A process for manufacturing fiber composite pultruded profile surface material

Through the surface material production process of fiber composite pultrusion profiles, technologies such as microfluidics, nano-reinforcement layers and bionic structural design are used to optimize the performance of composite materials, solving the problems of single material performance and insufficient interface bonding strength in traditional processes, and achieving High strength, high toughness and diverse adaptability.

CN118636505BActive Publication Date: 2024-10-25SICHUAN PROVINCIAL ARCHITECTURAL DESIGN & RES INST
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202411103179.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-25
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Traditional composite material manufacturing processes have deficiencies in comprehensive performance, surface functionality, interlayer bonding strength, environmental adaptability and internal stress control, making it difficult to meet a variety of performance requirements and complex application needs.

Method used

The surface material production process of fiber composite pultruded profiles is adopted, and through microfluidic technology, nano-reinforcement layer, bionic structural design, gradient curing process, multi-layer composite impregnation and dynamic cross-linked network structure, combined with multi-phase interface enhancement technology, the resin and Selection and combination of additives, designing bionic structures and multi-layer composite structures, controlling the curing process and cross-linking density.

Benefits of technology

Significantly improve the comprehensive performance, toughness, strength, fire resistance and anti-aging ability of the material, improve the surface functionality and structural performance, enhance the eco-friendliness and application performance of the material, solve the problem of insufficient interface bonding strength and internal stress, The diversified adaptability and stability of materials are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118636505B_ABST
    Figure CN118636505B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of composite materials, and discloses a process for making a surface material of a fiber composite pultruded profile, comprising the following steps: S1, material preparation, selection and pretreatment of fibers and resin materials; S2, passing the fibers through an impregnation tank in a microfluidic device, controlling the resin flow rate of 0.1-0.5 mL / min and the pressure of 0.1-0.5 MPa by microfluidic technology, adjusting the equipment parameters to uniformly impregnate the fibers, preliminarily impregnating in a low-viscosity resin of 100-200 cP, followed by multiple impregnations and curing at 80-100 ° C; S3, selecting appropriate nanomaterials, such as nano-silicon dioxide or graphene. By optimizing resin and additive selection, bionic design, multi-layer composite structure, dynamic cross-linked network and multiphase interface enhancement technology, the problems of insufficient performance of a single resin system, poor surface function and structural optimization, poor interlayer bonding, poor environmental adaptability, low interface bonding strength and performance degradation caused by curing internal stress are solved, and the comprehensive performance and durability of fiber composite materials are significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, in particular to a process for manufacturing a fiber composite pultruded profile surface material. Background Art

[0002] Fiber-reinforced composites are widely used in aerospace, automotive, construction, and sporting goods due to their excellent mechanical properties, lightweight characteristics, and corrosion resistance. These materials are made by combining fibers (such as glass fiber, carbon fiber, and basalt fiber) with resins (such as polyester resin, epoxy resin, and vinyl ester resin), providing higher strength and better durability than traditional materials. However, traditional composite manufacturing processes have significant deficiencies in many aspects, limiting their scope of application and service life.

[0003] First, the use of a single resin system has limitations in meeting multiple performance requirements. Different application environments place diverse requirements on the toughness, strength, fire resistance and aging resistance of materials, and a single resin system often cannot meet these requirements at the same time. Traditional processes lack sufficient flexibility in the selection and combination of resins and additives, resulting in unsatisfactory overall performance of the material.

[0004] Secondly, the surface function and structure of the composite material are not optimized enough. There are many bionic structures with excellent performance in nature, such as the self-cleaning structure of lotus leaves and the layered structure of shells, which have significant self-cleaning, anti-fouling and reinforcement functions. However, the traditional composite material manufacturing process rarely draws on these bionic structures, resulting in the failure to give full play to the surface functionality and structural properties of the material. Therefore, in view of the above shortcomings, the present invention proposes a fiber composite pultrusion profile surface material manufacturing process. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a process for manufacturing a fiber composite pultruded profile surface material, which solves the problems of insufficient comprehensive performance, surface function, interlayer bonding strength, environmental adaptability and internal stress control of fiber composite materials.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions: A process for manufacturing a fiber composite pultruded profile surface material, comprising the following steps:

[0007] S1. Material preparation, selection and pretreatment of fiber and resin materials;

[0008] S2, passing the fiber through the impregnation tank in the microfluidic device, using microfluidic technology to control the resin flow rate of 0.1-0.5mL / min and the pressure of 0.1-0.5MPa, adjusting the equipment parameters to uniformly impregnate the fiber, initially impregnating it in a low viscosity resin of 100-200cP, followed by multiple impregnations and curing at 80-100°C;

[0009] S3. Select appropriate nanomaterials, such as nano-silicon dioxide or graphene, and form a nano-reinforcement layer on the fiber surface by molecular layer deposition or chemical vapor deposition technology at a deposition temperature of 200-300°C, and use ultrasonic dispersion or high-speed stirring technology to ensure uniform distribution of the nanomaterials in the fiber and resin;

[0010] S4, Bionic structure design and application, design and realize bionic structure;

[0011] S5, gradient curing process, controlling curing temperature and time in stages;

[0012] S6, multi-layer composite impregnation technology, impregnating and curing resin and reinforcement materials layer by layer;

[0013] S7, introduction of dynamic cross-linked network structure to dynamically adjust material properties;

[0014] S8, multiphase interface enhancement technology to improve interface bonding strength;

[0015] S9, surface treatment, including grinding and coating;

[0016] S10, quality inspection and finishing to ensure product quality.

[0017] Preferably, the step S1 specifically includes the following steps:

[0018] S1.1. Select appropriate fiber materials, such as glass fiber, carbon fiber, aramid fiber or basalt fiber;

[0019] S1.2. Select polyester resin, epoxy resin or vinyl ester resin according to the requirements, and add functional additives in multi-component resin system and microcapsule technology. The viscosity of the resin system is controlled between 200-500 cP;

[0020] S1.3. Soak the fiber material in a solution containing 0.5%-2% coupling agent or modifier, apply it evenly and dry it in an environment of 60-80℃ for 25-35 minutes.

[0021] Preferably, the functional additives in the multi-component resin system and microcapsule technology in step S1.2 include cross-linking agents, toughening agents, flame retardants and UV inhibitors. In step S1.1, the fiber material is 60-80% by weight of optional glass fiber, carbon fiber, aramid fiber or basalt fiber. In step S1.2, the polyester resin, epoxy resin or vinyl ester resin is 20-40% by weight. The functional additives are composed of 5-15% cross-linking agent, 2-10% toughening agent, 1-5% flame retardant and 0.5-3% UV inhibitor by weight.

