A method for preparing an impact-resistant modified composite protective film for automatic doors
By reacting maleic anhydride-grafted polyethylene with intermediates such as nano-silica to form modified polyethylene, and mixing it with other materials to prepare an impact-resistant modified composite protective film, it solves the problem of self-healing performance of traditional polyethylene films. deficiencies, achieving high impact resistance and self-healing performance in automatic door applications.
Patent Information
- Application Number
- CN202411070443.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-06
AI Technical Summary
Traditional polyethylene films lack self-healing properties in automatic door applications and cannot meet modern needs, especially in terms of impact and scratch performance.
By reacting maleic anhydride-grafted polyethylene with intermediates such as nanosilica to form modified polyethylene, and mixing it with high-density polyethylene, polypropylene and other materials, it is prepared using a twin-screw extruder and a film blowing machine. Impact-resistant modified composite protective film, nano-silica particles are evenly distributed to improve impact resistance, and self-healing properties are improved through self-healing bonds.
The prepared film not only has excellent impact resistance, but also has good self-healing properties. It can automatically repair when damaged and extend its service life.
Smart Images

Figure CN118620261B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of films, in particular to a method for preparing an impact-resistant modified composite protective film for automatic doors. Background Art
[0002] Automatic doors are widely used in large buildings, shopping malls, homes and other fields. The application range is very wide. However, during the use of automatic doors, they are often subject to impact, scratching and other problems, which in turn affects the service life of the automatic doors. Therefore, it is necessary to cover the surface of the automatic door with a layer of protective film.
[0003] Polyethylene is a thermoplastic resin prepared by polymerization of ethylene monomer. It has excellent properties and is widely used in packaging materials, wires and cables, etc. Polyethylene films prepared from polyethylene have good mechanical properties, chemical corrosion resistance, low temperature impact resistance and low price and are widely used. However, with the rapid development of science and technology, traditional polyethylene films can no longer meet the demand, so they need to be modified to expand their application areas.
[0004] For example, the patent with authorization announcement number CN 106393911 B discloses a polyethylene terephthalate-modified linear low-density polyethylene composite film and a processing method thereof. The polyethylene composite film prepared by the invention has good impact resistance, tensile properties, etc., but does not improve its self-healing properties. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing an impact-resistant modified composite protective film for automatic doors. The prepared film has excellent impact resistance and self-repairing properties.
[0007] (II) Technical solution
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] A method for preparing an impact-resistant modified composite protective film for an automatic door, the preparation method comprising:
[0010] Step (1), adding maleic anhydride grafted polyethylene to xylene solvent, and then adding intermediate 3 thereto, wherein the amount ratio of maleic anhydride grafted polyethylene to intermediate 3 is 100g:(5-10)g, stirring and dispersing, reacting at 65-75°C for 20-30h, after the reaction is completed, filtering, washing, and drying to obtain modified polyethylene.
[0011] Step (2), adding high-density polyethylene, modified polyethylene, polypropylene, and dioctyl phthalate into a high-speed mixer, wherein the amount ratio of high-density polyethylene, modified polyethylene, polypropylene, and dioctyl phthalate is 100g: (50-100)g: (10-30)g: (15-25)g, mixing evenly, using a twin-screw extruder to extrude granules, and then placing the granules in a film blowing machine for film blowing to obtain an impact-resistant modified composite protective film for automatic doors.
[0012] Preferably, in step (2), the temperature of the twin-screw extruder is set to 172-183°C; the film blowing temperature of the film blowing machine is set to 190-230°C, the stretching speed is 23.1 r / min, and the blow-up ratio is 3.5.
[0013] Preferably, in step (1), the preparation method of intermediate 3 is:
[0014] S1. Under nitrogen conditions, add nano-silica to toluene solvent, stir and disperse for 20-40 minutes, add allyltriethoxysilane thereto, react at 75-85°C for 20-30 hours, and after the reaction is completed, filter under negative pressure, wash, and dry to obtain olefinated nano-silica.
[0015] S2. Under nitrogen conditions, D-cystine and olefinated nano-silica were added to methanol solvent, stirred and dispersed, and reacted at 40-60° C. for 24-48 hours. After the reaction was completed, negative pressure filtration was performed, washed, and dried to obtain intermediate 1.
[0016] S3. Under nitrogen conditions, add intermediate 1 and 2-furanmethylamine to N,N-dimethylformamide solvent, stir and disperse, then add N,N-dicyclohexylcarbodiimide (DCC) and 4-dimethylaminopyridine (DMPA) thereto, stir and react at room temperature for 20-40 hours. After the reaction is completed, filter, wash and dry to obtain intermediate 2.
