A method for preparing layered three-dimensional nanosheets

By inducing the self-assembly of polylactone block copolymers in situ using a highly active catalyst in a low-temperature environment, the problems of high energy consumption and pollution in the existing technology are solved, and the large-scale preparation and unique morphology of three-dimensional nanosheets are realized. It has significant technological progress and practical value.

CN118620189BActive Publication Date: 2024-11-08HEBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411109885.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-08
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing preparation process of polylactone or block copolymers usually needs to be carried out at low or high temperatures, which consumes high energy, is highly polluted, and is difficult to achieve large-scale preparation of three-dimensional nanoassemblies.

Method used

Using high-active catalysts such as phosphazene and diphenyl phosphate in a low temperature environment of -10℃~55℃, in a solvent-free condition, the polylactone block copolymer crystallization self-assembly is formed, forming hexagonal or Shunshaped three-dimensional nanosheets.

Benefits of technology

The large-scale preparation of three-dimensional nanosheets with simple process, green energy-saving and low-cost three-dimensional nanosheets is achieved, and the impact of solvents on the assembly morphology is eliminated, providing a unique three-dimensional nanosheet morphology and broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118620189B_ABST
    Figure CN118620189B_ABST
Patent Text Reader

Abstract

The present invention is a method for preparing layered three-dimensional nanosheets. The method uses highly active catalysts such as phosphazene and diphenyl phosphate, and in a lactone body, in a low temperature environment of ‑10°C to ‑55°C, without the need for solvents, to induce the self-assembly of the crystals of the generated polylactone block copolymer in situ, and can form hexagonal or shuttle-shaped three-dimensional nanosheets. The synthesis method disclosed in the present invention is simple in process, green and energy-saving, low in cost, and can prepare three-dimensional nanosheets on a large scale, with significant technological progress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer synthesis, and particularly relates to a method for preparing layered three-dimensional nanosheets. Background Art

[0002] Block copolymer solution self-assembly is an important method for preparing nanoparticles with precise structures. However, traditional solution self-assembly is usually carried out at a low concentration (<1 wt%), which is costly and difficult to achieve large-scale preparation. Polymerization-induced self-assembly (PISA) successfully achieves high-concentration preparation of nanoparticles (up to 50%) by utilizing the continuous growth of solvophobic segments and in-situ precipitation self-assembly during the polymerization of block copolymers. However, in most PISA implementations, since only the solvophobic effect is used as the driving force, only low-dimensional morphological self-assemblies such as zero-dimensional nanospheres, one-dimensional nanowires, and two-dimensional nanosheets can be formed, and high-dimensional three-dimensional nanoassemblies are difficult to prepare. Therefore, people try to use the crystallization force of crystalline or semi-crystalline polymers as a new crystallization driving force to drive the nanoparticle morphology to a higher order during the PISA process. Semi-crystalline polylactones represented by polycaprolactone and polylactide are widely used as nucleation components for the formation of nanoparticles because they can crystallize at room temperature. Therefore, the core lies in how to develop new polylactone synthesis methods to achieve large-scale preparation of three-dimensional nanoassemblies.

[0003] Patent 202311673149.1 discloses a new process for synthesizing polycaprolactone with narrow molecular weight distribution and high molecular weight using a binary catalytic system composed of an organic base and an organic acid at a temperature of 60-180°C and a pressure of 0-0.1MPa. Patent CN117757053A discloses a new method for multi-branched polylactone, with a reaction temperature of 120-140°C and requiring prepolymerization and post-reaction. Patent CN116769149A discloses a new process for inducing a bulk ring-opening reaction of caprolactone at 80-200°C using a ketimine ligand-diethylzinc as a catalyst, and the polymerization time is only 3 s - 60 min. In the technology disclosed in patent CN11925508B, a double metal cyanide complex is used as a catalyst, an epoxy compound is used as an initiator, and bulk polymerization is carried out at 100-150°C. The synthesized polycaprolactone product has a high tensile strength. Patent CN103497315A successfully prepared a star-shaped comb-shaped polycaprolactone. Due to the use of highly active organic non-metallic catalysts, the polymerization temperature can be controlled at 0-50°C, but aromatic hydrocarbons or alkyl halides are used as solvents. Chen et al. (Polymer, 54 (2013), 6760.) used reversible addition-fragmentation chain transfer agent polymerization and atom transfer radical method to synthesize polycaprolactone- b-block copolymers of polydimethylaminoethyl ester, and then self-assembled in water to prepare low-concentration two-dimensional nanosheets (0.1 wt%). Paul et al. (Nat Commun, 11 (2020), 4690.) used 1,5,7-triazabicyclo[4.4.0]dec-5-ene as a catalyst to disclose a method for rapidly preparing polyethylene glycol- b - A new technology for polylactide block copolymers. Since lactide is soluble in toluene solvent, but polylactide is not soluble, rod-shaped and flake-shaped nanoparticles are prepared in situ during the polymerization of lactide.

