A corona-resistant enameled wire and a preparation method thereof

By combining modified polyimide and montmorillonite with epoxy resin, the corona and heat insulation properties of the paint film are enhanced, and the existing enameled wires are easily insulating and damaged under high-frequency pulse voltage and poor adhesion under high-temperature environments are solved. The problem has achieved higher corona resistance and heat insulation, and is suitable for harsh environments of frequency converter motors in new energy vehicles.

CN118629707BActive Publication Date: 2024-11-01XUANCHENG HONGTONG ELECTRICAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411090219.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-01
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Existing enameled wires are prone to insulating damage under high-frequency pulse voltages, and polyimide enameled wires have poor adhesion and insufficient corona resistance in high-temperature, high-speed, heavy-duty environments, making them difficult to be suitable for the harsh conditions of frequency converter motors of new energy vehicles. .

Method used

Modified polyimide and modified montmorillonite are combined with epoxy resin, and nano-alumina composite filler and modified montmorillonite are prepared through chemical reactions and sol-gel method to enhance the corona resistance and isolation of the paint film. Thermal and adhesion properties, improve elongation and breakdown voltage.

Benefits of technology

It significantly improves the high temperature, heat insulation, scratch resistance and corona resistance of enameled wire, extends its service life, and enhances performance stability in high temperature and corrosion environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a field of enameled wire, and discloses a corona-resistant enameled wire and a preparation method thereof. The corona-resistant enameled wire comprises a conductor core material and an enameled wire varnish coated on the conductor core material, wherein the enameled wire varnish comprises the following components in parts by weight: 40-50 parts of modified polyimide, 5-10 parts of epoxy resin, 2-5 parts of modified montmorillonite, and 10-20 parts of a solvent. The modified polyimide is prepared by grafting a silicon dioxide-coated nano-alumina composite filler with polyimide by chemical reaction. The modified montmorillonite is prepared by grafting a flame retardant after co-modifying montmorillonite with γ-aminopropyltriethoxysilane and γ-methacryloxypropyltrimethoxysilane. The invention provides the enameled wire with excellent high temperature resistance and heat insulation effect by adding modified polyimide, epoxy resin and modified montmorillonite, and has good corona resistance, scratch resistance and adhesion, and at the same time, the elongation and breakdown voltage are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of enameled wires, and in particular relates to a corona-resistant enameled wire and a preparation method thereof. Background Art

[0002] At present, new energy vehicles are developing rapidly. The core component of new energy vehicles is the variable frequency drive motor. The strong partial discharge generated by the insulating enameled wire between the turns of the motor winding under the action of high-frequency pulse voltage is currently the main cause of insulation damage in the variable frequency motor. The rapid reversal of the pulse voltage of the variable frequency drive motor forms a strong reverse electric field superposition on the surface of the electromagnetic wire, and at the same time there is a tangential electric field, which makes the space charge gradually penetrate inside the medium, resulting in aging of the polymer insulation layer. In order to adapt to the requirements of high instantaneous power, high power density, variable speed working conditions, strong overload capacity and large starting torque, higher requirements are put forward for the corona resistance of the enameled wire. The corona resistance of the enameled wire is determined by the corona resistance of the insulating layer material. Improving the corona resistance of the insulating layer material is the key to solving the technical problems of the variable frequency motor.

[0003] Enameled wire is a main type of winding wire, which consists of a metal wire core and an insulating enameled layer. The bare wire is annealed and softened, then painted and baked several times. Enameled wire is widely used in motors, transformers, generators, electronic equipment and other fields. At present, the types of enameled wire paint films mainly include polyurethane, polyester, polyimide, polyamide-imide and composite coating enameled wire paint. Among them, polyimide enameled wire paint is the insulating paint with the highest temperature resistance grade among the enameled wires. The long-term use temperature can reach above 220°C. However, pure polyimide has high brittleness, insufficient tensile and compressive strength, and high friction coefficient and wear rate. Therefore, it is difficult to be used in harsh environments such as high temperature, high speed and heavy load. In addition, polyimide enameled wire paint has poor adhesion to copper conductors. Poor adhesion will cause the enameled wire to peel off during use, limiting the application of enameled wire in actual production. Moreover, with the development of technology, the use environment of polyimide enameled wire is becoming more and more harsh, especially under high temperature conditions. Although polyamide-imide is not easy to soften, it has a high dielectric constant and is prone to form charge channels for breakdown. Summary of the invention