[0017] S4. Under nitrogen conditions, add intermediate 2 and N-(2-aminoethyl)maleimide to N,N-dimethylformamide solvent, stir and disperse, react at 50-65°C for 20-36h. After the reaction is completed, filter, wash and dry to obtain intermediate 3.
[0018] Preferably, in step S1, the usage ratio of nano-silicon dioxide and allyltriethoxysilane is 1 g: (0.12-0.25) mol.
[0019] Preferably, in step S2, the usage ratio of D-cystine to olefinated nano-silica is 1 mol: (4-5) mol.
[0020] Preferably, in step S3, the usage ratio of the intermediate 1, 2-furanmethylamine, DCC and DMPA is 1 mol: (2-2.5) mol: (2-3) mol: (2-3) mol.
[0021] Preferably, in step S4, the usage ratio of intermediate 2 and N-(2-aminoethyl)maleimide is 1 mol:(2-2.5) mol.
[0022] 3. Beneficial technical effects
[0023] The present invention uses the hydroxyl contained in nano silicon dioxide and allyl triethoxysilane to undergo condensation reaction to obtain olefinic nano silicon dioxide. D-cystine and olefinic nano silicon dioxide are used as raw materials, and an intermediate 1 is obtained through reaction. The intermediate 1 is sequentially reacted with 2-furan methylamine and N-(2-aminoethyl) maleimide through amidation reaction and DA reaction to obtain an intermediate 3, and then the intermediate 3 is subjected to ring-opening reaction with maleic anhydride grafted polyethylene to obtain modified polyethylene. Finally, the modified polyethylene, polypropylene and the like are added to the polyethylene and mixed evenly, extruded and granulated, and film blown to obtain an impact-resistant modified composite protective film for automatic doors.
[0024] The intermediate 3 prepared by a series of reactions contains nano silicon dioxide. The nano silicon dioxide itself is easy to agglomerate and has poor compatibility with organic substances. The present invention makes it organic, reduces the degree of agglomeration, increases its compatibility with organic substances, and improves its dispersion effect in organic substances. The intermediate 3 is reacted with maleic anhydride grafted polyethylene, and the obtained product is added to polyethylene to prepare a film. The nano silicon dioxide particles are uniformly distributed in the film material. When subjected to external impact, the nano silicon dioxide particles, as stress concentration points, can absorb more impact energy, and as the impact energy increases, can induce shear yield of the matrix around the particles, further improving the impact resistance of the film.
[0025] The intermediate 3 prepared by the present invention contains a DA bond and a disulfide bond, both of which are self-repairing bonds and have good self-repairing properties. When the intermediate 3 is added to a film, when the film is damaged by the outside and shows scratches, it can be self-repaired, thereby extending the service life of the film. In addition, the nano-silicon dioxide particles contained therein have the characteristics of small particle size and high surface activity, and have a strong interfacial force with the material. When the material is damaged by cracks, the nano-silicon dioxide can effectively locate the damaged area, diffuse and migrate to the crack area, and repair the damaged part, further improving the self-repairing performance of the film. The film prepared by the present invention has good self-repairing performance and impact resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1This is the preparation route of intermediate 3. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0028] Preparation method of maleic anhydride grafted polyethylene: add 10g of maleic anhydride, 100g of low-density polyethylene, and 1g of diisopropylbenzene peroxide into a high-speed mixer and mix for 5 minutes, then place it in a twin-screw extruder, extrude and granulate, the extruder temperature is 200°C, and obtain maleic anhydride grafted polyethylene. Embodiment 1
[0029] (1) Under nitrogen conditions, 5 g of nano-silica was added to 100 mL of toluene solvent, and the mixture was stirred and dispersed for 40 min. 1 mol of allyltriethoxysilane was added thereto, and the mixture was reacted at 80 °C for 28 h. After the reaction was completed, the mixture was filtered under negative pressure, washed, and dried to obtain olefinated nano-silica.
[0030] (2) Under nitrogen conditions, 20 mmol of D-cystine and 100 mmol of olefinated nano-silica were added to 100 mL of methanol solvent, stirred and dispersed, and reacted at 50° C. for 48 h. After the reaction was completed, the mixture was filtered under negative pressure, washed, and dried to obtain intermediate 1.
