A method for improving the processing performance of high specific gravity tungsten alloy
Through the mixing of ammonium paratungstate solution and low-melting metal powder and hydrogen reduction, a micron-level pre-alloy powder is formed. Combined with powder rolling and liquid phase sintering technology, the cracking and edge cracking of high specific gravity tungsten alloys during cold rolling is solved. Improves the yield and processing performance and reduces production costs.
Patent Information
- Application Number
- CN202411097281.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-12
AI Technical Summary
High specific gravity tungsten alloys are prone to defects such as cracking and edge cracking during cold rolling, resulting in low yield and high production costs. It is difficult for the prior art to form a complete alloy structure and weak binding force.
The prealloy powder is prepared by mixing ammonium paratungstate solution with low melting point metal powder, reducing hydrogen, controlling the carbon and oxygen content, and forming a micron-level two-phase alloy structure through powder rolling, liquid phase sintering and heat treatment to improve processing performance.
The toughness and strength of high specific gravity tungsten alloys are significantly improved, cracking and edge cracking are reduced, yield is improved, production costs are reduced, and application scope is expanded.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-density tungsten alloy product processing, in particular to a method for improving the processing performance of high-density tungsten alloy. Background Art
[0002] High-density tungsten alloy refers to a typical two-phase alloy with tungsten as the matrix and a small amount of Ni, Co, Mo, Fe, Cu and other elements added into it, and is also called "high-density alloy". Due to the large performance difference between the tungsten matrix and other added elements, and its typical two-phase alloy structure, the processing performance of high-density tungsten alloy is poor. For example, high-density tungsten alloy is generally difficult to cold-roll, or during the cold-rolling process, it is easy to have defects such as cracking and edge cracking, which greatly affects the product yield of high-density tungsten alloy.
[0003] The existing manufacturing method of high-density tungsten alloy generally includes the following process steps: pure tungsten powder is mixed with other added element powders, then pressed or rolled, then liquid-phase sintered to form a sintered billet, then rolled (including hot rolling and cold rolling), and finally heat treated to form a plate or block of the required thickness.
[0004] In the above method, commercially available pure tungsten powder is usually used and mixed with metal powders of other added elements, or a certain proportion of binder is added to modify the powder, and then the subsequent process as described above is carried out to prepare a plate or block of the required thickness.
[0005] The disadvantage of the above method is that it is difficult for pure tungsten powder to form a true metallurgical complete alloy structure with other metal powders of added elements in the subsequent liquid phase sintering process, but a typical two-phase alloy structure. The bonding force between particles is weak, and it is easy to cause cracking and edge cracking of the billet during the subsequent cold rolling process. As a result, the actual yield rate of high-density tungsten alloy materials prepared by the above method is relatively low. In addition, high-density tungsten alloys also have a large work hardening effect, and the actual processing annealing passes are more, so the production cost is high. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects and shortcomings of the prior art and provide a method for improving the processing performance of high-density tungsten alloys, so as to improve the processing performance and product yield of high-density tungsten alloys and reduce production costs.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A method for improving the processing performance of high specific gravity tungsten alloy, characterized in that it specifically comprises the following steps:
[0009] S1. Prepare ammonium paratungstate solution, select two low melting point metal powders, add them into the ammonium paratungstate solution and mix them evenly, dry them after the water evaporates, and obtain mixed powder, wherein the particle size of the low melting point metal powder is 10-50μm;
[0010] S2. Under the conditions of a heating temperature of 900-1050°C, a heating time of 150-240 min, a hydrogen dew point of <40°C, and a hydrogen flow rate of 15-35 L / min, the mixed powder obtained in step S1 is subjected to hydrogen reduction to obtain a pre-alloyed powder having a particle size of 3.5-45 μm, a carbon content of not more than 50 ppm, and an oxygen content of not more than 300 ppm;
[0011] S3. Pressing the pre-alloyed powder obtained in step S2 into a high specific gravity tungsten alloy green body, and then performing liquid phase sintering to obtain a high specific gravity tungsten alloy sintered body;
[0012] S4. rolling the high-density tungsten alloy sintered billet obtained in step S3, and then performing heat treatment to obtain a high-density tungsten alloy plate;
[0013] S5. Process the high-density tungsten alloy plate obtained in step S4 into a high-density tungsten alloy product with specified shape and size.