[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a corona resistant enameled wire and a preparation method thereof. By adding modified polyimide, epoxy resin and modified montmorillonite, the enameled wire is given excellent high temperature resistance and heat insulation effect, and has good corona resistance, scratch resistance and adhesion performance, while the elongation and breakdown voltage are improved.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A corona-resistant enameled wire comprises a conductor core material and an enameled wire enamel coated on the conductor core material, wherein the enameled wire enamel comprises the following components in parts by weight: 40 to 50 parts of modified polyimide, 5 to 10 parts of epoxy resin, 2 to 5 parts of modified montmorillonite, and 10 to 20 parts of a solvent;

[0007] The modified polyimide is prepared by grafting a silicon dioxide-coated nano-alumina composite filler with polyimide by chemical reaction; the modified montmorillonite is prepared by co-modifying montmorillonite with γ-aminopropyltriethoxysilane and γ-methacryloxypropyltrimethoxysilane and then grafting 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.

[0008] Preferably, the co-solvent is one or more combinations of N,N-dimethylacetamide, N-methylpyrrolidone, N,N-dimethylformamide, ethanol, toluene and acetone.

[0009] Preferably, the preparation method of the modified polyimide comprises the following steps:

[0010] A. Dissolve 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl in a reactor containing N-methylpyrrolidone, add 3,5-diaminobenzoic acid, stir and disperse for 40-60 min under a nitrogen atmosphere, then add 4,4'-biphenyl ether dianhydride in an ice-water bath to react for 10-12 h. After the reaction is completed, heat to 110-125°C for 1-2 h, 140-155°C for 1-2 h, and 190-205°C for 10-12 h to obtain a carboxylated polyimide;

[0011] B. Ultrasonic dispersion of silica-coated nano-alumina composite filler in a mixed solution of ethanol and deionized water, adding γ-aminopropyltriethoxysilane and triethylamine under a nitrogen atmosphere, and reflux reaction at 70-90° C. for 5-8 hours. After the reaction is completed, the mixture is filtered, washed, and dried to obtain an amino composite filler;

[0012] C. Ultrasonic dispersion of the amino composite filler in N-methylpyrrolidone, addition of N-hydroxysuccinimide and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stirring and dissolving at room temperature, and then adding carboxylated polyimide to react for 8-12 hours to obtain modified polyimide.

[0013] Preferably, in step A, the molar ratio of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,5-diaminobenzoic acid and 4,4'-biphenyl ether dianhydride is 1:1-1.2:2-2.2.

[0014] Preferably, in step C, the addition ratio of the amino composite filler and the carboxylated polyimide is 0.2-0.4 g: 80-100 mL.

[0015] Preferably, the method for preparing the silica-coated nano-alumina composite filler in step B comprises the following steps:

[0016] B1. Place isopropanol and deionized water in a reactor, add aluminum isopropoxide at 70-90°C, stir and disperse for 2-4 hours, then remove water and isopropanol in the system by vacuum distillation, dry the obtained product, and calcine at 600-750°C for 8-12 hours to obtain nano-alumina;

[0017] B2. Take nano-alumina, ethanol and deionized water in a reactor, add ammonia water to adjust the pH value of the system to 10-12, and place it in a water bath at 25-30℃ for constant temperature heating for 40-70min after ultrasonic dispersion. Take tetraethyl silicate and dissolve it in a mixed solution of ethanol and deionized water, mix it evenly, let it stand for 20-30min, and then add it to the reactor. Continue to react for 18-24h. After the reaction is completed, centrifuge, wash and dry it to obtain a silica-coated nano-alumina composite filler.

[0018] Preferably, in step B1, the molar ratio of aluminum isopropoxide to deionized water is 1:3-5.