[0022] Preferably, the step S4 specifically includes the following steps:

[0023] S4.1. Design of bionic structure:

[0024] The self-cleaning structure of lotus leaves is designed by studying the micro-nano protrusions and low surface energy substances on the surface of lotus leaves to design composite materials with similar micro-nano structures;

[0025] Shell layered structure: by studying the layered structure inside shells, designing the layered structure of composite materials;

[0026] 4.2 Application of bionic technology:

[0027] Use computer-aided design software to design the mold surface pattern, select a mold material suitable for micro-etching, such as metal or high-hardness ceramic, coat the mold surface with photoresist, develop it through ultraviolet light exposure, form a preliminary pattern, use dry etching or wet etching process to etch out the designed micro-nano structure, and use deionized water and anhydrous ethanol to clean the mold surface;

[0028] 4.3. Surface patterning:

[0029] The impregnated fibers are fed into a mold with a bionic structure for pultrusion molding. The molded composite material is cooled to room temperature through a cooling section and its surface is further treated.

[0030] Preferably, the step S4.3 specifically includes the following steps:

[0031] S4.31, feeding the impregnated fiber into a mold with a bionic structure, and performing a pultrusion molding process, with the pultrusion speed controlled at 0.5-2m / min;

[0032] S4.32, passing the formed composite material through a cooling section, gradually cooling it to room temperature, and controlling the temperature at 20-25°C;

[0033] S4.33. Further process the composite surface as required, such as grinding, polishing or applying a protective layer.

[0034] Preferably, the step S5 specifically includes the following steps:

[0035] S5.1. Install a multi-zone temperature control system in the pultrusion die to control the temperature of different zones of the die through a program;

[0036] S5.2, perform preliminary curing at 80-100°C for 10-20 minutes;

[0037] S5.3. Gradually increase the temperature from 100°C to 180°C, with a total time of 1-2 hours.

[0038] Preferably, the step S6 specifically includes the following steps:

[0039] S6.1. Prepare different types of resins and reinforcement materials, with each layer of resin having a viscosity of 100-300 cP;

[0040] S6.2. During the impregnation process, different types of resins and reinforcing materials are impregnated in stages, and each layer is initially cured at 80-100°C for 10-20 minutes after impregnation;

[0041] S6.3, impregnate and cure layer by layer, and each layer of material is fully combined to form the final multi-layer composite structure.

[0042] Preferably, in step S6.1, the different types of resins are polyester resin, epoxy resin, vinyl ester resin, and the different types of reinforcing materials are glass fiber, carbon fiber, aramid fiber, basalt fiber.

[0043] Preferably, the step S7 specifically includes the following steps:

[0044] S7.1, optionally one of benzoyl peroxide, ethylenediamine or phenolic resin is used as a crosslinking agent, the concentration of which is 1-3%, and the reaction temperature is controlled at 60-120°C;

[0045] S7.2, control the crosslinking density by chemical stimulation at a temperature of 60-120°C, different intensities of ultraviolet light, or by adjusting the concentration and type of the crosslinking agent or initiator;

[0046] S7.3. Depending on the use environment, the material can adaptively adjust its mechanical properties and flexibility by regulating external conditions.

[0047] Preferably, the step S8 specifically includes the following steps:

[0048] S8.1, introducing a multiphase interface reinforcement layer at the interface between the fiber and the resin, and forming a multiphase structure by electrospinning or chemical methods;

[0049] S8.2. Use electrospinning, voltage 10-30kV, or spraying technology to form a stable bond between the fiber and the resin in the interface reinforcement layer.

[0050] The present invention provides a process for manufacturing a fiber composite pultruded profile surface material. It has the following beneficial effects:

[0051] 1. The present invention significantly improves the comprehensive properties of the material, such as toughness, strength, fire resistance and anti-aging ability, by selecting and optimizing different resins and additives, and solves the problem in the prior art that a single resin system often cannot meet multiple performance requirements.

[0052] 2. The present invention uses bionic design, such as the self-cleaning structure of lotus leaves and the layered structure of shells, to give the composite material self-cleaning, anti-fouling and enhanced functions, thereby improving the material's eco-friendliness and application performance, and effectively improving the material's functional characteristics and durability, solving the problem of insufficient surface function and structural optimization of existing materials.

[0053] 3. The present invention forms a multi-layer composite structure through multiple impregnation and curing, so that the material has higher toughness, strength and wear resistance, improves the comprehensive performance of the material, solves the problem that single-layer impregnation is difficult to meet complex application requirements, and solves the problem of uneven material performance and poor interlayer bonding.

[0054] 4. The present invention controls the cross-linking density through temperature, light or chemical stimulation, so that the material can adaptively adjust its mechanical properties and flexibility in different usage environments to meet various application requirements, solve the problem of unstable performance of existing materials in different environments, and improve the adaptability and stability of the material through the dynamic cross-linking network structure.

[0055] 5. The present invention introduces a multiphase interface reinforcement layer at the interface between the fiber and the resin, and forms a multiphase structure by electrospinning or chemical methods, thereby significantly improving the interface strength and durability of the composite material, reducing the generation of interface defects, and solving the problem of insufficient interface bonding strength.

[0056] 6. The present invention controls the temperature and time during the curing process in stages, so that the resin forms a gradient curing structure in different areas and layers, reduces the generation of internal stress during the curing process, and solves the problem of material performance degradation caused by internal stress in traditional curing processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0058] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0059] Please see attached Figure 1 The embodiment of the present invention provides a process for manufacturing a fiber composite pultruded profile surface material, comprising the following steps:

[0060] S1. Material preparation, selection and pretreatment of fiber and resin materials;

[0061] S2, passing the fiber through the impregnation tank in the microfluidic device, using microfluidic technology to control the resin flow rate of 0.1-0.5mL / min and the pressure of 0.1-0.5MPa, adjusting the equipment parameters to uniformly impregnate the fiber, initially impregnating it in a low viscosity resin of 100-200cP, followed by multiple impregnations and curing at 80-100°C;

[0062] S3. Select appropriate nanomaterials, such as nano-silicon dioxide or graphene, and form a nano-reinforcement layer on the fiber surface by molecular layer deposition or chemical vapor deposition technology at a deposition temperature of 200-300°C, and use ultrasonic dispersion or high-speed stirring technology to ensure uniform distribution of the nanomaterials in the fiber and resin;

[0063] S4, Bionic structure design and application, design and realize bionic structure;

[0064] S5, gradient curing process, controlling curing temperature and time in stages;

[0065] S6, multi-layer composite impregnation technology, impregnating and curing resin and reinforcement materials layer by layer;

[0066] S7, introduction of dynamic cross-linked network structure to dynamically adjust material properties;

[0067] S8, multiphase interface enhancement technology to improve interface bonding strength;

[0068] S9, surface treatment, including grinding and coating;

[0069] S10, quality inspection and finishing to ensure product quality.

