al2O3) = 2.5. Mix hexadecyl trimethylammonium bromide and solution B in deionized water while stirring, adjust the pH value to 11, add solution A dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution A to aluminum in solution B to be 0.8. Place the resulting mixed solution in a water bath, age at 30°C for 4 h, and crystallize at 90°C for 7 h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).

[0099] Step 2: 1690 g of manganese nitrate tetrahydrate, 378 g of cerium nitrate hexahydrate, 546 g of copper sulfate pentahydrate, 4830 g of low silicon-aluminum ratio molecular sieve, and 450 g of aluminum sol are placed in 11487 g of deionized water and stirred to obtain a mixed solution with a solid content of 30%.

[0100] Step 3: The mixed solution obtained in step 2 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 15°C. The obtained grinding slurry had a particle size D90 of 2 μm-4 μm and a viscosity of 85.1 mPa·S.

[0101] Step 4: The mixed solution obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively through a bottom feeding vacuum coating device, the coating vacuum degree is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100°C for 0.5 h and calcined at 500°C for 3 h to prepare a pretreatment agent for silicon-containing VOCs.

[0102] Comparative Example 4

[0103] A method for preparing a silicon-containing VOCs pretreatment agent comprises the following steps:

[0104] Step 1: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution A. Prepare solution B by mixing aluminum oxide, sodium oxide and a certain amount of deionized water according to n (Na2O) / n (Al2O3) = 2.5. Mix hexadecyl trimethylammonium bromide and solution B in deionized water while stirring, adjust the pH value to 11, add solution A dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution A to aluminum in solution B to be 0.8. Place the resulting mixed solution in a water bath, age at 30°C for 4 h, and crystallize at 90°C for 7 h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).

[0105] Step 2: 1088 g of cobalt nitrate hexahydrate, 378 g of cerium nitrate hexahydrate, 546 g of copper sulfate pentahydrate, 4830 g of low silicon-aluminum ratio molecular sieve, and 450 g of aluminum sol are placed in 11487 g of deionized water and stirred to obtain a mixed solution with a solid content of 30%.

[0106] Step 3: The mixed solution obtained in step 2 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 15°C. The obtained grinding slurry had a particle size D90 of 2 μm-4 μm and a viscosity of 85.1 mPa·S.

[0107] Step 4: The mixed solution obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively through a bottom feeding vacuum coating device, the coating vacuum degree is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100°C for 0.5 h and calcined at 500°C for 3 h to prepare a pretreatment agent for silicon-containing VOCs.

[0108] Comparative Example 5

[0109] A method for preparing a silicon-containing VOCs pretreatment agent comprises the following steps:

[0110] Step 1: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution A. Prepare solution B by mixing aluminum oxide, sodium oxide and a certain amount of deionized water according to n (Na2O) / n (Al2O3) = 2.5. Mix hexadecyl trimethylammonium bromide and solution B in deionized water while stirring, adjust the pH value to 11, add solution A dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution A to aluminum in solution B to be 0.8. Place the resulting mixed solution in a water bath, age at 30°C for 4 h, and crystallize at 90°C for 7 h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).

[0111] Step 2: 1690 g of manganese nitrate tetrahydrate, 1088 g of cobalt nitrate hexahydrate, 378 g of cerium nitrate hexahydrate, 720 g of cadmium nitrate nonahydrate, 4530 g of low silicon-aluminum ratio molecular sieve, and 450 g of aluminum sol are placed in 11066 g of deionized water and stirred to obtain a mixed solution with a solid content of 30%.

[0112] Step 3: The mixed solution obtained in step 2 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 15°C. The obtained grinding slurry had a particle size D90 of 2 μm-4 μm and a viscosity of 85.1 mPa·S.

[0113] Step 4: The mixed solution obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively through a bottom feeding vacuum coating device, the coating vacuum degree is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100°C for 0.5 h and calcined at 500°C for 3 h to prepare a pretreatment agent for silicon-containing VOCs.

[0114] Performance Verification:

[0115] The silicon-containing VOCs pretreatment agent prepared in the examples and comparative examples was tested. A sample of the same size as the precious metal sample was drilled with a drill bit. The pretreatment agent was placed in front of the VOCs precious metal catalyst and connected in series with it. After the pretreatment agent was added, the activity of the VOCs catalyst changed over time.

[0116] Test conditions: xylene: 1000ppm, tetraethyl silicate: 200ppm, volume space velocity: 15000 h -1 .