[0014] In step S1, the mass ratio of the two metal powders to the ammonium paratungstate solution is 10:100-110, and the concentration of the ammonium paratungstate solution is 2.4%-3%.
[0015] Furthermore, in the step S1, the purified water is first heated to 60-80°C, and then the ammonium paratungstate particles are added to the purified water at a mass ratio of purified water to ammonium paratungstate particles of 1000:25-30, and stirred to dissolve, so as to prepare an ammonium paratungstate solution.
[0016] Furthermore, in the step S1, the temperature of the ammonium paratungstate solution is maintained at 60-80°C, and two metal powders are added thereto at an addition rate of 1-1.5 kg / min, and stirred for 30-60 minutes while adding, so that the two metal powders and the ammonium paratungstate solution are evenly mixed to form a mixed solution, and then the temperature of the mixed solution is increased to 100°C, and stirring is continued to gradually evaporate the water in the mixed solution.
[0017] Furthermore, in the step S1, the drying temperature is 100-120° C., and the drying time is 60-120 min.
[0018] Furthermore, in the step S2, the mixed powder is loaded into a molybdenum boat or a stainless steel boat, which is placed in a rotary continuous hydrogen reduction furnace for hydrogen reduction, and the loading capacity of each molybdenum boat or stainless steel boat is 1-2.5 kg.
[0019] Furthermore, in the step S3, the pre-alloyed powder is pressed into a high-density tungsten alloy green billet by a powder rolling process, the rolling pressure is 100-220 kN, and the rolling speed is 1-3 m / min.
[0020] Furthermore, in the step S3, a hydrogen-protected tunnel furnace or a hydrogen-protected box furnace is used to perform liquid phase sintering on the high-density tungsten alloy green body pressed in the step S5, the sintering temperature is 1300-1600° C., and the sintering time is 2-5 hours.
[0021] Furthermore, in the step S4, the high specific gravity tungsten alloy sintered billet is rolled by cold rolling process, the rolling pressure is 45-80 T, and the rolling speed is 15-45 m / min.
[0022] Furthermore, in the step S4, a hydrogen protection furnace is used to heat treat the high specific gravity tungsten alloy plate, the heat treatment temperature is 600-950° C., the heat treatment time is 90-240 min, and the hydrogen flow rate is 10-25 L / min.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention adopts ammonium paratungstate solution to replace pure tungsten powder, mixes it with other low-melting-point metal powders, and then prepares micron-level mixed pre-alloy powders in the powder particle level range of 3.5-45μm by hydrogen reduction, and at the same time controls the carbon content of the pre-alloy powder to be ≤50ppm and the oxygen content to be ≤300ppm. After powder batching, rolling molding, and liquid phase sintering, a high-density tungsten alloy sintered blank is obtained, forming a two-phase alloy structure in the micron level range. The obtained sintered blank has better toughness and sufficient strength, thereby greatly improving the subsequent processing performance of the high-density tungsten alloy product, greatly reducing the proportion of cracking and edge cracking, and improving the material yield; at the same time, due to the technical measures for controlling the carbon content and oxygen content in the pre-alloy powder, the processing hardening performance of the high-density tungsten alloy product is improved to a certain extent, the processing passes are reduced, and the production cost is reduced.
[0025] 2. The high specific gravity tungsten alloy applicable to the present invention has a wider application range.
[0026] 3. The material yield rate of the high-density tungsten alloy products prepared by the method of the present invention is increased by 20-40% compared with the conventional method, and the thinner the thickness of the high-density tungsten alloy plate produced, the more obvious the effect of improving the yield rate. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0028] A method for improving the processing performance of high specific gravity tungsten alloy, specifically comprising the following steps:
[0029] S1. Prepare an ammonium paratungstate solution, then select 50kg Ni powder and 50kg Fe powder with a particle size of 10μm, add them to 1000kg ammonium paratungstate solution, mix them evenly, and dry them after the water evaporates to obtain a WNiFe mixed powder with a tungsten content of 13.5%. In this embodiment, the method for preparing the ammonium paratungstate solution is as follows: first, heat pure water to 60°C, then add ammonium paratungstate particles to the pure water at a mass ratio of pure water to ammonium paratungstate particles of 1000:25, and stir and dissolve them to prepare an ammonium paratungstate solution.