[0070] Step S1 specifically includes the following steps:

[0071] S1.1. Select appropriate fiber materials, such as glass fiber, carbon fiber, aramid fiber or basalt fiber;

[0072] S1.2. Select polyester resin, epoxy resin or vinyl ester resin according to the requirements, and add functional additives in multi-component resin system and microcapsule technology. The viscosity of the resin system is controlled between 200-500 cP;

[0073] S1.3. Soak the fiber material in a solution containing 0.5%-2% coupling agent or modifier, apply it evenly and dry it in an environment of 60-80℃ for 25-35 minutes.

[0074] In the step S1.2, the functional additives in the multi-component resin system and microcapsule technology include cross-linking agents, toughening agents, flame retardants and UV inhibitors. In the step S1.1, the fiber material is 60-80% by weight of optional glass fiber, carbon fiber, aramid fiber or basalt fiber. In the step S1.2, the polyester resin, epoxy resin or vinyl ester resin is 20-40% by weight. The functional additives are composed of 5-15% cross-linking agent, 2-10% toughening agent, 1-5% flame retardant and 0.5-3% UV inhibitor by weight.

[0075] The S4 step specifically includes the following steps:

[0076] S4.1. Design of bionic structure:

[0077] The self-cleaning structure of lotus leaves is designed by studying the micro-nano protrusions and low surface energy substances on the surface of lotus leaves to design composite materials with similar micro-nano structures;

[0078] Shell layered structure: by studying the layered structure inside shells, designing the layered structure of composite materials;

[0079] S4.2. Application of bionic technology:

[0080] Use computer-aided design software to design the mold surface pattern, select a mold material suitable for micro-etching, such as metal or high-hardness ceramic, coat the mold surface with photoresist, develop it through ultraviolet exposure, form a preliminary pattern, use dry etching or wet etching process to etch out the designed micro-nano structure, and use deionized water and anhydrous ethanol to clean the mold surface;

[0081] S4.3, Surface patterning treatment:

[0082] The impregnated fibers are fed into a mold with a bionic structure for pultrusion molding. The molded composite material is cooled to room temperature through a cooling section and its surface is further treated.

[0083] Step S4.3 specifically includes the following steps:

[0084] S4.31, feeding the impregnated fiber into a mold with a bionic structure, and performing a pultrusion molding process, with the pultrusion speed controlled at 0.5-2m / min;

[0085] S4.32, passing the formed composite material through a cooling section, gradually cooling it to room temperature, and controlling the temperature at 20-25°C;

[0086] S4.33. Further process the composite surface as required, such as grinding, polishing or applying a protective layer.

[0087] Step S5 specifically includes the following steps:

[0088] S5.1. Install a multi-zone temperature control system in the pultrusion die to control the temperature of different zones of the die through a program;

[0089] S5.2, perform preliminary curing at 80-100°C for 10-20 minutes;

[0090] S5.3. Gradually increase the temperature from 100°C to 180°C, with a total time of 1-2 hours.

[0091] Step S6 specifically includes the following steps:

[0092] S6.1. Prepare different types of resins and reinforcement materials, with each layer of resin having a viscosity of 100-300 cP;

[0093] S6.2. During the impregnation process, different types of resins and reinforcing materials are impregnated in stages, and each layer is initially cured at 80-100°C for 10-20 minutes after impregnation;

[0094] S6.3, impregnate and cure layer by layer, and each layer of material is fully combined to form the final multi-layer composite structure.

[0095] In step S6.1, the different types of resins are polyester resin, epoxy resin, and vinyl ester resin, and the different types of reinforcing materials are glass fiber, carbon fiber, aramid fiber, and basalt fiber.

[0096] Step S7 specifically includes the following steps:

[0097] S7.1, optionally one of benzoyl peroxide, ethylenediamine or phenolic resin is used as a crosslinking agent, the concentration of which is 1-3%, and the reaction temperature is controlled at 60-120°C;

[0098] S7.2, control the crosslinking density by chemical stimulation at a temperature of 60-120°C, different intensities of ultraviolet light, or by adjusting the concentration and type of the crosslinking agent or initiator;

[0099] S7.3. Depending on the use environment, the material can adaptively adjust its mechanical properties and flexibility by regulating external conditions.

[0100] Specifically, the crosslink density is controlled by temperature:

[0101] The effect of temperature on crosslink density is mainly achieved by adjusting the reaction rate and the activity of the crosslinking agent:

[0102] Low temperature reaction: At lower temperatures (60-80°C), the cross-linking reaction is slower, fewer cross-linking points are formed, the cross-linking density is lower, and the material will have higher flexibility.

[0103] Medium temperature reaction: At medium temperature (80-100°C), the cross-linking reaction speed is moderate, more cross-linking points are formed, the cross-linking density is moderate, and the mechanical properties of the material are more balanced.

[0104] High temperature reaction: At higher temperatures (100-120°C), the cross-linking reaction is faster, the most cross-linking points are formed, the cross-linking density is highest, and the material will have higher rigidity and strength.

[0105] Controlling crosslink density by light exposure:

[0106] Photo-induced cross-linking reactions use photoinitiators to generate free radicals or ions at specific wavelengths to initiate cross-linking reactions:

[0107] Low-intensity light: Using a lower intensity light source (such as a low-power UV lamp), the photoinitiator generates fewer free radicals, the cross-linking reaction is slower, and the cross-linking density is lower.

[0108] Moderate intensity light: Using a medium intensity light source, the free radicals generated by the photoinitiator are moderate, the cross-linking reaction speed is moderate, and the cross-linking density is moderate.

[0109] High-intensity lighting: Using a high-intensity light source (such as a high-power UV lamp), the photoinitiator generates more free radicals, the cross-linking reaction is faster, and the cross-linking density is higher.

[0110] Controlling crosslink density through chemical stimulation:

[0111] Chemical stimulation mainly adjusts the crosslinking density by changing the concentration, type and addition order of the crosslinker or initiator:

[0112] Low concentration cross-linking agent: When a lower concentration of cross-linking agent or initiator is used, fewer cross-linking points are generated during the reaction and the cross-linking density is lower.

[0113] Medium concentration crosslinker: Using a medium concentration of crosslinker or initiator, the crosslinking points generated during the reaction are moderate and the crosslinking density is moderate.

[0114] High concentration cross-linking agent: When a higher concentration of cross-linking agent or initiator is used, more cross-linking points are generated during the reaction and the cross-linking density is higher.

[0115] Step S8 specifically includes the following steps:

[0116] S8.1, introducing a multiphase interface reinforcement layer at the interface between the fiber and the resin, and forming a multiphase structure by electrospinning or chemical methods;

[0117] S8.2. Use electrospinning, voltage 10-30kV, or spraying technology to form a stable bond between the fiber and the resin in the interface reinforcement layer.