[0004] In summary, the existing preparation process of polylactone homopolymer or block copolymer usually needs to be carried out at low temperature and solvent, or in high temperature bulk, which consumes high energy, causes great pollution, and has low concentration, making it difficult to achieve large-scale preparation of assemblies at the same time. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing layered three-dimensional nanosheets in view of the limitations of current technologies. The method uses highly active catalysts such as phosphazene and diphenyl phosphate to induce the self-assembly of polylactone block copolymer crystals in a lactone body at a low temperature of -10°C to 55°C without solvent to form hexagonal or shuttle-shaped three-dimensional nanosheets. The synthesis method disclosed in the present invention is simple in process, green and energy-saving, low in cost, and can be used to prepare three-dimensional nanosheets on a large scale, which is a significant technological advancement.

[0006] The technical solution of the present invention is:

[0007] A method for preparing a layered three-dimensional nanosheet, the method comprising the following steps:

[0008] (1) Add the dried lactone, alcohol initiator and catalyst into the reactor, seal it, evacuate it and fill it with nitrogen;

[0009] Wherein, the weight ratio of lactone, alcohol initiator and catalyst is 100: 0.1-10: 0.1-5, preferably 100: 0.5-6: 0.2-4, more preferably 100: 1.0-3: 0.5-2;

[0010] The lactone is a cyclic lactone, which is a low melting point cyclic lactone ( T m ≤45℃), or low melting point cyclic lactone and high melting point cyclic lactone ( T m >45℃) mixture;

[0011] The catalyst is phosphazene, stannous isooctanoate, scandium trifluoromethanesulfonate, diethyl zinc, zinc octoate, diphenyl phosphate or 1,5,7-triazabicyclo[4.4.0]dec-5-ene;

[0012] (2) The reactor is stirred at -10°C to 55°C, and the lactone bulk ring-opening polymerization reaction is carried out for 4.5-52 hours;

[0013] (3) adding a terminator to the reaction solution in the previous step to stop the reaction, washing, and vacuum drying to obtain layered three-dimensional nanosheets;

[0014] The mass of the terminator is 0.5-2%, preferably 0.8-1.0%, of the mass of the lactone.

[0015] The washing in step (3) is washing with an alcohol solvent and filtering.

[0016] The layered three-dimensional nanosheet is a hexagonal or shuttle-shaped multilayer structure, 5-30 μm long, 1-10 μm wide, 40-5000 nm thick, and a single layer thickness of 10-20 nm. The size of the three-dimensional nanosheet is preferably 10-25 μm long, 5-8 μm wide, and 100-3000 nm thick, especially 15-20 μm long, 6-7 μm wide, and 500-1000 nm thick.

[0017] The low melting point cyclic lactone monomer is one or more of propiolactone, butyrolactone, valerolactone, caprolactone, and enantholactone; the high melting point cyclic lactone is one or more of lactide, trimethylene carbonate, and 3,6-dimethylmorpholine-2,5-dione;

[0018] The types of catalyst and lactone directly determine the reaction temperature. To ensure that the bulk polymerization reaction is carried out between -10°C and 55°C, the reaction temperature is preferably -10°C to 25°C for 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 10°C to 30°C for diphenyl phosphate or phosphazene, 25°C to 40°C for scandium trifluoromethanesulfonate, and 45°C to 55°C for stannous isooctanoate.