[0030] It should be noted that when adding Ni powder and Fe powder to the ammonium paratungstate solution, the temperature of the ammonium paratungstate solution is maintained at 60°C, and Ni powder and Fe powder are added thereto at a rate of 1 kg / min, and stirring is performed for 60 minutes while adding, so that the Ni powder and Fe powder are evenly mixed with the ammonium paratungstate solution to form a mixed solution, and then the temperature of the mixed solution is increased to 100°C, and stirring is continued to gradually evaporate the water in the mixed solution.
[0031] In addition, during drying, the drying temperature is 100° C. and the drying time is 120 min.
[0032] S2. Under the conditions of a heating temperature of 900°C, a heating time of 240 min, a hydrogen dew point of 20°C, and a hydrogen flow rate of 15 L / min, the WNiFe mixed powder obtained in step S1 is subjected to hydrogen reduction to obtain a pre-alloyed powder having a particle size of 3.5 μm, a carbon content of 25 ppm, and an oxygen content of 35 ppm.
[0033] Specifically, the WNiFe mixed powder is loaded into a molybdenum boat, which is placed in a rotary continuous hydrogen reduction furnace for hydrogen reduction. The loading capacity of each molybdenum boat is 12.5 kg.
[0034] S3. Pressing the pre-alloyed powder obtained in step S2 into a high specific gravity tungsten alloy green body, and then performing liquid phase sintering to obtain a high specific gravity tungsten alloy sintered body.
[0035] Specifically, the pre-alloyed powder was pressed into a high-density tungsten alloy green billet using a powder rolling process, with a rolling pressure of 100 kN and a rolling speed of 3 m / min.
[0036] In addition, a hydrogen-protected tunnel furnace is used to perform liquid phase sintering on the high-density tungsten alloy green body pressed in step S5, with a sintering temperature of 1300° C. and a sintering time of 5 hours.
[0037] S4. The high specific gravity tungsten alloy sintered blank obtained in step S3 is rolled and then heat treated to obtain a tungsten alloy plate having a tungsten content of 13.5%.
[0038] Specifically, the high specific gravity tungsten alloy sintered billet is rolled by cold rolling process, with a rolling pressure of 45 T and a rolling speed of 45 m / min.
[0039] In addition, a hydrogen protection furnace was used to heat treat the high specific gravity tungsten alloy plate. The heat treatment temperature was 600°C, the heat treatment time was 240 min, and the hydrogen flow rate was 10 L / min.
[0040] S5. Process the high-density tungsten alloy plate obtained in step S4 into a high-density tungsten alloy product with specified shape and size. Example 2
[0041] A method for improving the processing performance of high specific gravity tungsten alloy, specifically comprising the following steps:
[0042] S1. Prepare ammonium paratungstate solution, then select 50kg Ni powder and 50kg Fe powder with a particle size of 20μm and add them to 1040kg ammonium paratungstate solution, mix them evenly, and dry them after the water evaporates to obtain WNiFe mixed powder with a tungsten content of 14.6%.
[0043] In this embodiment, the method for preparing the ammonium paratungstate solution is as follows: first, pure water is heated to 65° C., and then the ammonium paratungstate particles are added to the pure water at a mass ratio of pure water to ammonium paratungstate particles of 1000:26, and stirred to dissolve, thereby preparing the ammonium paratungstate solution.
[0044] It should be noted that when adding Ni powder and Fe powder to the ammonium paratungstate solution, the temperature of the ammonium paratungstate solution was maintained at 65°C, and Ni powder and Fe powder were added thereto at a rate of 1.2 kg / min, and stirred for 40 minutes while adding, so that the Ni powder and Fe powder were evenly mixed with the ammonium paratungstate solution to form a mixed solution, and then the temperature of the mixed solution was increased to 100°C, and stirring was continued to gradually evaporate the water in the mixed solution.
[0045] In addition, during drying, the drying temperature is 110° C. and the drying time is 100 min.
[0046] S2. Under the conditions of a heating temperature of 960°C, a heating time of 180 min, a hydrogen dew point of 25°C, and a hydrogen flow rate of 20 L / min, the WNiFe mixed powder obtained in step S1 is subjected to hydrogen reduction to obtain a pre-alloyed powder with a particle size of 10 μm, a carbon content of 30 ppm, and an oxygen content of 40 ppm.