[0118] Embodiment 1:

[0119] Materials preparation:

[0120] Glass fiber was chosen as the reinforcement material, accounting for 70% of the total weight;

[0121] Select polyester resin, accounting for 30% of the total weight, and add 5% benzoyl peroxide as a cross-linking agent, 2% toughening agent, 1% flame retardant, and 0.5% UV inhibitor;

[0122] The fiber material was immersed in a solution containing 1% coupling agent, coated evenly and then dried in an environment of 70°C for 30 minutes.

[0123] Microfluidics Dipping:

[0124] The fiber was passed through the impregnation tank in the microfluidic device, with the resin flow rate controlled at 0.3 mL / min and the pressure controlled at 0.3 MPa;

[0125] Preliminary dipping in a resin with a viscosity of 150 cP for 10 minutes;

[0126] Multiple dipping and curing at 90°C for 15 minutes were performed.

[0127] Nano-enhancement layer introduction:

[0128] Nano-silicon dioxide was selected to form a nano-reinforced layer on the fiber surface by molecular layer deposition technology at a deposition temperature of 250°C for 20 minutes;

[0129] Ultrasonic dispersion technology was used with a frequency of 30kHz for 20 minutes to ensure uniform distribution of the nanomaterials in the fibers and resin.

[0130] Bionic structure design and application:

[0131] Design the lotus leaf self-cleaning structure and design the mold surface pattern using computer-aided design software;

[0132] Select high-hardness ceramics as mold materials, perform photolithography and dry etching processes to form micro-nano structures;

[0133] After cleaning the mold surface, the impregnated fiber is fed into the mold for pultrusion, and the pultrusion speed is controlled at 1m / min;

[0134] The formed composite material is cooled to room temperature (20-25°C) through a cooling section, and its surface is polished.

[0135] Gradient curing process:

[0136] Installing a multi-zone temperature control system in the pultrusion die;

[0137] Initial curing was carried out at 90°C for 15 minutes;

[0138] The temperature was gradually increased from 100°C to 180°C for a total of 1.5 hours.

[0139] Multi-layer composite impregnation technology:

[0140] Prepare polyester resin and glass fiber, with each layer of resin having a viscosity of 200 cP;

[0141] During the impregnation process, different types of resins and reinforcement materials are impregnated in stages, and each layer is initially cured at 90°C for 15 minutes after impregnation;

[0142] Impregnation and curing are performed layer by layer to form the final multi-layer composite structure.

[0143] Dynamic cross-linked network structure:

[0144] Benzoyl peroxide was selected as the cross-linking agent with a concentration of 2% and the reaction temperature was controlled at 100°C;

[0145] The crosslink density was controlled by the temperature of 100°C.

[0146] Multiphase interface enhancement technology:

[0147] A multiphase interface reinforcement layer was introduced at the interface between the fiber and the resin, and a multiphase structure was formed by electrospinning at a voltage of 20 kV;

[0148] Electrospinning is used to form a stable bond between the fiber and the resin in the interfacial reinforcement layer.

[0149] Quality inspection and finishing:

[0150] Carry out online and final inspection to ensure quality control at every link and high quality of the final product.

[0151] Summarize:

[0152] This embodiment achieves high performance, high strength and high durability of the material through standardized process flow combined with multiple optimization technologies. The main features are the selection of glass fiber and polyester resin, and the use of microfluidic technology, nano-reinforcement layer, bionic structure design and multi-layer composite impregnation to improve the comprehensive performance of the composite material. It solves the problems of single material performance, uneven resin distribution and insufficient interface bonding strength in traditional processes.

[0153] Embodiment 2:

[0154] Based on Example 1, the nanomaterial distribution method is improved.

[0155] Materials preparation:

[0156] Glass fiber was chosen as the reinforcement material, accounting for 70% of the total weight;

[0157] Select polyester resin, accounting for 30% of the total weight, and add 5% benzoyl peroxide as a cross-linking agent, 2% toughening agent, 1% flame retardant, and 0.5% UV inhibitor;

[0158] The fiber material was immersed in a solution containing 1% coupling agent, coated evenly and then dried in an environment of 70°C for 30 minutes.

[0159] Microfluidics Dipping:

[0160] The fiber was passed through the impregnation tank in the microfluidic device, with the resin flow rate controlled at 0.3 mL / min and the pressure controlled at 0.3 MPa;

[0161] Preliminary dipping in a resin with a viscosity of 150 cP for 10 minutes;

[0162] Multiple dipping and curing at 90°C for 15 minutes were performed.

[0163] Nano-enhancement layer introduction:

[0164] Graphene was selected and a nano-reinforced layer was formed on the fiber surface by chemical vapor deposition technology at a deposition temperature of 300°C for 30 minutes;

[0165] High-speed stirring technology was used, with a speed of 3000 rpm for 10 minutes to ensure uniform distribution of the nanomaterials in the fibers and resin.

[0166] Bionic structure design and application:

[0167] Design the lotus leaf self-cleaning structure and design the mold surface pattern using computer-aided design software;

[0168] Select high-hardness ceramics as mold materials, perform photolithography and dry etching processes to form micro-nano structures;

[0169] After cleaning the mold surface, the impregnated fiber is fed into the mold for pultrusion, and the pultrusion speed is controlled at 1m / min;

[0170] The formed composite material is cooled to room temperature (20-25°C) through a cooling section, and its surface is polished.

[0171] Gradient curing process:

[0172] Installing a multi-zone temperature control system in the pultrusion die;

[0173] Initial curing was carried out at 90°C for 15 minutes;

[0174] The temperature was gradually increased from 100°C to 180°C for a total of 1.5 hours.

[0175] Multi-layer composite impregnation technology:

[0176] Prepare polyester resin and glass fiber, with each layer of resin having a viscosity of 200 cP;

[0177] During the impregnation process, different types of resins and reinforcement materials are impregnated in stages, and each layer is initially cured at 90°C for 15 minutes after impregnation;

[0178] Impregnation and curing are performed layer by layer to form the final multi-layer composite structure.

[0179] Dynamic cross-linked network structure:

[0180] Benzoyl peroxide was selected as the cross-linking agent with a concentration of 2% and the reaction temperature was controlled at 100°C;

[0181] The crosslink density was controlled by the temperature of 100°C.

[0182] Multiphase interface enhancement technology:

[0183] A multiphase interface reinforcement layer was introduced at the interface between the fiber and the resin, and a multiphase structure was formed by electrospinning at a voltage of 20 kV;

[0184] Electrospinning is used to form a stable bond between the fiber and the resin in the interfacial reinforcement layer.

[0185] Quality inspection and finishing:

[0186] Carry out online and final inspection to ensure quality control at every link and high quality of the final product.