[0019] The alcohol initiator is one of alkyl alcohol, polyethylene glycol monomethyl ether, ethylene glycol, polyethylene glycol, polypropylene glycol, glycerol, and polyvinyl alcohol. The alkyl alcohol is a monoalcohol or diol containing 1 to 16 carbon atoms, preferably one of ethanol, n-propanol, n-hexanol, n-decanediol, n-dodecyl alcohol, and n-tetradecanol.

[0020] The terminator is benzoic acid;

[0021] The present invention has the following beneficial effects:

[0022] The three-dimensional nanosheet provided by the invention has a unique morphology and is obtained by in-situ crystallization and self-assembly of a linear, branched or comb-shaped polylactone block copolymer. The three-dimensional nanosheet is symmetrically fan-shaped when viewed from the side and hexagonal or shuttle-shaped when viewed from the top. The nanosheets are stacked layer by layer with a clear layered structure.

[0023] The preparation method of the three-dimensional nanosheets of the present invention, although the raw materials (alcohol initiator, lactone monomer and catalyst) used are similar to the preparation method of some polycaprolactones at present, compared with the preparation technology of the three-dimensional nanosheets commonly used at present, according to the technical points of the present invention, the assembly process of the three-dimensional nanosheets proposed by the present invention is in the bulk polymerization process at low temperature, and no solvent is used, which eliminates the influence of different solvents on the morphology of the assembly, and the preparation method is simple; the reaction temperature is low, and it is green, energy-saving and environmentally friendly; it can be produced by existing devices, and there is no need to upgrade the production line, the production cost is low, and it is easy to prepare three-dimensional nanosheets on a large scale, which has significant technical progress. Those skilled in the art can mix in small batches in the laboratory according to actual engineering needs, or industrially scale up production. Layered three-dimensional nanosheets show broad application prospects in many fields, for example, ① preparation of photonic crystals, used as high-precision optical devices; ② used as a carrier of catalysts, and preparation of high-efficiency metal catalysts; ③ the polylactone used has excellent degradation performance and is used as a biomedical material. Therefore, the layered three-dimensional nanosheets and the preparation method thereof provided by the present invention have great practical value. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0025] Figure 1 This is a scanning electron microscope image of the three-dimensional nanosheet synthesized in Example 1 of the present invention.

[0026] Figure 2 This is a scanning electron microscope image of the three-dimensional nanosheet synthesized in Example 3 of the present invention. DETAILED DESCRIPTION

[0027] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. The preferred embodiments of the present invention are given below. However, the present invention can be implemented in a variety of different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to enable the technical personnel to have a more thorough and comprehensive understanding of the disclosure of the present invention.

[0028] Unless otherwise defined, the technical means and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The terms used in the present specification are only for describing the embodiments and do not limit the protection scope of the present invention.

[0029] Example 1: (1) 100 g of caprolactone, 0.1 g of polyethylene glycol monomethyl ether, and 0.2 g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene were added to a reactor, magnetically stirred and sealed, and vacuum-nitrogen filling cycles were repeated to discharge water and air from the system and fill with nitrogen;

[0030] (2) Maintaining the reactor temperature at 0°C to initiate bulk ring-opening polymerization, the magnetic stirring was continued for 4 hours;

[0031] (3) When layered three-dimensional nanosheets begin to form in the reaction system (monitored by a real-time online turbidity detector), continue the reaction for 60 minutes, then add 2.0 g of benzoic acid terminator to stop the reaction, then add methanol in batches for washing and filtering, repeat the methanol-washing and filtering for more than 3 times, filter out the product and vacuum dry it to obtain layered three-dimensional nanosheets. Its scanning electron microscope image is shown in the figure. Figure 1 The three-dimensional nanosheets are 18-25 μm long, 4-5 μm wide, 3-5 μm thick, 15-20 nm thick, and 20-35 nm apart. The single-layer nanosheets are not stacked in parallel, but grow divergently from the crystal nucleus to form a multi-layer structure that looks like a symmetrical fan-shaped structure from the side, resembling an open thick book; it looks like a hexagonal or shuttle-shaped structure from a top view. When the nanosheets are stacked thicker, the edges of the hexagonal structure are not obvious and turn into a shuttle shape.