[0047] Specifically, the WNiFe mixed powder is loaded into a molybdenum boat, which is placed in a rotary continuous hydrogen reduction furnace for hydrogen reduction. The loading capacity of each molybdenum boat is 1.5 kg.
[0048] S3. Pressing the pre-alloyed powder obtained in step S2 into a high specific gravity tungsten alloy green body, and then performing liquid phase sintering to obtain a high specific gravity tungsten alloy sintered body.
[0049] Specifically, the pre-alloyed powder was pressed into a high-density tungsten alloy green billet using a powder rolling process, with a rolling pressure of 150 kN and a rolling speed of 2 m / min.
[0050] In addition, a hydrogen-protected tunnel furnace is used to perform liquid phase sintering on the high-density tungsten alloy green body pressed in step S5, with a sintering temperature of 1400° C. and a sintering time of 4 hours.
[0051] S4. The high-density tungsten alloy sintered blank obtained in step S3 is rolled and then heat-treated to obtain a high-density tungsten alloy plate.
[0052] Specifically, the high specific gravity tungsten alloy sintered billet is rolled by cold rolling process, with a rolling pressure of 60 T and a rolling speed of 30 m / min.
[0053] In addition, a hydrogen protection furnace was used to heat treat the high specific gravity tungsten alloy plate. The heat treatment temperature was 700°C, the heat treatment time was 200 min, and the hydrogen flow rate was 15 L / min.
[0054] S5. Process the high-density tungsten alloy plate obtained in step S4 into a high-density tungsten alloy product with specified shape and size. Example 3
[0055] A method for improving the processing performance of high specific gravity tungsten alloy, specifically comprising the following steps:
[0056] S1. Prepare ammonium paratungstate solution, then select 50kg Ni powder and 50kg Cu powder with a particle size of 30μm and add them to 1080kg ammonium paratungstate solution, mix them evenly, and dry them after the water evaporates to obtain WNiCu mixed powder with a tungsten content of 16%.
[0057] In this embodiment, the method for preparing the ammonium paratungstate solution is as follows: firstly, pure water is heated to 70°C, and then the ammonium paratungstate particles are added to the pure water at a mass ratio of pure water to ammonium paratungstate particles of 1000:28, and stirred to dissolve to prepare the ammonium paratungstate solution.
[0058] It should be noted that when adding Ni powder and Cu powder to the ammonium paratungstate solution, the temperature of the ammonium paratungstate solution was maintained at 70°C, and Ni powder and Cu powder were added thereto at a rate of 1.4 kg / min, and stirred for 50 minutes while adding, so that the Ni powder and Cu powder were evenly mixed with the ammonium paratungstate solution to form a mixed solution, and then the temperature of the mixed solution was increased to 100°C, and stirring was continued to gradually evaporate the water in the mixed solution.
[0059] In addition, during drying, the drying temperature is 115° C. and the drying time is 80 min.
[0060] S2. Under the conditions of a heating temperature of 1000°C, a heating time of 180 min, a hydrogen dew point of 30°C, and a hydrogen flow rate of 30 L / min, the WNiCu mixed powder obtained in step S1 is subjected to hydrogen reduction to obtain a pre-alloyed powder with a particle size of 30 μm, a carbon content of 35 ppm, and an oxygen content of 45 ppm.
[0061] Specifically, the WNiCu mixed powder is loaded into a stainless steel boat, which is placed in a rotary continuous hydrogen reduction furnace for hydrogen reduction, and the loading capacity of each stainless steel boat is 2 kg.
[0062] S3. Pressing the pre-alloyed powder obtained in step S2 into a high specific gravity tungsten alloy green body, and then performing liquid phase sintering to obtain a high specific gravity tungsten alloy sintered body.
[0063] Specifically, the pre-alloyed powder is pressed into a high-density tungsten alloy green billet by a powder rolling process, with a rolling pressure of 200 kN and a rolling speed of 1.5 m / min.
[0064] In addition, a hydrogen-protected box furnace is used to perform liquid phase sintering on the high-density tungsten alloy green body pressed in step S5, with a sintering temperature of 1500° C. and a sintering time of 3 hours.