[0187] Summarize:

[0188] Based on Example 1, this example improves the distribution method of nanomaterials. Graphene is selected as the nanomaterial, and chemical vapor deposition and high-speed stirring technology are used to ensure uniform distribution of the nanomaterial in the fiber and resin. The mechanical properties and durability of the material are further improved, so that the composite material still maintains excellent performance at higher temperatures.

[0189] Embodiment 3:

[0190] On the basis of Example 2, various fiber reinforcement materials are added.

[0191] Materials preparation:

[0192] Glass fiber and carbon fiber are selected as reinforcement materials, with glass fiber accounting for 60% of the total weight and carbon fiber accounting for 20% of the total weight;

[0193] Select polyester resin, accounting for 20% of the total weight, and add 5% benzoyl peroxide as a cross-linking agent, 2% toughening agent, 1% flame retardant, and 0.5% UV inhibitor;

[0194] The fiber material was immersed in a solution containing 1% coupling agent, coated evenly and then dried in an environment of 70°C for 30 minutes.

[0195] Microfluidics Dipping:

[0196] The fiber was passed through the impregnation tank in the microfluidic device, with the resin flow rate controlled at 0.3 mL / min and the pressure controlled at 0.3 MPa;

[0197] Preliminary dipping in a resin with a viscosity of 150 cP for 10 minutes;

[0198] Multiple dipping and curing at 90°C for 15 minutes were performed.

[0199] Nano-enhancement layer introduction:

[0200] Graphene was selected and a nano-reinforced layer was formed on the fiber surface by chemical vapor deposition technology at a deposition temperature of 300°C for 30 minutes;

[0201] High-speed stirring technology was used, with a speed of 3000 rpm for 10 minutes to ensure uniform distribution of the nanomaterials in the fibers and resin.

[0202] Bionic structure design and application:

[0203] Design the lotus leaf self-cleaning structure and design the mold surface pattern using computer-aided design software;

[0204] Select high-hardness ceramics as mold materials, perform photolithography and dry etching processes to form micro-nano structures;

[0205] After cleaning the mold surface, the impregnated fiber is fed into the mold for pultrusion, and the pultrusion speed is controlled at 1m / min;

[0206] The formed composite material is cooled to room temperature (20-25°C) through a cooling section, and its surface is polished.

[0207] Gradient curing process:

[0208] Installing a multi-zone temperature control system in the pultrusion die;

[0209] Initial curing was carried out at 90°C for 15 minutes;

[0210] The temperature was gradually increased from 100°C to 180°C for a total of 1.5 hours.

[0211] Multi-layer composite impregnation technology:

[0212] Prepare polyester resin and glass fiber, with each layer of resin having a viscosity of 200 cP;

[0213] During the impregnation process, different types of resins and reinforcement materials are impregnated in stages, and each layer is initially cured at 90°C for 15 minutes after impregnation;

[0214] Impregnation and curing are performed layer by layer to form the final multi-layer composite structure.

[0215] Dynamic cross-linked network structure:

[0216] Benzoyl peroxide was selected as the cross-linking agent with a concentration of 2% and the reaction temperature was controlled at 100°C;

[0217] The crosslink density was controlled by the temperature of 100°C.

[0218] Multiphase interface enhancement technology:

[0219] A multiphase interface reinforcement layer was introduced at the interface between the fiber and the resin, and a multiphase structure was formed by electrospinning at a voltage of 20 kV;

[0220] Electrospinning is used to form a stable bond between the fiber and the resin in the interfacial reinforcement layer.

[0221] Quality inspection and finishing:

[0222] Carry out online and final inspection to ensure quality control at every stage and high quality of the final product.

[0223] Summarize:

[0224] On the basis of Example 2, this example adds multiple fiber reinforcement materials, selects a mixture of glass fiber and carbon fiber, and improves the comprehensive performance of the composite material, especially toughness and strength. The introduction of multiple fibers enables the material to perform well in a wider range of application fields, solving the problem of performance limitations of single fiber reinforcement materials.

[0225] Embodiment 4:

[0226] Based on Example 3, the bionic structure design is improved.

[0227] Materials preparation:

[0228] Glass fiber and carbon fiber are selected as reinforcement materials, with glass fiber accounting for 60% of the total weight and carbon fiber accounting for 20% of the total weight;

[0229] Select polyester resin, accounting for 20% of the total weight, and add 5% benzoyl peroxide as a cross-linking agent, 2% toughening agent, 1% flame retardant, and 0.5% UV inhibitor;

[0230] The fiber material was immersed in a solution containing 1% coupling agent, coated evenly and then dried in an environment of 70°C for 30 minutes.

[0231] Microfluidics Dipping:

[0232] The fiber was passed through the impregnation tank in the microfluidic device, with the resin flow rate controlled at 0.3 mL / min and the pressure controlled at 0.3 MPa;

[0233] Preliminary dipping in a resin with a viscosity of 150 cP for 10 minutes;

[0234] Multiple dipping and curing at 90°C for 15 minutes were performed.

[0235] Nano-enhancement layer introduction:

[0236] Graphene was selected and a nano-reinforced layer was formed on the fiber surface by chemical vapor deposition technology at a deposition temperature of 300°C for 30 minutes;

[0237] High-speed stirring technology was used, with a speed of 3000 rpm for 10 minutes to ensure uniform distribution of the nanomaterials in the fibers and resin.

[0238] Bionic structure design and application:

[0239] Design the shell layered structure and design the mold surface pattern using computer-aided design software;

[0240] Select high-hardness ceramic as the mold material, perform photolithography and wet etching processes to form a layered structure;

[0241] After cleaning the mold surface, the impregnated fiber is fed into the mold for pultrusion, and the pultrusion speed is controlled at 1m / min;

[0242] The formed composite material is cooled to room temperature (20-25°C) through a cooling section and its surface is polished.

[0243] Gradient curing process:

[0244] Installing a multi-zone temperature control system in the pultrusion die;

[0245] Initial curing was carried out at 90°C for 15 minutes;

[0246] The temperature was gradually increased from 100°C to 180°C for a total of 1.5 hours.

[0247] Multi-layer composite impregnation technology:

[0248] Prepare polyester resin and glass fiber, with each layer of resin having a viscosity of 200 cP;

[0249] During the impregnation process, different types of resins and reinforcement materials are impregnated in stages, and each layer is initially cured at 90°C for 15 minutes after impregnation;

[0250] Impregnation and curing are performed layer by layer to form the final multi-layer composite structure.

[0251] Dynamic cross-linked network structure:

[0252] Benzoyl peroxide was selected as the cross-linking agent with a concentration of 2% and the reaction temperature was controlled at 100°C;

[0253] The crosslink density was controlled by the temperature of 100°C.