[0032] Example 2: (1) 100 g of valerolactone, 0.5 g of n-dodecanol, and 0.3 g of diphenyl phosphate were added to a reactor, mechanically stirred and sealed, and vacuum-nitrogen filling cycles were repeated to discharge water and air from the system and fill with nitrogen;

[0033] (2) Controlling the reactor temperature at 10°C to initiate bulk ring-opening polymerization, and continuing mechanical stirring for 12 hours;

[0034] (3) When layered three-dimensional nanosheets begin to form in the reaction system, continue the reaction for 120 minutes, then add 1.0 g of benzoic acid terminator to stop the reaction, then add methanol in batches for washing and filtering, repeat the methanol-washing and filtering for more than 3 times, filter out the product and vacuum dry it to obtain layered three-dimensional nanosheets with a length of 25-30 μm, a width of 4-5 μm, a thickness of 4-5 μm, and a single layer thickness of 10-14 nm.

[0035] Example 3: (1) 100 g of butyrolactone, 0.5 g of polypropylene glycol, and 0.8 g of scandium trifluoroformate were added to a reactor, stirred evenly, and sealed, and vacuum-nitrogen filling cycles were repeated to discharge water and air from the system and fill with nitrogen;

[0036] (2) The reactor temperature was controlled at 30°C to initiate bulk ring-opening polymerization, and magnetic stirring was continued for 48 hours;

[0037] (3) When layered three-dimensional nanosheets begin to form in the reaction system, continue the reaction for 240 minutes, then add 1.6 g of benzoic acid terminator to stop the reaction, then add methanol in batches for washing and filtering, repeat the methanol-washing and filtering for more than 3 times, filter out the product and vacuum dry it to obtain layered three-dimensional nanosheets with a length of 18-25 μm, a width of 4-5 μm, a thickness of 200-500 nm, a single layer thickness of 10-15 nm, and an interlayer spacing of 15-30 nm. The magnified scanning electron microscope image is shown in the figure. Figure 2 The figure shows more clearly that the single-layer nanosheets are not stacked in parallel, but grow divergently from the crystal core, gradually forming a multi-layer structure that looks like a symmetrical fan-shaped structure when viewed from the side. The crystal core in the middle is similar to the spine of a book, resembling an open thick book.

[0038] Example 4: (1) 80 g of caprolactone, 20 g of lactide, 1.2 g of glycerol, and 1.0 g of phosphazene were added to a reactor, mechanically stirred and sealed, and vacuum-nitrogen filling cycles were repeated to discharge water and air from the system and fill with nitrogen;

[0039] (2) Controlling the reactor temperature at 20°C, initiating bulk ring-opening polymerization, and continuing mechanical stirring for 6 hours;

[0040] (3) When layered three-dimensional nanosheets begin to form in the reaction system, continue the reaction for 150 minutes, then add 0.8 g of benzoic acid terminator to stop the reaction, then add ethanol in batches for washing and filtering, repeat the methanol-washing and filtering for more than 3 times, filter out the product and vacuum dry it to obtain layered three-dimensional nanosheets with a length of 10-18 μm, a width of 6-8 μm, a thickness of 800-1200 nm, and a single layer thickness of 10-15 nm.

[0041] Example 5: (1) 90 g of propiolactone, 10 g of 3,6-dimethylmorpholine-2,5-dione, 5 g of polyethylene glycol, and 0.5 g of zinc octoate were added to a reactor, stirred evenly, and sealed, and vacuum-nitrogen filling cycles were repeated to discharge water and air from the system and fill with nitrogen;

[0042] (2) The reactor temperature was controlled at 35°C to initiate bulk ring-opening polymerization, and magnetic stirring was continued for 40 hours;

[0043] (3) When layered three-dimensional nanosheets begin to form in the reaction system, continue the reaction for 120 minutes, then add 1.2 g of benzoic acid terminator to stop the reaction, then add methanol in batches for washing and filtering, repeat the methanol-washing and filtering for more than 3 times, filter out the product and vacuum dry it to obtain layered three-dimensional nanosheets with a length of 5-10 μm, a width of 1-4 μm, a thickness of 40-1000 nm, and a single layer thickness of 10-13 nm.