[0019] Preferably, the preparation method of the modified montmorillonite comprises the following steps:

[0020] A. Ultrasonic dispersion of montmorillonite in a mixed solution of ethanol and deionized water, adding γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane and triethylamine, reacting at 50-70°C for 4-8h, filtering, washing and drying after the reaction to obtain activated montmorillonite;

[0021] B. Take 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and activated montmorillonite in a reactor, add deionized water for ultrasonic dispersion, place it at 90-120°C for reflux reaction for 5-7 hours, and after the reaction is completed, filter, wash and dry to obtain modified montmorillonite.

[0022] Preferably, in step B, the mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to activated montmorillonite is 1:2-4.

[0023] The method for preparing the corona-resistant enameled wire as described above comprises the following steps:

[0024] S1. Weigh each component by weight, mix the modified polyimide, epoxy resin, modified montmorillonite and co-solvent at 120-140° C. to obtain a wire enamel;

[0025] S2. Apply the obtained wire enamel on the surface of the conductor core material and then cure it to obtain a corona-resistant enameled wire.

[0026] Beneficial effects of the present invention:

[0027] The invention first synthesizes a carboxylated polyimide based on the structure of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,5-diaminobenzoic acid and 4,4'-biphenyl ether dianhydride. The flexible ether bond and the presence of trifluoromethyl can reduce the rigidity of the chain and weaken the interaction between the chains. The introduction of 3,5-diaminobenzoic acid breaks the symmetry of the polymer chain, provides good solubility and introduces a carboxyl group. At the same time, the invention adopts a sol-gel method to prepare a silica-coated nano-alumina composite filler. The surface of the nano-alumina is coated with an amorphous silica shell layer, which has excellent heat resistance and can be used as a medium to transfer and absorb heat, thereby preventing the occurrence of a heat concentration effect of a paint film. In addition, the invention uses γ-aminopropyltriethoxysilane as a bridging agent to graft the carboxylated polyimide to prepare a modified polyimide. After the silica-coated nano-alumina composite filler is modified by γ-aminopropyltriethoxysilane, a large number of hydroxyl groups on the particle surface react chemically with the active groups formed after the hydrolysis of γ-aminopropyltriethoxysilane, which reduces the surface force, inhibits the agglomeration phenomenon, and has better dispersion in the matrix, which can effectively prevent the extension of microcracks and prevent the reduction of mechanical properties of the paint film due to crack development. It can also effectively buffer part of the energy and improve the toughness of the paint film. The addition of modified polyimide gives the paint film excellent mechanical properties and heat resistance. At the same time, silica and nano-alumina can be used as corona-resistant fillers to give the paint film excellent corona resistance.

[0028] The present invention utilizes gamma-aminopropyltriethoxysilane and gamma-methacryloxypropyltrimethoxysilane to jointly modify montmorillonite, so that double bond groups and amino groups are grafted onto the surface of montmorillonite, and at the same time, the PH bond in the structure of the flame retardant 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide reacts with the double bond on the surface of the modified montmorillonite, thereby modifying the flame retardant on the surface of the montmorillonite, which can achieve a good flame retardant effect and has no migration and seepage problems, thereby ensuring that the paint film achieves a long-term flame retardant effect, and at the same time is conducive to the dispersion of the montmorillonite and avoids the generation of The agglomeration phenomenon leads to a decrease in its performance. In addition, the amino group on the surface of the modified montmorillonite can undergo a ring-opening reaction with the epoxy resin to enhance the interface bonding ability. The added epoxy resin has excellent adhesion, electrical insulation, mechanical properties and corrosion resistance. Montmorillonite has high thermal stability and excellent barrier properties, and excellent mechanical properties. Montmorillonite forms a large-area protective layer with its flaky shape, which can isolate the infiltration of corrosive media, achieve the effect of protecting the paint film, enhance the thermal insulation performance of the paint film, and at the same time improve the cooling and thermal insulation performance of the paint film in a corrosive environment. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1 A method for preparing a modified polyimide comprises the following steps:

[0031] A. Take 4.8g of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl and dissolve it in a reactor containing 100mL of N-methylpyrrolidone, add 2.3g of 3,5-diaminobenzoic acid, stir and disperse for 60min under nitrogen atmosphere, then add 9.5g of 4,4'-biphenyl ether dianhydride in an ice-water bath and react for 12h. After the reaction is completed, heat the mixture to 120℃ for 2h, 145℃ for 2h, and 195℃ for 12h to obtain carboxylated polyimide;