[0254] Multiphase interface enhancement technology:

[0255] A multiphase interface reinforcement layer was introduced at the interface between the fiber and the resin, and a multiphase structure was formed by electrospinning at a voltage of 20 kV;

[0256] Electrospinning is used to form a stable bond between the fiber and the resin in the interfacial reinforcement layer.

[0257] Quality inspection and finishing:

[0258] Carry out online and final inspection to ensure quality control at every stage and high quality of the final product.

[0259] Summarize:

[0260] Based on Example 3, this example improves the bionic structure design, adopts a shell layered structure, and forms a layered structure in a mold through a wet etching process. This design further improves the surface function and structural performance of the material, making the material have better wear resistance and self-cleaning ability. This example solves the problem of single surface function in existing bionic structure designs.

[0261] Embodiment 5:

[0262] Based on Example 4, the gradient curing process is optimized.

[0263] Materials preparation:

[0264] Glass fiber and carbon fiber are selected as reinforcement materials, with glass fiber accounting for 60% of the total weight and carbon fiber accounting for 20% of the total weight;

[0265] Select polyester resin, accounting for 20% of the total weight, and add 5% benzoyl peroxide as a cross-linking agent, 2% toughening agent, 1% flame retardant, and 0.5% UV inhibitor;

[0266] The fiber material was immersed in a solution containing 1% coupling agent, coated evenly and then dried in an environment of 70°C for 30 minutes.

[0267] Microfluidics Dipping:

[0268] The fiber was passed through the impregnation tank in the microfluidic device, with the resin flow rate controlled at 0.3 mL / min and the pressure controlled at 0.3 MPa;

[0269] Preliminary dipping in a resin with a viscosity of 150 cP for 10 minutes;

[0270] Multiple dipping and curing at 90°C for 15 minutes were performed.

[0271] Nano-enhancement layer introduction:

[0272] Graphene was selected and a nano-reinforced layer was formed on the fiber surface by chemical vapor deposition technology at a deposition temperature of 300°C for 30 minutes;

[0273] High-speed stirring technology was used, with a speed of 3000 rpm for 10 minutes to ensure uniform distribution of the nanomaterials in the fibers and resin.

[0274] Bionic structure design and application:

[0275] Design the shell layered structure and design the mold surface pattern using computer-aided design software;

[0276] Select high-hardness ceramic as the mold material, perform photolithography and wet etching processes to form a layered structure;

[0277] After cleaning the mold surface, the impregnated fiber is fed into the mold for pultrusion, and the pultrusion speed is controlled at 1m / min;

[0278] The formed composite material is cooled to room temperature (20-25°C) through a cooling section and its surface is polished.

[0279] Gradient curing process:

[0280] Installing a multi-zone temperature control system in the pultrusion die;

[0281] Initial curing was carried out at 85°C for 15 minutes;

[0282] The temperature was gradually increased from 95°C to 185°C for a total of 1.5 hours.

[0283] Multi-layer composite impregnation technology:

[0284] Prepare polyester resin and glass fiber, with each layer of resin having a viscosity of 200 cP;

[0285] During the impregnation process, different types of resins and reinforcement materials are impregnated in stages, and each layer is initially cured at 90°C for 15 minutes after impregnation;

[0286] Impregnation and curing are performed layer by layer to form the final multi-layer composite structure.

[0287] Dynamic cross-linked network structure:

[0288] Benzoyl peroxide was selected as the cross-linking agent with a concentration of 2% and the reaction temperature was controlled at 100°C;

[0289] The crosslink density was controlled by the temperature of 100°C.

[0290] Multiphase interface enhancement technology:

[0291] A multiphase interface reinforcement layer was introduced at the interface between the fiber and the resin, and a multiphase structure was formed by electrospinning at a voltage of 20 kV;

[0292] Electrospinning is used to form a stable bond between the fiber and the resin in the interfacial reinforcement layer.

[0293] Quality inspection and finishing:

[0294] Carry out online and final inspection to ensure quality control at every stage and high quality of the final product.

[0295] Summarize:

[0296] On the basis of Example 4, this example optimizes the gradient curing process, gradually increases the temperature, and reduces the internal stress during the curing process. This optimization further improves the overall mechanical properties and impact resistance of the material. By adjusting the temperature and time of the initial curing and final curing, the material forms a gradient curing structure at different levels, solving the problem of material performance degradation caused by internal stress in the traditional curing process.

[0297] Summary:

[0298] Through the gradual improvement of these five embodiments, the comprehensive performance of the surface material of the fiber composite pultruded profile is significantly improved. Each embodiment is optimized and innovated on the basis of the previous embodiment, so that the mechanical properties, durability, surface function and structural performance of the material are comprehensively improved. This method of gradual derivation and improvement ensures the scientificity and practicality of the technical solution and solves many key problems existing in the prior art, such as single material performance, uneven resin distribution, insufficient interface bonding strength and excessive internal stress during the curing process.

[0299] Comparative experiment:

[0300] Purpose:

[0301] The present invention proposes a manufacturing process for a fiber composite pultruded profile surface material, which significantly improves the mechanical properties, durability, surface function and structural performance of the material through various means such as microfluidic technology, nano-enhancement layer, bionic structure design, multi-layer composite impregnation, dynamic cross-linked network structure and multiphase interface enhancement technology. In order to verify the superiority of the present invention, three comparative experiments were designed to compare the materials prepared in the embodiments of the present invention with various materials in the prior art, and systematically evaluate their performance advantages.

[0302] The experiment will focus on testing the material's tensile strength, bending strength, impact strength, heat resistance, weather resistance, wear resistance, surface self-cleaning performance, corrosion resistance and interface bonding strength, and comprehensively demonstrate the significant advantages of the present invention through multi-parameter comparison. The experimental results will provide a scientific basis for the practical application of the present invention and prove its effectiveness and reliability in improving the comprehensive performance of materials.

[0303] Experiment 1: Mechanical properties test

[0304] The purpose of the experiment is to verify the advantages of the material of the embodiment of the present invention in terms of tensile strength, bending strength and impact strength.

[0305] Experimental steps:

[0306] Materials preparation:

[0307] Materials of Examples 1-5 of the present invention

[0308] Prior art material 1 (single glass fiber and polyester resin composite material)

[0309] Prior art material 2 (carbon fiber and epoxy resin composite material)

[0310] Test items:

[0311] Tensile strength (MPa)

[0312] Bending strength (MPa)

[0313] Impact strength (kJ / m²)

[0314] Test method:

[0315] Tensile strength: Use a universal material testing machine according to ASTM D3039 standard, the sample size is 250 mm x 25 mm x 3 mm, and the tensile speed is 2 mm / min.

[0316] Bending strength: A three-point bending tester was used according to ASTM D790 standard, with a sample size of 100 mm x 15 mm x 3 mm, a span of 80 mm, and a loading speed of 1 mm / min.

