Coupling agent for flame-retardant polyethylene cable material and preparation method thereof

By using coupling agents prepared by amidation reaction in polyethylene cable materials, the compatibility of inorganic flame retardant and polyvinyl matrix is ​​improved and specific functional groups are introduced, the thermal resistance and resistance of polyethylene cable materials at high temperatures is solved. The problem of insufficient combustion performance significantly improves the flame retardancy and mechanical properties of the material, ensuring the stability and safety of the material.

CN118638145BActive Publication Date: 2024-11-26SHANGHAI ZHEYINGHONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411105181.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-26
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing polyethylene cable materials have poor heat resistance and flame retardant properties in high temperature environments, are prone to combustion, and the compatibility of inorganic flame retardants with polyvinyl substrates is poor, affecting the processing performance and material stability.

Method used

Using a method of preparing a coupling agent for flame retardant polyethylene cable material, functional groups are connected to the silane coupling agent through amidation reaction, to improve the interface compatibility between the inorganic flame retardant and the polyethylene matrix, and to introduce two Phenylsulfone, Si-N flame retardant components, long carbon chain and carbon-carbon double bond structure enhances the flame retardant, heat resistance and mechanical properties of the material.

Benefits of technology

The flame retardancy, thermal oxidation resistance and mechanical strength of polyethylene cable materials are significantly improved, the uniform dispersion of inorganic flame retardants and the processing performance of the material are improved, and the long-term stability and safety of the material are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a coupling agent for flame retardant polyethylene cable material and a preparation method thereof, and belongs to the technical field of cable materials. The coupling agent prepared is connected to a functional group on a silane coupling agent KH-550 by an amidation reaction, and is used to prepare a polyethylene cable material, which can improve the interfacial compatibility of an inorganic flame retardant and a polyethylene matrix, and enhance the flame retardancy and smoke suppression performance of the material. In addition, the coupling agent also contains a variety of functional groups, which can enhance the flame retardancy, heat oxidation resistance and mechanical strength of the matrix, and the performance is stable and not easy to fall off. Therefore, the coupling agent prepared by the present invention is applied to polyethylene cable materials, which can greatly enhance the flame retardancy of the material, and the prepared material has good heat oxidation resistance, high mechanical strength, good processability, and long-term stable performance, and has important application value in the technical field of cable materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cable materials, and in particular relates to a coupling agent for flame-retardant polyethylene cable materials and a preparation method thereof. Background Art

[0002] Cables are carriers for transmitting electrical signals and electric currents. The stability of their power supply will directly determine the operating safety of the equipment. At the same time, with the development of electric energy, the application of electrical equipment is becoming more and more popular, and the performance requirements for cable materials are also getting higher and higher. The performance of cable materials directly affects the stability and safety of the entire system.

[0003] Common cable materials on the market include polyethylene, cross-linked polyethylene, polyvinyl chloride, polypropylene, fluoroplastics, chlorinated polyethers, polyamides and silicone rubber, among which polyethylene (PE) is a thermoplastic resin obtained by polymerization of ethylene monomers. Polyethylene has excellent electrical insulation, good processing performance, excellent wear resistance, excellent low temperature resistance, strong chemical stability, low price, and is widely used in the field of cable material technology. However, especially in high temperature environments, the heat resistance and flame retardancy of cable materials become key factors, while ordinary polyethylene cable materials have poor heat resistance and low oxygen index. When encountering high temperature or fire, they are prone to melting, deformation and even burning, which leads to cable function failure and even safety accidents. Therefore, the flame retardant properties of polyethylene need to be enhanced.

[0004] In order to enhance the flame retardant properties of polyethylene cable materials, the usual method is to add flame retardants. In recent years, as the concept of green environmental protection has become more and more popular, inorganic flame retardants have received more and more attention. However, the compatibility of inorganic flame retardants with organic polyethylene matrix is ​​poor, which not only affects the processing performance, but also requires the addition of a large amount of inorganic flame retardants to improve the flame retardant properties of cable materials, which has a great damage to the mechanical properties of cable materials. Therefore, coupling agents are commonly used to modify inorganic flame retardants to improve the compatibility of inorganic flame retardants with the matrix. However, during the processing of cable materials, other functional additives still need to be added to improve the performance of the materials, which will have a great impact on the homogeneity of cable materials. Therefore, it is urgent to solve the above problems to meet the higher requirements in the field of cable material technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a coupling agent for flame retardant polyethylene cable material and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a coupling agent for flame-retardant polyethylene cable material comprises the following steps:

[0008] S1. At room temperature and under nitrogen protection, add 4,4'-diaminodiphenyl sulfone, dimethylvinyl chlorosilane, N,N-dimethylformamide (DMF) and N,N-diisopropylethylamine to a three-necked flask equipped with a stirring device, mix well, heat to 70°C and keep for 6 hours. After the reaction is complete, filter, evaporate under reduced pressure, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 5:3), remove the eluent by rotary evaporation, and dry in vacuo to obtain intermediate 1;

[0009] Under the catalysis of N,N-diisopropylethylamine, 4,4'-diaminodiphenyl sulfone and dimethylvinyl chlorosilane undergo a nucleophilic substitution reaction. By controlling the molar ratio of the two to be close to 1:1 and a slight excess of 4,4'-diaminodiphenyl sulfone, only one amino group on 4,4'-diaminodiphenyl sulfone participates in the reaction to obtain intermediate 1. The specific reaction process is as follows:

[0010]

[0011] S2. Add n-decylamine, dicyclohexylcarbodiimide (DCC, dehydrating agent) and toluene to a three-necked flask equipped with a stirring device, mix and stir evenly, then mix nitrilotriacetic acid and sodium hydroxide solution, stir until the solid is completely dissolved, add to the three-necked flask, place the device in a 35°C water bath, heat in the water bath for 3h, and when the reaction is completed, filter, remove the solvent by vacuum distillation, and dry in vacuo to obtain intermediate 2;

[0012] Under the action of a dehydrating agent, n-decylamine and nitrilotriacetic acid undergo an amidation reaction. By controlling the molar ratio of the two to be close to 1:1 and the nitrilotriacetic acid to be slightly excessive, only one carboxyl group on the nitrilotriacetic acid participates in the reaction to obtain intermediate 2. The specific reaction process is as follows:

[0013]

[0014] S3, in a three-necked flask equipped with a stirring device, the intermediate 2, the intermediate 1, dicyclohexylcarbodiimide and toluene were stirred and mixed uniformly, and then placed in a water bath at 40°C and heated in the water bath for 5 hours. After the reaction was completed, the mixture was filtered and the solvent was removed by vacuum distillation. The mixture was purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 5:1), and the eluent was removed by rotary evaporation to obtain the intermediate 3;

[0015] Under the action of a dehydrating agent, intermediate 2 and intermediate 1 undergo an amidation reaction. By controlling the molar ratio of the two to be close to 1:1 and a slight excess of intermediate 2, only one carboxyl group on intermediate 2 participates in the reaction to obtain intermediate 3. The specific reaction process is as follows:

[0016]

[0017] S4. In a three-necked flask equipped with a stirring device, the intermediate 3, dicyclohexylcarbodiimide, 1-hydroxybenzotriazole (HOBT) and toluene were mixed and stirred for 30 minutes, and then γ-aminopropyltriethoxysilane (silane coupling agent KH-550) was added. The reaction temperature was controlled to 50°C for 8 hours. After the reaction was completed, the solvent was removed by vacuum distillation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 6:1), and the eluent was removed by rotary evaporation to obtain a coupling agent for flame-retardant polyethylene cable materials.

[0018] Under the action of a dehydrating agent, the intermediate 3 and the silane coupling agent KH-550 undergo an amidation reaction to obtain a coupling agent.

[0019] Furthermore, in step S1, the ratio of the amount of 4,4'-diaminodiphenyl sulfone, dimethylvinyl chlorosilane, N,N-dimethylformamide, and N,N-diisopropylethylamine is 25.6 g:11.9 g:100 mL:15 mL.

[0020] Furthermore, in step S2, the ratio of the amount of n-decylamine, dicyclohexylcarbodiimide, toluene, N,N-nitrilotriacetic acid, and sodium hydroxide solution is 15.7 g: 20.6 g: 100 mL: 20.1 g: 50 mL.

[0021] Furthermore, in step S3, the ratio of the amount of intermediate 2, intermediate 1, dicyclohexylcarbodiimide and toluene is 34.4 g: 33.2 g: 20.6 g: 200 mL.

[0022] Furthermore, in step S4, the ratio of the amount of intermediate 3, dicyclohexylcarbodiimide, 1-hydroxybenzotriazole, toluene, and γ-aminopropyltriethoxysilane is 64.4 g: 20.6 g: 13.5 g: 200 mL: 22.1 g.