[0065] S4. The high-density tungsten alloy sintered blank obtained in step S3 is rolled and then heat-treated to obtain a high-density tungsten alloy plate.
[0066] Specifically, the high specific gravity tungsten alloy sintered billet is rolled by cold rolling process, the rolling pressure is 70T, and the rolling speed is 20 m / min.
[0067] In addition, a hydrogen protection furnace was used to heat treat the high specific gravity tungsten alloy plate. The heat treatment temperature was 800°C, the heat treatment time was 120 minutes, and the hydrogen flow rate was 20L / min.
[0068] S5. Process the high-density tungsten alloy plate obtained in step S4 into a high-density tungsten alloy product with specified shape and size. Example 4
[0069] A method for improving the processing performance of high specific gravity tungsten alloy, specifically comprising the following steps:
[0070] S1. Prepare ammonium paratungstate solution, then select 50kg Ni powder and 50kg Cu powder with a particle size of 50μm and add them to 1100kg ammonium paratungstate solution, mix them evenly, and dry them after the water evaporates to obtain WNiCu mixed powder with a tungsten content of 17.2%.
[0071] In this embodiment, the method for preparing the ammonium paratungstate solution is as follows: firstly, pure water is heated to 80°C, and then the ammonium paratungstate particles are added to the pure water at a mass ratio of pure water to ammonium paratungstate particles of 1000:30, and stirred to dissolve to prepare the ammonium paratungstate solution.
[0072] It should be noted that when adding Ni powder and Cu powder to the ammonium paratungstate solution, the temperature of the ammonium paratungstate solution is maintained at 80°C, and Ni powder and Cu powder are added thereto at a rate of 1 kg / min, and stirring is performed for 30 minutes while adding, so that the Ni powder and Cu powder are evenly mixed with the ammonium paratungstate solution to form a mixed solution, and then the temperature of the mixed solution is increased to 100°C, and stirring is continued to gradually evaporate the water in the mixed solution.
[0073] In addition, during drying, the drying temperature is 120° C. and the drying time is 60 min.
[0074] S2. Under the conditions of a heating temperature of 1050°C, a heating time of 150 min, a hydrogen dew point of 35°C, and a hydrogen flow rate of 35 L / min, the WNiCu mixed powder obtained in step S1 is subjected to hydrogen reduction to obtain a pre-alloyed powder with a particle size of 45 μm, a carbon content of 40 ppm, and an oxygen content of 65 ppm.
[0075] Specifically, the WNiCu mixed powder is loaded into a stainless steel boat, and placed into a rotary continuous hydrogen reduction furnace for hydrogen reduction. The loading capacity of each stainless steel boat is 2.5 kg.
[0076] S3. Pressing the pre-alloyed powder obtained in step S2 into a high specific gravity tungsten alloy green body, and then performing liquid phase sintering to obtain a high specific gravity tungsten alloy sintered body.
[0077] Specifically, the pre-alloyed powder was pressed into a high-density tungsten alloy green billet using a powder rolling process, with a rolling pressure of 220 kN and a rolling speed of 1 m / min.
[0078] In addition, a hydrogen-protected box furnace is used to perform liquid phase sintering on the high-density tungsten alloy green body pressed in step S5, with a sintering temperature of 1600° C. and a sintering time of 2 h.
[0079] S4. The high-density tungsten alloy sintered blank obtained in step S3 is rolled and then heat-treated to obtain a high-density tungsten alloy plate.
[0080] Specifically, the high specific gravity tungsten alloy sintered billet is rolled by cold rolling process, the rolling pressure is 80 T, and the rolling speed is 15m / min.
[0081] In addition, a hydrogen protection furnace was used to heat treat the high specific gravity tungsten alloy plate. The heat treatment temperature was 950°C, the heat treatment time was 90 min, and the hydrogen flow rate was 25 L / min.
[0082] S5. Process the high-density tungsten alloy plate obtained in step S4 into a high-density tungsten alloy product with specified shape and size.
[0083] Comparative Example
[0084] A method for preparing a high-density tungsten alloy plate with a tungsten content of 16%, comprising the following steps:
[0085] S1. Weigh 1.9kg tungsten powder, 7kg nickel powder and 3kg iron powder into a mixer and mix for 4h-8h.