[0044] Example 6: (1) 100 g of enantholactone, 10 g of polyvinyl alcohol, and 5 g of stannous isooctanoate were added to a reactor, stirred evenly, and sealed, and vacuum-nitrogen filling cycles were repeated to discharge water and air from the system and fill with nitrogen;

[0045] (2) The reactor temperature was controlled at 55°C to initiate bulk ring-opening polymerization, and magnetic stirring was continued for 15 hours;

[0046] (3) When layered three-dimensional nanosheets begin to form in the reaction system, continue the reaction for 36 minutes, then add 2 g of benzoic acid terminator to stop the reaction, then add propanol in batches for washing and filtering, and repeat the methanol-washing and filtering for more than 3 times. Filter out the product and vacuum dry it to obtain layered three-dimensional nanosheets with a length of 15-20 μm, a width of 6-7 μm, a thickness of 500-800 nm, and a single layer thickness of 15-18 nm.

[0047] Comparative Example 1: (1) 1000 g of toluene, 100 g of caprolactone, 0.1 g of polyethylene glycol monomethyl ether and 0.2 g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene were added to a reactor, stirred evenly, sealed, and vacuum-nitrogen-filling cycles were repeated to discharge water and air from the system and then fill with nitrogen;

[0048] (2) The reactor temperature was controlled at 0°C to initiate bulk ring-opening polymerization, and magnetic stirring was continued for 4 hours;

[0049] (3) When the reaction system becomes turbid, continue the reaction for 60 minutes, then add 2.0 g of benzoic acid terminator to stop the reaction, then add methanol in batches for washing and filtering, repeat the methanol-washing and filtering for more than 3 times, filter out the product and vacuum dry it to obtain irregular spindle-shaped nanosheets with a thickness of 800-1200 nm.

[0050] Comparative Example 2: (1) 100 g of enantholactone, 10 g of polyvinyl alcohol, and 5 g of stannous isooctanoate were added to a reactor, stirred evenly, and sealed, and vacuum-nitrogen filling cycles were repeated to discharge water and air from the system and fill with nitrogen;

[0051] (2) Controlling the reactor temperature at 120°C to initiate bulk ring-opening polymerization, and continuing magnetic stirring for 15 hours;

[0052] (3) When the reaction system becomes viscous, continue the reaction for 36 minutes, then add 2 g of benzoic acid terminator to stop the reaction. After slowly cooling to room temperature, add propanol in batches for washing and filtering. Repeat methanol-washing and filtering for more than 3 times. Filter out the product and vacuum dry it to obtain a waxy solid. No regular morphology can be observed under an electron microscope.

[0053] Comparative Example 3: (1) 100 g of caprolactone, 0.1 g of polyethylene glycol monomethyl ether, and 0.2 g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene were added to a reactor, stirred evenly, sealed, and vacuum-nitrogen-filling cycles were repeated to discharge water and air from the system and fill with nitrogen;

[0054] (2) The reactor temperature was controlled at 0°C to initiate bulk ring-opening polymerization, and magnetic stirring was continued for 3 hours;

[0055] (3) When layered three-dimensional nanosheets begin to form in the reaction system, the reaction is continued for 600 minutes, and then 2.0 g of benzoic acid terminator is added to stop the reaction. Methanol is then added in batches for washing and filtering. The methanol-washing and filtering are repeated for more than 3 times. The product is filtered out and vacuum dried to form a waxy solid with no regular morphology under an electron microscope.

[0056] According to Examples 1-6 and Comparative Examples 1-3, it can be seen that in ordinary solution polymerization, although irregular shuttle-shaped nanosheets can also be obtained by selective solvents (Comparative Example 1), organic solvents are used, which are more polluting, difficult to post-process, have high energy consumption, and are difficult to produce on a large scale; in high-temperature bulk polymerization (Comparative Example 2), the reaction process is in a molten state, no assembly is generated, and in the cooling process after reaching a high conversion rate, the polylactone block copolymer gradually crystallizes and precipitates, but a regular morphology cannot be obtained; in low-temperature bulk reaction (Comparative Example 3), the ordinary method often prolongs the reaction time to increase the monomer conversion rate, and it is very easy to become a waxy solid at a high conversion rate, and it is also difficult to obtain a regular morphology. Therefore, compared with the prior art, the present invention can prepare three-dimensional nanosheets at low temperatures with high efficiency and low cost, and provides a new technical means for the large-scale preparation of nano assemblies with precise structures, with outstanding substantive characteristics and significant progress.