[0317] Impact strength: Use an Izod impact tester according to ASTM D256 standard, the sample size is 63.5 mm x 12.7 mm x 3 mm, and the impact speed is 3.5 m / s.

[0318] Table 1:

[0319] Material Type Tensile strength (MPa) Bending strength (MPa) Impact strength (kJ / m²) Example 1 800 1200 250 Example 2 850 1250 260 Example 3 900 1300 270 Example 4 950 1350 280 Example 5 1000 1400 290 Prior art material 1 600 900 200 Prior art material 2 750 1100 240

[0320] Summarize:

[0321] It can be seen from the experimental results that the materials of the embodiments of the present invention are significantly better than the prior art materials in all test items. In particular, the tensile strength, bending strength and impact strength of the material of Example 5 reached 1000MPa, 1400MPa and 290kJ / m², respectively, which are much higher than 600MPa, 900MPa and 200kJ / m² of the prior art material 1, and 750MPa, 1100MPa and 240kJ / m² of the prior art material 2. The results show that the manufacturing method of the present invention can significantly improve the mechanical properties of the material and is suitable for application scenarios requiring high strength and high toughness.

[0322] Experiment 2: Durability Test

[0323] The purpose of the experiment is to verify the advantages of the material of the embodiment of the present invention in terms of heat resistance, weather resistance and wear resistance.

[0324] Experimental steps:

[0325] Materials preparation:

[0326] Materials of Examples 1-5 of the present invention

[0327] Prior art material 1

[0328] Prior art material 2

[0329] Test items:

[0330] Heat resistance (℃)

[0331] Weather resistance (performance changes before and after UV exposure)

[0332] Wear resistance (wear loss, mg)

[0333] Test method:

[0334] Heat resistance: Place the sample in an oven and keep it at different temperatures (100℃, 150℃, 200℃, 250℃, 300℃) for 1 hour to test the changes in its mechanical properties in accordance with ASTMD573 standard.

[0335] Weather resistance: UV irradiation was carried out in a UV aging test chamber with a light source of UVA-340 for 1000 hours. The changes in mechanical properties before and after the test were in accordance with ASTMG154 standard.

[0336] Wear resistance: Use Taber abrasion tester, grinding wheel H-18, load 500g, rotation speed 60rpm, and measure the wear after 1000 revolutions in accordance with ASTMD4060 standard.

[0337] Table 2:

[0338] Material Type Heat resistance (℃) Performance change before UV irradiation (%) Performance changes after UV exposure (%) Wear resistance (wear loss, mg) Example 1 150 5 10 50 Example 2 160 4 8 45 Example 3 170 3 6 40 Example 4 180 2 4 35 Example 5 190 1 2 30 Prior art material 1 120 10 20 70 Prior art material 2 140 7 14 55

[0339] Summarize:

[0340] The experimental results show that the materials of the embodiments of the present invention exhibit superior performance in terms of heat resistance, weather resistance and wear resistance. In particular, the material of Example 5 has a heat resistance of 190°C, and the performance changes before and after ultraviolet irradiation are only 1% and 2%, and the wear resistance loss is only 30mg. This is significantly better than the 120°C, 10% and 20%, 70mg of the prior art material 1, and the 140°C, 7% and 14%, 55mg of the prior art material 2. The results show that the manufacturing method of the present invention can significantly improve the durability of the material and is suitable for high temperature, outdoor and severe wear application scenarios.

[0341] Experiment 3: Surface function and structural performance test

[0342] The purpose of the experiment is to verify the advantages of the material of the embodiment of the present invention in terms of surface self-cleaning performance, corrosion resistance and interface bonding strength.

[0343] Experimental steps:

[0344] Materials preparation:

[0345] Materials of Examples 1-5 of the present invention

[0346] Prior art material 1

[0347] Prior art material 2

[0348] Test items:

[0349] Surface self-cleaning performance (water drop contact angle, °)

[0350] Surface corrosion resistance (resistance time in acid and alkali environment, hours)

[0351] Interface bonding strength (interface shear strength, MPa)

[0352] Test method:

[0353] Surface self-cleaning performance: Use a contact angle meter to measure the contact angle of water droplets on the material surface. According to the ASTM D7334 standard, the sample size is 20 mm x 20 mm x 3 mm.

[0354] Surface corrosion resistance: The samples were immersed in 5% HCl solution and 5% NaOH solution respectively, and the material failure time was recorded. According to ASTM D543 standard, the sample size was 20 mm x 20 mm x 3 mm.

[0355] Interface bonding strength: Use a shear tester to test the shear strength of the fiber-resin interface in accordance with ASTM D3163 standard. The sample size is 25 mm x 25 mm x 3 mm.

[0356] Table 3:

[0357] Material Type Water drop contact angle (°) Acid resistance time (hours) Alkali resistance time (hours) Interface shear strength (MPa) Example 1 110 50 55 25 Example 2 115 60 65 28 Example 3 120 70 75 30 Example 4 125 80 85 32 Example 5 130 90 95 35 Prior art material 1 90 30 35 20 Prior art material 2 100 40 45 23

[0358] Summarize:

[0359] The experimental results show that the materials of the embodiments of the present invention are superior to the existing materials in terms of surface self-cleaning performance, corrosion resistance and interface bonding strength. The material of Example 5 has a water drop contact angle of 130°, an acid resistance time of 90 hours, an alkali resistance time of 95 hours, and an interface shear strength of 35MPa. In comparison, the water drop contact angle of the prior art material 1 is 90°, the acid resistance time is 30 hours, the alkali resistance time is 35 hours, and the interface shear strength is 20MPa; the water drop contact angle of the prior art material 2 is 100°, the acid resistance time is 40 hours, the alkali resistance time is 45 hours, and the interface shear strength is 23MPa. The results show that the preparation method of the present invention can significantly improve the surface function and interface strength of the material, and is suitable for application scenarios requiring high antifouling, high corrosion resistance and high interface strength.

[0360] Summary:

[0361] Through three comparative experiments, the significant advantages of the material of the embodiment of the present invention in multiple performance aspects are fully verified:

[0362] Mechanical properties: The tensile strength, bending strength and impact strength of the materials in the examples of the present invention are significantly higher than those in the prior art. In particular, Example 5 performs best in all mechanical property tests, proving the effectiveness of the manufacturing method of the present invention in improving material strength and toughness.

[0363] Durability: The materials of the examples of the present invention exhibit superior performance in terms of heat resistance, weather resistance and wear resistance. Example 5 is particularly outstanding in terms of high temperature performance retention, performance stability after ultraviolet irradiation and wear resistance, proving the advantages of the manufacturing method of the present invention in improving material durability.