[0086] S2 weighed 10g of organic binder was added to 1000ml of water and mixed for 3h to obtain an aqueous binder solution,
[0087] S3. The dry-mixed powder obtained in step S1 is mixed with the binder aqueous solution, heated in a water bath at 80-100°C, and stirred for 1h-1.5h to obtain a loose powder.
[0088] S4. The above powder is sieved and dried to obtain mixed tungsten alloy powder.
[0089] S5. Press the above tungsten alloy powder and sinter it at 1100-1200℃ to obtain a sintered blank of corresponding thickness.
[0090] S6. After the sintered billet is rolled and heat treated, a tungsten alloy sheet of corresponding thickness is obtained. The tungsten alloy sintered billet is rolled using a cold rolling process. The rolling pressure is 80-90 T and the rolling speed is 10-15m / min.
[0091] S7. Finally, a hydrogen protection furnace is used to heat treat the high specific gravity tungsten alloy plate. The heat treatment temperature is 950°C, the heat treatment time is 90 min, and the hydrogen flow rate is 25 L / min.
[0092] The tungsten alloy plates obtained in Examples 1, 2, 3, 4 and the comparative example were further processed into plates with a size (mm) of 0.2*110*300, and then the technical performance tests were performed on them, and the yield rate and rolling passes were compared. The results are shown in Table 1.
[0093] Table 1
[0094] Compare Projects Carbon content Oxygen content Thickness difference Edge cracking Yield Number of rolling passes Example 1 ≦35ppm ≦45ppm Thickness difference of the same plate is 0.005mm No cracking 77% 2 times Example 2 ≦30ppm ≦44ppm Thickness difference of the same plate is 0.005mm No cracking 74% 2 times Example 3 ≦32ppm ≦52ppm Thickness difference of the same plate is 0.005mm No cracking 75% 2 times Example 4 ≦25ppm ≦60ppm Thickness difference of the same plate is 0.005mm No cracking 76% 2 times Comparative Example About 130ppm About 900ppm Thickness difference of the same plate is 0.01mm Edge cracking 5-8mm 40-55% 5-7 times
[0095] As can be seen from Table 1, the present invention adopts ammonium paratungstate solution to replace pure tungsten powder, mixes it with other low-melting-point metal powders, and then prepares pre-alloyed powders of micron level mixed with each other in the powder particle level range of 3.5-45μm by hydrogen reduction, and at the same time controls the carbon content of the pre-alloyed powder to be ≤50ppm and the oxygen content to be ≤300ppm. After powder batching, rolling molding, and liquid phase sintering, a high-density tungsten alloy sintered blank is obtained, and a two-phase alloy structure in the micron level range is formed. The obtained sintered blank has better toughness and sufficient strength, and the thickness difference of the product, that is, the maximum thickness deviation, can reach 0.005mm, thereby greatly improving the subsequent processing performance of the high-density tungsten alloy product, greatly reducing the proportion of cracking and edge cracking, and the surface is flat and smooth, without cracks, holes, black spots, dirt and other appearance problems.
[0096] At the same time, it can be seen from Table 1 that the product prepared by the present invention has a yield rate of more than 70%, and can reach 77% at most; and, due to the technical measures of controlling the carbon content and oxygen content in the pre-alloyed powder, the processing hardening performance of the high-density tungsten alloy product is improved to a certain extent, the processing passes are reduced, and the production cost is reduced. It only takes about 2 weeks from feeding to producing the finished product.
[0097] The product yield rate of conventional powder metallurgy process can only reach 55% at most, and the production cycle is at least more than 4 weeks.
[0098] Therefore, the yield rate of the high-density tungsten alloy products prepared by the method of the present invention is improved by 20-40% compared with the conventional powder metallurgy process, and the thinner the thickness of the produced high-density tungsten alloy plate, the more obvious the effect of improving the yield rate.
[0099] Although this specification is described according to implementation modes, not every implementation mode includes only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
[0100] Therefore, the above description is only a preferred embodiment of the present application and is not intended to limit the scope of implementation of the present application; that is, all equivalent changes made according to the scope of the claims of the present application are within the protection scope of the claims of the present application.