[0031] (3) Under nitrogen conditions, 20 mmol of intermediate 1 and 45 mmol of 2-furanmethylamine were added to 150 mL of N,N-dimethylformamide solvent and dispersed with stirring. Then, 60 mmol of DCC and 40 mmol of DMPA were added thereto and stirred for reaction at room temperature for 24 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 2.
[0032] (4) Under nitrogen conditions, 10 mmol of intermediate 2 and 20 mmol of N-(2-aminoethyl)maleimide were added to 200 mL of N,N-dimethylformamide solvent, stirred and dispersed, and reacted at 65°C for 24 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain intermediate 3.
[0033] (5) 10 g of maleic anhydride grafted polyethylene was added to 200 mL of xylene solvent, and then 0.6 g of intermediate 3 was added thereto, stirred and dispersed, and reacted at 70° C. for 30 h. After the reaction was completed, the modified polyethylene was filtered, washed, and dried to obtain the modified polyethylene.
[0034] (6) Add 10 g of high-density polyethylene, 5 g of modified polyethylene, 1 g of polypropylene, and 2 g of dioctyl phthalate into a high-speed mixer, mix well, and use a twin-screw extruder to extrude and granulate. The temperature of the twin-screw extruder is set to 172-183°C. Then place it in a film blowing machine for film blowing. The film blowing temperature of the film blowing machine is set to 190-230°C, the stretching speed is 23.1 r / min, and the blowing ratio is 3.5, to obtain an impact-resistant modified composite protective film for automatic doors. Embodiment 2
[0035] (1) Under nitrogen conditions, 5 g of nano-silica was added to 100 mL of toluene solvent, and the mixture was stirred and dispersed for 30 min. 0.6 mol of allyltriethoxysilane was added thereto, and the mixture was reacted at 75 °C for 30 h. After the reaction was completed, the mixture was filtered under negative pressure, washed, and dried to obtain olefinated nano-silica.
[0036] (2) Under nitrogen conditions, 20 mmol of D-cystine and 90 mmol of olefinic nano-silica were added to 100 mL of methanol solvent, stirred and dispersed, and reacted at 60° C. for 24 h. After the reaction was completed, the mixture was filtered under negative pressure, washed, and dried to obtain intermediate 1.
[0037] (3) Under nitrogen conditions, 20 mmol of intermediate 1 and 45 mmol of 2-furanmethylamine were added to 150 mL of N,N-dimethylformamide solvent and dispersed with stirring. Then, 40 mmol of DCC and 60 mmol of DMPA were added thereto and stirred for reaction at room temperature for 20 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 2.
[0038] (4) Under nitrogen conditions, 10 mmol of intermediate 2 and 25 mmol of N-(2-aminoethyl)maleimide were added to 200 mL of N,N-dimethylformamide solvent, stirred and dispersed, and reacted at 50°C for 20 h. After the reaction, the mixture was filtered, washed, and dried to obtain intermediate 3.
[0039] (5) 10 g of maleic anhydride grafted polyethylene was added to 200 mL of xylene solvent, and then 0.6 g of intermediate 3 was added thereto, stirred and dispersed, and reacted at 65° C. for 20 h. After the reaction was completed, the modified polyethylene was filtered, washed, and dried to obtain the modified polyethylene.
[0040] (6) Add 10 g of high-density polyethylene, 6 g of modified polyethylene, 2 g of polypropylene, and 1.5 g of dioctyl phthalate into a high-speed mixer, mix well, and use a twin-screw extruder to extrude and granulate. The temperature of the twin-screw extruder is set to 172-183°C. Then place it in a film blowing machine for film blowing. The film blowing temperature of the film blowing machine is set to 190-230°C, the stretching speed is 23.1 r / min, and the blowing ratio is 3.5, to obtain an impact-resistant modified composite protective film for automatic doors. Embodiment 3
[0041] (1) Under nitrogen conditions, 5 g of nano-silica was added to 100 mL of toluene solvent, and the mixture was stirred and dispersed for 20 min. Then, 0.8 mol of allyltriethoxysilane was added thereto, and the mixture was reacted at 85 °C for 20 h. After the reaction was completed, the mixture was filtered under negative pressure, washed, and dried to obtain olefinated nano-silica.
[0042] (2) Under nitrogen conditions, 20 mmol of D-cystine and 80 mmol of olefinic nano-silica were added to 100 mL of methanol solvent, stirred and dispersed, and reacted at 40° C. for 36 h. After the reaction was completed, the mixture was filtered under negative pressure, washed, and dried to obtain intermediate 1.