[0032] B. 1.6 g of silica-coated nano-alumina composite filler was ultrasonically dispersed in a mixed solution of 25 mL of ethanol and 25 mL of deionized water, and 2.1 g of γ-aminopropyltriethoxysilane and 0.5 g of triethylamine were added under a nitrogen atmosphere, and the mixture was refluxed at 85° C. for 6 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain an amino composite filler;

[0033] C. Take 0.3 g of amino composite filler and ultrasonically disperse it in 100 mL of N-methylpyrrolidone, add 1.5 g of N-hydroxysuccinimide and 1.8 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stir and dissolve at room temperature, then add 80 mL of carboxylated polyimide and react for 12 hours to obtain modified polyimide.

[0034] The preparation method of the silica-coated nano-alumina composite filler comprises the following steps:

[0035] B1. Take 45 mL of isopropanol and 7 mL of deionized water in a reactor, add 20.4 g of aluminum isopropoxide at 85°C, stir and disperse for 2 hours, then remove the water and isopropanol in the system by vacuum distillation, dry the obtained product and calcine it at 700°C for 10 hours to obtain nano alumina;

[0036] B2. Take 2g of nano-alumina, 25mL of ethanol and 25mL of deionized water in a reactor, add ammonia water to adjust the pH value of the system to 11, and place it in a 25°C water bath for constant temperature heating for 60min after ultrasonic dispersion. Take 9.5mL of tetraethyl silicate and dissolve it in a mixed solution of 20mL of ethanol and 5mL of deionized water. After mixing evenly and standing for 30min, add it to the reactor and continue the reaction for 24h. After the reaction is completed, centrifuge, wash and dry to obtain a silica-coated nano-alumina composite filler.

[0037] Example 2 A method for preparing modified montmorillonite comprises the following steps:

[0038] A. Take 6 g of montmorillonite and ultrasonically disperse it in a mixed solution of 75 mL of ethanol and 75 mL of deionized water, add 1.55 g of γ-aminopropyltriethoxysilane, 1.03 g of γ-methacryloxypropyltrimethoxysilane and 0.002 g of triethylamine, and react at 65 ° C for 7 hours. After the reaction is completed, filter, wash and dry to obtain activated montmorillonite;

[0039] B. Take 3.2g 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 7.1g activated montmorillonite in a reactor, add 200mL deionized water for ultrasonic dispersion, place under reflux reaction at 95°C for 6h, and after the reaction is completed, filter, wash and dry to obtain modified montmorillonite.

[0040] Example 3 A corona-resistant enameled wire comprises a conductor core and a wire enamel coated on the conductor core, wherein the wire enamel comprises the following components in parts by weight: 40 parts of modified polyimide prepared in Example 1, 5 parts of epoxy resin, 2 parts of modified montmorillonite prepared in Example 2, and 10 parts of co-solvent N-methylpyrrolidone.

[0041] The preparation method of the above-mentioned corona resistant enameled wire comprises the following steps:

[0042] S1. Weigh each component by weight, mix the modified polyimide, epoxy resin, modified montmorillonite and co-solvent evenly at 125° C. to obtain a wire enamel;

[0043] S2. Apply the obtained wire enamel on the surface of the conductor core material and then cure it to obtain a corona-resistant enameled wire.

[0044] Example 4 A corona-resistant enameled wire comprises a conductor core and a wire enamel coated on the conductor core, wherein the wire enamel comprises the following components in parts by weight: 44 parts of modified polyimide prepared in Example 1, 7 parts of epoxy resin, 4 parts of modified montmorillonite prepared in Example 2, and 15 parts of co-solvent N-methylpyrrolidone.

[0045] The preparation method of the above-mentioned corona resistant enameled wire is the same as that of Example 3.