[0057] In addition, according to the above examples, low melting point lactones such as caprolactone and valerolactone are liquid at reaction temperature, and can be used as both monomers and solvents during the polymerization process. At the same time, polylactones are insoluble in lactone monomers, so polylactones can be crystallized and self-assembled without solvents. High melting point cyclic lactones, such as lactide and 3,6-dimethylmorpholine-2,5-dione, usually have high melting points and are solid at room temperature and difficult to polymerize. Therefore, the inventors use high melting point cyclic lactones in combination with low melting point cyclic lactone monomers, dissolving high melting point cyclic lactones in low melting point lactones to achieve bulk polymerization.

[0058] In addition, the inventors discovered through experiments that the size of the three-dimensional nanosheets is closely related to the ratio of the initiator and the polylactone blocks. When the polylactone content is higher, the nanosheet size is larger and the sample is thicker (Example 1); conversely, when the initiator content is lower, the nanosheet size is smaller and the sample is thinner (Example 3).

[0059] The technical features of the above-described embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above-described embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as a limitation on the scope of the invention patent. It should be pointed out that for those skilled in the art, without departing from the concept of the present invention, several variations and improved embodiments can be made, which all belong to the protection scope of the present invention.

[0060] Matters not covered by the present invention are known technologies.

Claims

1. A method for preparing a layered three-dimensional nanosheet, characterized in that the method comprises the following steps: (1) Add the dried lactone, alcohol initiator and catalyst into the reactor, seal it, evacuate it and fill it with nitrogen; in, The weight ratio of lactone, alcohol initiator and catalyst is 100: 0.1-10: 0.1-5; The lactone is a low melting point cyclic lactone T m ≤45℃, or low melting point cyclic lactone and high melting point cyclic lactone T m >45℃ mixture; The low melting point cyclic lactone is one or more of propiolactone, butyrolactone, valerolactone, caprolactone, and enantholactone; the high melting point cyclic lactone is one or more of lactide, trimethylene carbonate, and 3,6-dimethylmorpholine-2,5-dione; The catalyst is phosphazene, stannous isooctanoate, scandium trifluoromethanesulfonate, diethyl zinc, zinc octoate or diphenyl phosphate; The alcohol initiator is one of alkyl alcohol, polyethylene glycol monomethyl ether, ethylene glycol, polyethylene glycol, polypropylene glycol, glycerol, and polyvinyl alcohol; (2) The reactor is stirred at 10°C to 55°C, and the lactone bulk ring-opening polymerization reaction is carried out for 4.5-52 hours; (3) adding a terminator to the reaction solution in the previous step to stop the reaction, washing, and vacuum drying to obtain layered three-dimensional nanosheets; The mass of the terminator is 0.5-2% of the mass of the lactone.

2. The method for preparing the layered three-dimensional nanosheet according to claim 1, characterized in that The terminator is benzoic acid.

3. The method for preparing the layered three-dimensional nanosheet according to claim 1, characterized in that The washing in step (3) is washing with an alcohol solvent and filtering.

4. The method for preparing the layered three-dimensional nanosheet according to claim 1, characterized in that The layered three-dimensional nanosheet is a hexagonal or shuttle-shaped multilayer structure with a length of 5-30 μm, a width of 1-10 μm, a thickness of 40-5000 nm, and a single layer thickness of 10-20 nm.

5. The method for preparing layered three-dimensional nanosheets as claimed in claim 1, characterized in that when the catalyst is diphenyl phosphate or phosphazene, the reaction temperature is 10-30°C; when the catalyst is scandium trifluoromethanesulfonate, the reaction temperature is 25-40°C; when the catalyst is stannous isooctanoate, the reaction temperature is 45-55°C.

6. The method for preparing the layered three-dimensional nanosheet according to claim 1, characterized in that The alkyl alcohol is one of ethanol, n-propanol, n-hexanol, n-decanediol, n-dodecanol and n-tetradecanol.