[0043] (3) Under nitrogen conditions, 20 mmol of intermediate 1 and 40 mmol of 2-furanmethylamine were added to 150 mL of N,N-dimethylformamide solvent and dispersed with stirring. Then, 50 mmol of DCC and 40 mmol of DMPA were added thereto and stirred for reaction at room temperature for 30 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 2.
[0044] (4) Under nitrogen conditions, 10 mmol of intermediate 2 and 25 mmol of N-(2-aminoethyl)maleimide were added to 200 mL of N,N-dimethylformamide solvent, stirred and dispersed, and reacted at 55°C for 36 h. After the reaction, the mixture was filtered, washed, and dried to obtain intermediate 3.
[0045] (5) Add 10 g of maleic anhydride grafted polyethylene to 200 mL of xylene solvent, then add 1 g of intermediate 3, stir and disperse, and react at 75° C. for 24 h. After the reaction is completed, filter, wash, and dry to obtain modified polyethylene.
[0046] (6) Add 10 g of high-density polyethylene, 8 g of modified polyethylene, 2.5 g of polypropylene, and 2.5 g of dioctyl phthalate into a high-speed mixer, mix well, and use a twin-screw extruder to extrude and granulate. The temperature of the twin-screw extruder is set to 172-183°C. Then place it in a film blowing machine for film blowing. The film blowing temperature of the film blowing machine is set to 190-230°C, the stretching speed is 23.1 r / min, and the blowing ratio is 3.5, to obtain an impact-resistant modified composite protective film for automatic doors. Embodiment 4
[0047] (1) Under nitrogen conditions, 5 g of nano-silica was added to 100 mL of toluene solvent, and the mixture was stirred and dispersed for 40 min. 1.25 mol of allyltriethoxysilane was added thereto, and the mixture was reacted at 80 °C for 24 h. After the reaction was completed, the mixture was filtered under negative pressure, washed, and dried to obtain olefinated nano-silica.
[0048] (2) Under nitrogen conditions, 20 mmol of D-cystine and 90 mmol of olefinic nano-silica were added to 100 mL of methanol solvent, stirred and dispersed, and reacted at 50° C. for 36 h. After the reaction was completed, the mixture was filtered under negative pressure, washed, and dried to obtain intermediate 1.
[0049] (3) Under nitrogen conditions, 20 mmol of intermediate 1 and 50 mmol of 2-furanmethylamine were added to 150 mL of N,N-dimethylformamide solvent and dispersed with stirring. Then, 60 mmol of DCC and 50 mmol of DMPA were added thereto and stirred for reaction at room temperature for 40 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 2.
[0050] (4) Under nitrogen conditions, 10 mmol of intermediate 2 and 24 mmol of N-(2-aminoethyl)maleimide were added to 200 mL of N,N-dimethylformamide solvent, stirred and dispersed, and reacted at 60°C for 26 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain intermediate 3.
[0051] (5) 10 g of maleic anhydride grafted polyethylene was added to 200 mL of xylene solvent, and then 0.5 g of intermediate 3 was added thereto, and the mixture was stirred and dispersed. The mixture was reacted at 70° C. for 30 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain modified polyethylene.
[0052] (6) Add 10 g of high-density polyethylene, 10 g of modified polyethylene, 3 g of polypropylene, and 2.5 g of dioctyl phthalate into a high-speed mixer, mix well, and use a twin-screw extruder to extrude and granulate. The temperature of the twin-screw extruder is set to 172-183°C. Then place it in a film blowing machine for film blowing. The film blowing temperature of the film blowing machine is set to 190-230°C, the stretching speed is 23.1 r / min, and the blowing ratio is 3.5, to obtain an impact-resistant modified composite protective film for automatic doors.
[0053] Comparative Example 1
[0054] The difference between this comparative example and Example 1 is that in step (6), maleic anhydride grafted polyethylene is used instead of modified polyethylene.
[0055] Referring to GB / T9639.1-2008, a dart impact tester was used to test the impact performance of the film. The film size was 30 mm × 30 mm.
[0056] With reference to GB / T1040-1992, a universal material testing machine was used to test the tensile properties of the film at a test speed of 10 mm / min.
[0057] Table 1: Impact performance test and tensile performance test results of various embodiments and comparative examples
[0058]
[0059] It can be seen from the table that the protective film prepared by the present invention has excellent impact resistance and tensile properties, the maximum dart impact breakage mass can reach 70g, and the maximum tensile strength can reach 48.7MPa.