[0046] Example 5 A corona-resistant enameled wire comprises a conductor core and a wire enamel coated on the conductor core, wherein the wire enamel comprises the following components in parts by weight: 50 parts of the modified polyimide prepared in Example 1, 10 parts of epoxy resin, 5 parts of the modified montmorillonite prepared in Example 2, and 18 parts of the co-solvent N-methylpyrrolidone.

[0047] The preparation method of the above-mentioned corona resistant enameled wire is the same as that of Example 3.

[0048] Comparative Example 1 A corona-resistant enameled wire comprises a conductor core and a wire enamel coated on the conductor core, wherein the wire enamel comprises the following components in parts by weight: 50 parts of polyimide, 10 parts of epoxy resin, 5 parts of modified montmorillonite prepared in Example 2, and 18 parts of cosolvent N-methylpyrrolidone.

[0049] The preparation method of the above-mentioned corona resistant enameled wire is the same as that of Example 3.

[0050] Comparative Example 2 A corona-resistant enameled wire comprises a conductor core and a wire enamel coated on the conductor core, wherein the wire enamel comprises the following components in parts by weight: 50 parts of the modified polyimide prepared in Example 1, 10 parts of epoxy resin, 5 parts of montmorillonite, and 18 parts of co-solvent N-methylpyrrolidone.

[0051] The preparation method of the above-mentioned corona resistant enameled wire is the same as that of Example 3.

[0052] Performance Testing

[0053] The performance of the enameled wire varnishes and enameled wires prepared in Examples 3-5 and Comparative Examples 1-2 was tested. The conductor core material was a bare copper wire with a diameter of 0.9 mm and the paint film thickness was 0.1 mm:

[0054] a. Use a high-frequency pulse voltage tester to test the corona resistance of the prepared paint film. Paint film test conditions: room temperature, pulse frequency of 20kHz, pulse duty rate of 50%, pulse voltage peak-to-peak value of 2.5kV; use an elongation tensile tester to test the enameled wire for elongation; use an automatic voltage tester to test the breakdown voltage of the enameled wire; use an intelligent unidirectional paint scraping tester to test the enameled wire for scratch resistance; use a quick break tester to test the enameled wire for quick break; use the limiting oxygen index to test the flame retardant performance, and the data results are shown in Table 1.

[0055] b. Wire enameling paint was applied to the surface of the steel plate after sandblasting, and dried and cured at 25°C for 48 hours. The thickness of the dry film was 1mm, and the heat source temperature was 250°C. After a 4-hour heat insulation test, the temperature difference between the heat source and the surface of the coating sample was measured, and the heat insulation performance test was performed; the coating was corroded and immersed in a 50°C, 3.5% NaCl solution for 4 hours, and the temperature difference before and after corrosion was measured. The heat insulation performance test in the corrosive environment was performed, and the data results are shown in Table 1.

[0056] Table 1 Test results of sample performance

[0057]

[0058] It can be seen from the data in Table 1 that the enameled wires prepared in Examples 3-5 of the present invention have excellent high temperature resistance and heat insulation effect, good corona resistance and scratch resistance, high elongation at break, and greatly improved breakdown voltage, which can improve the safety and application range of the prepared enameled wires.