[0117] Figure 1 This is a graph of the activity attenuation of the VOCs noble metal catalyst when the silicon-containing VOCs pretreatment agent prepared in Examples 1-8 is used in combination with the VOCs noble metal catalyst. Figure 2 This is a graph of the activity decay of the VOCs noble metal catalyst when the silicon-containing VOCs pretreatment agent prepared in Examples 1, 9, 10 and the comparative example is used in combination with the VOCs noble metal catalyst.

[0118] The test results of Examples 1-8 show that as the silicon-aluminum ratio increases, the aluminum sites in the pretreatment agent coating decrease, resulting in a decrease in the sites where the silicon element in the VOCs can preferentially bind, and more silicon escapes into the rear-end precious metal catalyst to generate silicon dioxide crystals that cover the catalyst surface, causing the activity to drop rapidly. The test results of Examples 9-10 show that when multi-component transition metals such as manganese, cobalt, cerium, and copper are introduced into the pretreatment agent coating, due to the synergistic effect between the multiple metals, compared to the single manganese oxide in Example 2, the pretreatment agent of Example 10 has a higher catalytic activity, which can catalyze some of the undecomposed macromolecular organic silicon in the VOCs, making it easier to capture and fix. However, it does not mean that the introduction of too many transition metals will bring better treatment effects. Compared with Comparative Examples 1 and 5, the introduction of more types of metals will reduce the pretreatment effect.

[0119] Figure 3 The XRD spectrum of the surface coating of the pretreatment agent obtained in Example 10 is shown in FIG. Figure 3 It can be seen that after the activity decay test, there is a characteristic peak of silica on the surface of the pretreatment agent coating, which indicates that the silicon element in the VOCs is captured by the aluminum site in the pretreatment agent coating and generates silica crystals.

[0120] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a silicon-containing VOCs pretreatment agent, characterized in that: The steps include: A low silicon-aluminum ratio molecular sieve with a silicon-aluminum ratio of 0.8-2 is prepared by using a silicon source and an aluminum source; Mixing a transition metal precursor, a binder and the low silicon-aluminum ratio molecular sieve in water, and grinding to obtain a mixed slurry; the transition metal is at least one of cerium, manganese, cobalt and copper; The mixed slurry is coated on a carrier by a vacuum coating method, and then dried and calcined to obtain a pretreatment agent for silicon-containing VOCs; The solid content of the mixed slurry is 30%-35%. The solid composition of the mixed slurry is: based on the mass percentage of each raw material, the transition metal precursor is 35%-45%, the low silicon-aluminum ratio molecular sieve is 20%-27%, and the rest is a binder.

2. The preparation method according to claim 1, characterized in that The preparation method of the low silicon-aluminum ratio molecular sieve comprises the following steps: Prepare a water glass solution as solution A; Sodium oxide and aluminum oxide are mixed in a molar ratio of 2.4-2.6:1 and added into water to obtain solution B after reaction; a surfactant is added into solution B and the pH is adjusted to 9-11; The solution A is added dropwise to the solution B with adjusted pH, and the ratio of silicon in solution A to aluminum in solution B is controlled to be 0.8-2; after the addition is completed, the solution is heated in a water bath, crystallized, cooled, washed and dried to obtain a molecular sieve with a low silicon-aluminum ratio.

3. The preparation method according to claim 2, characterized in that: The water bath has a temperature of 28-32°C and a time of 3-5h; The crystallization temperature is 88-92° C. and the time is 5-8 h.

4. The preparation method according to claim 1, characterized in that: The transition metal precursor is a salt of a transition metal; The binder is silica sol or alumina sol.

5. The preparation method according to claim 1, characterized in that: The carrier is a cordierite honeycomb ceramic carrier.

6. The preparation method according to claim 1, characterized in that: The drying temperature is 80°C-120°C and the time is 0.1 h-0.5 h.

7. The preparation method according to claim 1, characterized in that: The calcination temperature is 450°C-600°C and the time is 1h-5h.

8. A pretreatment agent for silicon-containing VOCs, characterized in that: The compound is prepared by the preparation method described in any one of claims 1 to 7.

9. Use of the silicon-containing VOCs pretreatment agent according to claim 8 in VOCs treatment; The application is: the silicon-containing VOCs pretreatment agent is placed in front of the precious metal catalyst to capture the silicon element in the silicon-containing VOCs gas on the aluminum site in the low silicon-aluminum ratio molecular sieve to generate silicon dioxide crystals, so that the silicon element stays on the pretreatment agent, thereby reducing the contact probability between the organic silicon in the silicon-containing VOCs gas and the precious metal catalyst.