[0060] The tensile strength of the film was tested using a tensile testing machine at a tensile speed of 200 mm / min and the data was recorded. The film was cut with scissors and repaired at 80°C for 12 h. The tensile strength of the film was tested again using a tensile testing machine and the data was recorded. Self-healing efficiency (%) = tensile strength after repair / tensile strength before repair × 100.
[0061] Table 2: Self-repair performance test results of various embodiments and comparative examples
[0062]
[0063] It can be seen from the table that the film prepared by the present invention has good self-repairing performance, and the maximum self-repairing efficiency can reach 75.0%.
[0064] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing an impact-resistant modified composite protective film for automatic doors, It is characterized in that The preparation method is: Step (1), adding maleic anhydride grafted polyethylene to xylene solvent, then adding intermediate 3 thereto, stirring and dispersing, reacting at 65-75° C. for 20-30 hours, filtering, washing and drying after the reaction to obtain modified polyethylene, wherein the amount ratio of maleic anhydride grafted polyethylene to intermediate 3 is 100 g:(5-10) g; Step (2), adding high-density polyethylene, modified polyethylene, polypropylene, and dioctyl phthalate to a high-speed mixer, mixing evenly, using a twin-screw extruder to extrude and granulate, and then placing it in a film blowing machine for film blowing to obtain an automatic door impact-resistant modified composite protective film, wherein the amount ratio of the high-density polyethylene, modified polyethylene, polypropylene, and dioctyl phthalate is 100g: (50-100)g: (10-30)g: (15-25)g; the preparation method of the intermediate 3 is: S1. Under nitrogen conditions, add nano-silica to toluene solvent, stir and disperse for 20-40 minutes, add allyl triethoxysilane thereto, react at 75-85°C for 20-30 hours, and after the reaction is completed, filter under negative pressure, wash, and dry to obtain olefinated nano-silica; S2. Under nitrogen conditions, D-cystine and olefinic nano-silica are added to a methanol solvent, stirred and dispersed, and reacted at 40-60° C. for 24-48 hours. After the reaction is completed, negative pressure filtration, washing, and drying are performed to obtain an intermediate 1; S3, under nitrogen conditions, adding intermediate 1, 2-furanmethylamine to N,N-dimethylformamide solvent, stirring and dispersing, then adding DCC and DMPA thereto, stirring and reacting at room temperature for 20-40 hours, after the reaction is completed, filtering, washing, and drying to obtain intermediate 2; S4. Under nitrogen conditions, add intermediate 2 and N-(2-aminoethyl)maleimide to N,N-dimethylformamide solvent, stir and disperse, react at 50-65°C for 20-36h. After the reaction is completed, filter, wash and dry to obtain intermediate 3.
2. The method for preparing the impact-resistant modified composite protective film for automatic doors according to claim 1, It is characterized in that In the step (2), the temperature of the twin-screw extruder is set to 172-183° C.; the film blowing temperature of the film blowing machine is set to 190-230° C., the stretching speed is 23.1 r / min, and the blowing ratio is 3.
5.
3. The method for preparing the impact-resistant modified composite protective film for automatic doors according to claim 1, It is characterized in that In the step S1, the usage ratio of nano-silicon dioxide and allyltriethoxysilane is 1 g: (0.12-0.25) mol.
4. The method for preparing the impact-resistant modified composite protective film for automatic doors according to claim 1, It is characterized in that In the step S2, the usage ratio of D-cystine to olefinated nano-silica is 1 mol:(4-5) mol.
5. The method for preparing the impact-resistant modified composite protective film for automatic doors according to claim 1, It is characterized in that In the step S3, the usage ratio of the intermediate 1, 2-furanmethylamine, DCC and DMPA is 1 mol:(2-2.5) mol:(2-3) mol:(2-3) mol.
6. The method for preparing the impact-resistant modified composite protective film for automatic doors according to claim 1, It is characterized in that In the step S4, the usage ratio of the intermediate 2 and N-(2-aminoethyl)maleimide is 1 mol:(2-2.5) mol.
Citation Information
Patent Citations
A polyethylene terephthalate modified linear low-density polyethylene composite film and its processing method
CN106393911B
Cyclotriphosphazene type epoxy resin preparation method
CN107337692A
Diels-Alder bond containing self-repairing flame retardant polyurethane elastomer and preparation method thereof
CN108440735A
High-wear-resistance plastic floor and preparation method thereof
CN118061628A
Rubber composition for chafer, and heavy-load pneumatic tire using the same
JP2001226526A