Claims
1. A method for improving the processing performance of high specific gravity tungsten alloy, characterized by: The specific steps include: S1. Prepare ammonium paratungstate solution, select two low melting point metal powders, add them into the ammonium paratungstate solution and mix them evenly, dry them after the water evaporates, and obtain mixed powder, wherein the particle size of the low melting point metal powder is 10-50μm; S2. Under the conditions of a heating temperature of 900-1050°C, a heating time of 150-240 min, a hydrogen dew point of less than 40°C, and a hydrogen flow rate of 15-35 L / min, the mixed powder obtained in step S1 is subjected to hydrogen reduction to obtain a pre-alloyed powder having a particle size of 3.5-45 μm, a carbon content of not more than 50 ppm, and an oxygen content of not more than 300 ppm; S3. Pressing the pre-alloyed powder obtained in step S2 into a high specific gravity tungsten alloy green body, and then performing liquid phase sintering to obtain a high specific gravity tungsten alloy sintered body; S4. rolling the high-density tungsten alloy sintered billet obtained in step S3, and then performing heat treatment to obtain a high-density tungsten alloy plate; S5. Process the high-density tungsten alloy plate obtained in step S4 into a high-density tungsten alloy product with specified shape and size. In step S1, the mass ratio of the two low melting point metal powders to the ammonium paratungstate solution is 10:100-110, and the concentration of the ammonium paratungstate solution is 2.4%-3%.
2. A method for improving the processing performance of high specific gravity tungsten alloy according to claim 1, characterized in that: In the step S1, the purified water is first heated to 60-80°C, and then the ammonium paratungstate particles are added to the purified water at a mass ratio of purified water to ammonium paratungstate particles of 1000:25-30, and stirred to dissolve, so as to prepare an ammonium paratungstate solution.
3. A method for improving the processing performance of high specific gravity tungsten alloy according to claim 1, characterized in that: In the step S1, the temperature of the ammonium paratungstate solution is maintained at 60-80°C, and two metal powders are added thereto at an addition rate of 1-1.5 kg / min, and stirred for 30-60 minutes while adding, so that the two metal powders and the ammonium paratungstate solution are evenly mixed to form a mixed solution, and then the temperature of the mixed solution is increased to 100°C, and stirring is continued to gradually evaporate the water in the mixed solution.
4. A method for improving the processing performance of high specific gravity tungsten alloy according to claim 1, characterized in that: In the step S1, the drying temperature is 100-120° C. and the drying time is 60-120 min.
5. A method for improving the processing performance of high specific gravity tungsten alloy according to claim 1, characterized in that: In the step S2, the mixed powder is loaded into a molybdenum boat or a stainless steel boat, which is placed in a rotary continuous hydrogen reduction furnace for hydrogen reduction. The loading capacity of each molybdenum boat or stainless steel boat is 1-2.5 kg.
6. A method for improving the processing performance of high specific gravity tungsten alloy according to claim 1, characterized in that: In the step S3, the pre-alloyed powder is pressed into a high-density tungsten alloy green billet by a powder rolling process, the rolling pressure is 100-220 kN, and the rolling speed is 1-3 m / min.
7. A method for improving the processing performance of high specific gravity tungsten alloy according to claim 1, characterized in that: In the step S3, a hydrogen-protected tunnel furnace or a hydrogen-protected box furnace is used to liquid-phase sinter the high-density tungsten alloy green body pressed in step S5, the sintering temperature is 1300-1600° C., and the sintering time is 2-5 hours.
8. A method for improving the processing performance of high specific gravity tungsten alloy according to claim 1, characterized in that: In the step S4, the high specific gravity tungsten alloy sintered billet is rolled by cold rolling process, the rolling pressure is 45-80 T, and the rolling speed is 15-45 m / min.
9. A method for improving the processing performance of high specific gravity tungsten alloy according to claim 1, characterized in that: In the step S4, a hydrogen protection furnace is used to heat treat the high specific gravity tungsten alloy plate, the heat treatment temperature is 600-950°C, the heat treatment time is 90-240min, and the hydrogen flow rate is 10-25 L / min.
10. The method for improving the processing performance of high specific gravity tungsten alloy according to claim 1, characterized in that: The low melting point metal powder is selected from two of Ni powder, Fe powder and Cu powder.