[0023] Furthermore, the mass fraction of the sodium hydroxide solution in step S2 is 8-12%.

[0024] The coupling agent prepared by the present invention connects functional groups on the silane coupling agent KH-550 through an amidation reaction, and the silane alkoxy group at one end of the coupling agent can react with the oxygen-containing functional group on the surface of the inorganic flame retardant and be grafted on the surface of the inorganic flame retardant. The addition of the coupling agent can greatly improve the interface compatibility between the inorganic flame retardant and the polyethylene matrix, reduce the agglomeration phenomenon of the inorganic flame retardant, and make the inorganic flame retardant uniformly dispersed in the matrix, which not only enhances its processability, but also makes the flame retardant and smoke suppression performance of the inorganic flame retardant fully exerted, greatly enhancing the flame retardant and smoke suppression performance of the matrix; in addition, the coupling agent molecule also contains diphenyl sulfone, Si-N flame retardant components, long carbon chains and carbon-carbon double bond structures, wherein the diphenyl sulfone itself has good heat oxidation resistance, can enhance the heat oxidation resistance of the matrix, and is thermally desulfurized to generate SO2, sulfurous acid and water, which can promote the Fri es rearrangement reaction accelerates the carbonization of the matrix, which can effectively enhance the flame retardant properties of the matrix; not only that, the Si-N flame retardant component has the synergistic flame retardant effect of silicon-based and nitrogen-based flame retardants, and compared with the general silicon-based flame retardants in which silicon and oxygen are directly connected, Si-N is a covalent bond, with stable physical and chemical properties, and is not easy to generate SiO2 during combustion but instead generates a denser Si-C or Si-Si layer, further improving the flame retardant properties of the matrix; the introduced long carbon chain belongs to the methylene chain segment, which has good flexibility, can improve the mechanical strength of the matrix, and can also be inserted into the matrix macromolecular chain to improve stability; finally, the introduced carbon-carbon double bond can cross-link with the matrix, and can form a chemical interface between the inorganic flame retardant and the matrix, and the coupling agent forms a good isolation modification structure between the aluminum hydroxide and the matrix rubber, further improving the compatibility of the inorganic flame retardant with the matrix.

[0025] Beneficial effects of the present invention:

[0026] The coupling agent prepared by the present invention is used to connect functional groups on the silane coupling agent KH-550 through an amidation reaction, and is used to prepare polyethylene cable materials, which can improve the interface compatibility between the inorganic flame retardant and the polyethylene matrix, and enhance the flame retardancy and smoke suppression performance of the material. In addition, the coupling agent also contains a variety of functional groups, which can enhance the flame retardancy, heat oxidation resistance and mechanical strength of the matrix, and the performance is stable and not easy to fall off. Therefore, the coupling agent prepared by the present invention will be applied to polyethylene cable materials, which can greatly enhance the flame retardancy of the material, and the prepared material has good heat oxidation resistance, high mechanical strength, good processability, long-term stable performance, and has important application value in the field of cable material technology. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] Preparation of coupling agent:

[0030] S1. At room temperature, under nitrogen protection, in a three-necked flask equipped with a stirring device, add 25.6 g of 4,4'-diaminodiphenyl sulfone, 11.9 g of dimethylvinyl chlorosilane, 100 mL of N,N-dimethylformamide and 15 mL of N,N-diisopropylethylamine, mix well, heat to 70°C and keep for 6 hours. After the reaction is complete, filter, evaporate under reduced pressure, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 5:3), remove the eluent by rotary evaporation, and dry in vacuo to obtain intermediate 1;

[0031] S2. Add 15.7 g of n-decylamine, 20.6 g of dicyclohexylcarbodiimide and 100 mL of toluene to a three-necked flask equipped with a stirring device, mix and stir evenly, then mix 20.1 g of nitrilotriacetic acid and 50 mL of sodium hydroxide solution (mass fraction 8%), stir until the solid is completely dissolved, add to the three-necked flask, place the device in a 35°C water bath, heat in the water bath for 3 h, complete the reaction, filter, remove the solvent by reduced pressure distillation, and vacuum dry to obtain intermediate 2;

[0032] S3, in a three-necked flask equipped with a stirring device, 34.4 g of intermediate 2, 33.2 g of intermediate 1, 20.6 g of dicyclohexylcarbodiimide and 200 mL of toluene were stirred and mixed uniformly, and then placed in a 40°C water bath, heated in a water bath for 5 h. After the reaction was completed, the mixture was filtered, and the solvent was removed by vacuum distillation. The mixture was then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 5:1), and the eluent was removed by rotary evaporation to obtain intermediate 3;