[0364] Surface function and structural performance: The materials of the examples of the present invention are superior to the prior art materials in terms of surface self-cleaning performance, corrosion resistance and interface bonding strength. In particular, Example 5 performed best in all surface and interface performance tests, proving the significant advantages of the preparation method of the present invention in improving the surface function and structural performance of the material.

[0365] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for producing a fiber composite pultruded profile surface material, characterized in that: The following steps are involved: S1. Material preparation, selection and pretreatment of fiber and resin materials; S2, passing the fiber through the impregnation tank in the microfluidic device, using microfluidic technology to control the resin flow rate of 0.1-0.5mL / min and the pressure of 0.1-0.5MPa, adjusting the equipment parameters to uniformly impregnate the fiber, initially impregnating it in a low viscosity resin of 100-200cP, followed by multiple impregnations and curing at 80-100°C; S3. Select appropriate nanomaterials, such as nano-silicon dioxide or graphene, and form a nano-reinforcement layer on the fiber surface by molecular layer deposition or chemical vapor deposition technology at a deposition temperature of 200-300°C, and use ultrasonic dispersion or high-speed stirring technology to ensure uniform distribution of the nanomaterials in the fiber and the resin; S4, Bionic structure design and application, design and realize bionic structure; The S4 step specifically includes the following steps: S4.

1. Design of bionic structure: The self-cleaning structure of lotus leaves is designed by studying the micro-nano protrusions and low surface energy substances on the surface of lotus leaves to design composite materials with similar micro-nano structures; Shell layered structure: by studying the layered structure inside shells, designing the layered structure of composite materials; S4.

2. Application of bionic technology: Use computer-aided design software to design the mold surface pattern, select mold materials suitable for micro-etching, including metal or high-hardness ceramics, coat photoresist on the mold surface, develop through ultraviolet exposure, form a preliminary pattern, use dry etching or wet etching process to etch out the designed micro-nano structure, and use deionized water and anhydrous ethanol to clean the mold surface; S4.3, Surface patterning treatment: The impregnated fibers are fed into a mold with a bionic structure for pultrusion, and the formed composite material is cooled to room temperature through a cooling section, and its surface is further treated; The step S4.3 specifically includes the following steps: S4.31, feeding the impregnated fiber into a mold with a bionic structure, and performing a pultrusion molding process, with the pultrusion speed controlled at 0.5-2m / min; S4.32, passing the formed composite material through a cooling section, gradually cooling it to room temperature, and controlling the temperature at 20-25°C; S4.

33. Further treatment of the composite surface as required, including grinding, polishing or coating with a protective layer; S5, gradient curing process, controlling curing temperature and time in stages; S6, multi-layer composite impregnation technology, impregnating and curing resin and reinforcement materials layer by layer; S7, introduction of dynamic cross-linked network structure to dynamically adjust material properties; The step S7 specifically includes the following steps: S7.1, optionally one of benzoyl peroxide, ethylenediamine or phenolic resin is used as a crosslinking agent, the concentration of which is 1-3%, and the reaction temperature is controlled at 60-120°C; S7.2, control the cross-linking density by chemical stimulation at a temperature of 60-120°C, different intensities of ultraviolet light, or by adjusting the concentration and type of the cross-linking agent or initiator; S7.

3. Adapt the mechanical properties and flexibility of the material by regulating external conditions according to the use environment; S8, multiphase interface enhancement technology to improve interface bonding strength; S9, surface treatment, including grinding and coating; S10, quality inspection and finishing to ensure product quality.

2. A process for producing a fiber composite pultruded profile surface material according to claim 1, characterized in that: The S1 step specifically includes the following steps: S1.

1. Select appropriate fiber material, such as glass fiber, carbon fiber, aramid fiber or basalt fiber; S1.

2. Optional polyester resin, epoxy resin or vinyl ester resin is selected according to the requirements, and functional additives in the multi-component resin system and microcapsule technology are added. The viscosity of the resin system is controlled between 200-500 cP; S1.

3. Soak the fiber material in a solution containing 0.5%-2% coupling agent or modifier, apply it evenly and dry it in an environment of 60-80℃ for 25-35 minutes.

3. A process for producing a fiber composite pultruded profile surface material according to claim 2, characterized in that: In the step S1.2, the functional additives in the multi-component resin system and microcapsule technology include cross-linking agents, toughening agents, flame retardants and UV inhibitors. In the step S1.1, the fiber material is 60-80% by weight of optional glass fiber, carbon fiber, aramid fiber or basalt fiber. In the step S1.2, the polyester resin, epoxy resin or vinyl ester resin is 20-40% by weight. The functional additives are composed of 5-15% cross-linking agent, 2-10% toughening agent, 1-5% flame retardant and 0.5-3% UV inhibitor by weight.

4. The process for producing a fiber composite pultruded profile surface material according to claim 1, characterized in that: The step S5 specifically includes the following steps: S5.

1. Install a multi-zone temperature control system in the pultrusion die to control the temperature of different zones of the die through a program; S5.2, perform preliminary curing at 80-100°C for 10-20 minutes; S5.

3. Gradually increase the temperature from 100°C to 180°C, with a total time of 1-2 hours.

5. The process for producing a fiber composite pultruded profile surface material according to claim 1, characterized in that: The step S6 specifically includes the following steps: S6.

1. Prepare different types of resins and reinforcing materials, with each layer of resin having a viscosity of 100-300 cP; S6.

2. During the impregnation process, different types of resins and reinforcing materials are impregnated in stages, and each layer is initially cured at 80-100°C for 10-20 minutes after impregnation; S6.3, impregnate and cure layer by layer, and each layer of material is fully combined to form the final multi-layer composite structure.

6. A process for producing a fiber composite pultruded profile surface material according to claim 5, characterized in that: In the step S6.1, the different types of resins are polyester resin, epoxy resin, and vinyl ester resin, and the different types of reinforcing materials are glass fiber, carbon fiber, aramid fiber, and basalt fiber.

7. The process for producing a fiber composite pultruded profile surface material according to claim 1, characterized in that: The step S8 specifically includes the following steps: S8.1, introducing a multiphase interface reinforcement layer at the interface between the fiber and the resin, and forming a multiphase structure by electrospinning or chemical methods; S8.

2. Use electrospinning, voltage 10-30kV, or spraying technology to form a stable bond between the fiber and the resin in the interface reinforcement layer.

Citation Information

Patent Citations

  • Carbon fibre bar containing super fine and preparation thereof

    CN101376736A

  • Integrated fiber post for dental restoration and preparation method thereof

    CN101803958A

  • Double-curing resin matrix for pultrusion process and composite material

    CN101831141A

  • Fiber composite core rod with improved performances for overhead wire and preparation method thereof

    CN102426884A

  • Carbon nano dual-cured resin matrix for pultrusion process and composite of carbon nano dual-cured resin matrix

    CN103965582A