[0059] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0060] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A corona-resistant enameled wire, characterized in that: It comprises a conductor core material and an enameled wire varnish coated on the conductor core material, wherein the enameled wire varnish comprises the following components in parts by weight: 40 to 50 parts of modified polyimide, 5 to 10 parts of epoxy resin, 2 to 5 parts of modified montmorillonite, and 10 to 20 parts of a solvent; The modified polyimide is prepared by grafting a silicon dioxide-coated nano-alumina composite filler with polyimide by chemical reaction; the modified montmorillonite is prepared by co-modifying montmorillonite with γ-aminopropyltriethoxysilane and γ-methacryloxypropyltrimethoxysilane and then grafting 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide; The preparation method of the modified polyimide comprises the following steps: A. Dissolve 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl in a reactor containing N-methylpyrrolidone, add 3,5-diaminobenzoic acid, stir and disperse for 40-60 min under a nitrogen atmosphere, then add 4,4'-biphenyl ether dianhydride in an ice-water bath to react for 10-12 h. After the reaction is completed, heat to 110-125°C for 1-2 h, 140-155°C for 1-2 h, and 190-205°C for 10-12 h to obtain a carboxylated polyimide; B. Ultrasonic dispersion of silica-coated nano-alumina composite filler in a mixed solution of ethanol and deionized water, adding γ-aminopropyltriethoxysilane and triethylamine under a nitrogen atmosphere, and reflux reaction at 70-90° C. for 5-8 hours. After the reaction is completed, the mixture is filtered, washed, and dried to obtain an amino composite filler; C. Ultrasonic dispersion of the amino composite filler in N-methylpyrrolidone, addition of N-hydroxysuccinimide and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stirring and dissolving at room temperature, and then adding carboxylated polyimide to react for 8-12 hours to obtain modified polyimide; The preparation method of the modified montmorillonite comprises the following steps: A. Ultrasonic dispersion of montmorillonite in a mixed solution of ethanol and deionized water, adding γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane and triethylamine, reacting at 50-70°C for 4-8h, filtering, washing and drying after the reaction to obtain activated montmorillonite; B. Take 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and activated montmorillonite in a reactor, add deionized water for ultrasonic dispersion, place it at 90-120°C for reflux reaction for 5-7 hours, and after the reaction is completed, filter, wash and dry to obtain modified montmorillonite.

2. The corona-resistant enameled wire according to claim 1, characterized in that: The co-solvent is one or more combinations of N,N-dimethylacetamide, N-methylpyrrolidone, N,N-dimethylformamide, ethanol, toluene and acetone.

3. The corona-resistant enameled wire according to claim 1, characterized in that: In step A, the molar ratio of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,5-diaminobenzoic acid and 4,4'-biphenyl ether dianhydride is 1:1-1.2:2-2.

2.

4. The corona-resistant enameled wire according to claim 1, characterized in that: In the step C, the addition ratio of the amino composite filler and the carboxylated polyimide is 0.2-0.4 g: 80-100 mL.

5. The corona-resistant enameled wire according to claim 1, characterized in that: The method for preparing the silica-coated nano-alumina composite filler in step B comprises the following steps: B1. Place isopropanol and deionized water in a reactor, add aluminum isopropoxide at 70-90°C, stir and disperse for 2-4 hours, then remove water and isopropanol in the system by vacuum distillation, dry the obtained product, and calcine at 600-750°C for 8-12 hours to obtain nano-alumina; B2. Take nano-alumina, ethanol and deionized water in a reactor, add ammonia water to adjust the pH value of the system to 10-12, and place it in a water bath at 25-30℃ for constant temperature heating for 40-70min after ultrasonic dispersion. Take tetraethyl silicate and dissolve it in a mixed solution of ethanol and deionized water, mix it evenly, let it stand for 20-30min, and then add it to the reactor. Continue to react for 18-24h. After the reaction is completed, centrifuge, wash and dry it to obtain a silica-coated nano-alumina composite filler.

6. The corona-resistant enameled wire according to claim 5, characterized in that: In step B1, the molar ratio of aluminum isopropoxide to deionized water is 1:3-5.

7. The corona-resistant enameled wire according to claim 1, characterized in that: In the step B, the mass ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to activated montmorillonite is 1:2-4.

8. The corona-resistant enameled wire according to any one of claims 1 to 7, characterized in that: The preparation method of the enameled wire comprises the following steps: S1. Weigh each component by weight, mix the modified polyimide, epoxy resin, modified montmorillonite and co-solvent at 120-140° C. to obtain a wire enamel; S2. Apply the obtained wire enamel on the surface of the conductor core material and then cure it to obtain a corona-resistant enameled wire.

Citation Information

Patent Citations

  • Preparation method of special high-impact-resistance polystyrene material for television shell

    CN110577716A

  • Self-adhesive paint, corona-resistant polyimide paint and preparation method thereof

    CN111393949A

  • Ultraviolet crosslinking wear-resistant short-circuit-resistant halogen-free flame-retardant polyolefin material capable of resisting temperature of 125 DEG C and preparation method thereof

    CN115612199A

  • High-temperature-resistant heat dissipation powder coating and preparation method thereof

    CN115710459A

  • Insulated covering material and insulating coating conductor

    JP2006134813A