[0033] S4. In a three-necked flask equipped with a stirring device, 64.4 g of intermediate 3, 20.6 g of dicyclohexylcarbodiimide, 13.5 g of 1-hydroxybenzotriazole and 200 mL of toluene were mixed and stirred for 30 min, and then 22.1 g of γ-aminopropyltriethoxysilane was added. The reaction temperature was controlled to 50 °C for 8 h. After the reaction was completed, the solvent was removed by vacuum distillation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 6:1), and the eluent was removed by rotary evaporation to obtain a coupling agent for flame-retardant polyethylene cable materials.

[0034] Example 2

[0035] Preparation of coupling agent:

[0036] S1. At room temperature, under nitrogen protection, in a three-necked flask equipped with a stirring device, add 51.2 g of 4,4'-diaminodiphenyl sulfone, 23.8 g of dimethylvinyl chlorosilane, 200 mL of N,N-dimethylformamide and 30 mL of N,N-diisopropylethylamine, mix well, heat to 70°C and keep for 6 hours. After the reaction is complete, filter, evaporate under reduced pressure, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 5:3), remove the eluent by rotary evaporation, and dry in vacuo to obtain intermediate 1;

[0037] S2. Add 31.4 g of n-decylamine, 41.2 g of dicyclohexylcarbodiimide and 200 mL of toluene to a three-necked flask equipped with a stirring device, mix and stir evenly, then mix 40.2 g of nitrilotriacetic acid and 100 mL of sodium hydroxide solution (mass fraction 12%), stir until the solid is completely dissolved, add to the three-necked flask, place the device in a 35°C water bath, heat in the water bath for 3 h, complete the reaction, filter, remove the solvent by reduced pressure distillation, and vacuum dry to obtain intermediate 2;

[0038] S3, in a three-necked flask equipped with a stirring device, 68.8g of intermediate 2, 66.4g of intermediate 1, 41.2g of dicyclohexylcarbodiimide and 400mL of toluene were stirred and mixed uniformly, and then placed in a 40°C water bath, heated in a water bath for 5h, the reaction was completed, filtered, and the solvent was removed by vacuum distillation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, and the volume ratio of the two was 5:1), and the eluent was removed by rotary evaporation to obtain intermediate 3;

[0039] S4. In a three-necked flask equipped with a stirring device, 128.8 g of intermediate 3, 41.2 g of dicyclohexylcarbodiimide, 27.0 g of 1-hydroxybenzotriazole and 400 mL of toluene were mixed and stirred for 30 min, and then 44.2 g of γ-aminopropyltriethoxysilane was added. The reaction temperature was controlled to 50 °C for 8 h. After the reaction was completed, the solvent was removed by vacuum distillation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 6:1), and the eluent was removed by rotary evaporation to obtain a coupling agent for flame-retardant polyethylene cable materials.

[0040] Comparative Example

[0041] A commercially available silane coupling agent was used.

[0042] The coupling agent in Example 1 is used as one of the raw materials for preparing cable materials, wherein the amount of the coupling agent is 8g, 12g and 16g respectively, and the prepared cable materials are counted as samples 1-3 respectively. The preparation process is as follows:

[0043] 80g of linear low-density polyethylene, 20g of aluminum hydroxide, 25g of magnesium hydroxide and a weighed coupling agent are added to a high-speed mixer in sequence for mixing. After mixing evenly, they are transferred to a twin-screw plasticator for plasticizing. After plasticizing evenly, they are water-cooled and drawn into strips and pelletized. Then, they are dried in a centrifugal dryer to obtain cable materials.

[0044] The coupling agent of the comparative example is used as one of the raw materials for preparing the cable material to prepare the cable material, and the preparation process of the comparative sample is as follows:

[0045] 80g of linear low-density polyethylene, 20g of aluminum hydroxide, 25g of magnesium hydroxide and 16g of coupling agent are added to a high-speed mixer in sequence for mixing. After mixing evenly, they are transferred to a twin-screw plasticator for plasticizing. After plasticizing evenly, they are water-cooled and drawn into strips and pelletized. Then, they are dried in a centrifugal dryer to obtain cable materials.

[0046] Samples 1-3 and comparative samples were made into corresponding shapes according to different test standards and subjected to the following performance tests:

[0047] The national standard GB / T 2406-2008 "Test method for combustion performance of plastics" was used to measure the limiting oxygen index of the sample before and after being placed at room temperature for 360 days;

[0048] The smoke density is measured using the national standard GB / T 8323.2-2008 "Plastic smoke generation Part 2: Single chamber method for determination of smoke density test method";

[0049] The notched impact strength was determined using the national standard GB / T 1843-2008 "Determination of Izod Impact Strength of Plastics"; the tensile properties of the sample before and after hot air oxidation for 72 hours were determined using the national standard GB / T 1040-2006 "Determination of Tensile Properties of Plastics";

[0050] The measured results are shown in the following table:

[0051]

[0052] It can be seen from the above table that the coupling agent prepared in the embodiment of the present invention can be applied to polyethylene cable materials to greatly enhance the flame retardancy of the material, and the prepared material has good heat and oxidation resistance, high mechanical strength, good processability, and long-term stable performance, and has important application value in the field of cable material technology.

[0053] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0054] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a coupling agent for flame-retardant polyethylene cable materials, characterized in that: The following steps are involved: S1, after 4,4'-diaminodiphenyl sulfone, dimethylvinyl chlorosilane, N,N-dimethylformamide and N,N-diisopropylethylamine are mixed evenly, the temperature is raised to 70°C and kept for reaction for 6 hours. After the reaction is completed, the mixture is filtered, distilled under reduced pressure, purified by column chromatography, rotary evaporated, and dried under vacuum to obtain intermediate 1; The structure of intermediate 1 is shown below: ; S2, n-decylamine, dicyclohexylcarbodiimide and toluene were mixed and stirred evenly, and then nitrilotriacetic acid and sodium hydroxide solution were mixed, and stirred until the solid was completely dissolved, and added to a three-necked flask, and heated in a water bath at 35°C for 3h. After the reaction was completed, the mixture was filtered, distilled under reduced pressure, and dried in vacuo to obtain intermediate 2; The structure of intermediate 2 is shown below: ; S3, after mixing intermediate 2, intermediate 1, dicyclohexylcarbodiimide and toluene evenly, place in a 40°C water bath, heat in the water bath for 5 hours, and when the reaction is complete, filter, distill under reduced pressure, purify by column chromatography, and rotary evaporate to obtain intermediate 3; The structure of intermediate 3 is shown below: ; S4. After the intermediate 3, dicyclohexylcarbodiimide, 1-hydroxybenzotriazole and toluene are mixed and stirred for 30 minutes, γ-aminopropyltriethoxysilane is added and reacted at 50°C for 8 hours. After the reaction is completed, vacuum distillation is performed, column chromatography is used for purification, and rotary evaporation is performed to obtain a coupling agent for flame-retardant polyethylene cable materials.

2. The method for preparing a coupling agent for flame-retardant polyethylene cable material according to claim 1, characterized in that: In step S1, the ratio of 4,4'-diaminodiphenyl sulfone, dimethylvinyl chlorosilane, N,N-dimethylformamide and N,N-diisopropylethylamine is 25.6 g:11.9 g:100 mL:15 mL.

3. The method for preparing a coupling agent for flame-retardant polyethylene cable material according to claim 1, characterized in that: In step S2, the ratio of n-decylamine, dicyclohexylcarbodiimide, toluene, N,N-nitrilotriacetic acid, and sodium hydroxide solution is 15.7 g: 20.6 g: 100 mL: 20.1 g: 50 mL.

4. The method for preparing a coupling agent for flame-retardant polyethylene cable material according to claim 1, characterized in that: In step S3, the ratio of the amount of intermediate 2, intermediate 1, dicyclohexylcarbodiimide and toluene is 34.4 g:33.2 g:20.6 g:200 mL.

5. The method for preparing a coupling agent for flame-retardant polyethylene cable material according to claim 1, characterized in that: In step S4, the ratio of the amount of intermediate 3, dicyclohexylcarbodiimide, 1-hydroxybenzotriazole, toluene, and γ-aminopropyltriethoxysilane is 64.4 g: 20.6 g: 13.5 g: 200 mL: 22.1 g.

6. The method for preparing a coupling agent for flame-retardant polyethylene cable material according to claim 1, characterized in that: The mass fraction of the sodium hydroxide solution in step S2 is 8-12%.

7. A coupling agent for flame retardant polyethylene cable material, characterized in that: Prepared according to the method according to any one of claims 1 to 6.