Nano-ceramic reinforced polypropylene hollow wall winding tube and preparation method thereof
By optimizing the formulation and process, nano-ceramic-reinforced polypropylene hollow-wall spiral tubes were prepared, solving the problems of insufficient heat resistance and impact resistance, and achieving efficient performance improvement and cost control.
Patent Information
- Application Number
- CN202411116882.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Existing polypropylene hollow wall spiral pipes have shortcomings in terms of heat resistance and cost, and their impact resistance needs to be improved.
By rationally proportioning polypropylene, nano-ceramics, modifying agents, and other auxiliary materials, a specific process is used to prepare nano-ceramic reinforced polypropylene hollow wall wound tubes, including mixing, extrusion, winding, and cooling processes. Cucurbita-dicarboxylic acid complex and zinc stearate-modified nano-silicon carbide are introduced to promote β-crystal formation and dispersion.
It significantly improves the heat resistance, ring stiffness, and impact resistance of polypropylene hollow wall spiral pipes, while reducing production costs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pipelines, and in particular to a nano-ceramic reinforced polypropylene hollow wall winding pipe and a preparation method thereof. Background Art
[0002] Drain pipes are connected by pipes, pipe connectors and valves, and are used to transport liquids. They are mainly used for municipal drainage, outdoor drainage of buildings, buried farmland drainage, industrial sewage, road drainage, sewage treatment plants, drainage of sports fields and squares, and electrical and telecommunications projects. Traditional drainage pipes are mainly cement pipes and clay pipes, which generally have defects such as heavy weight, high production energy consumption and cost, poor chemical and corrosion resistance, short service life, and easy to cause environmental pollution. Based on the defects of traditional pipes, R&D personnel have been developing special materials for plastic pipes and the production process of plastic pipes.
[0003] Polypropylene hollow wall winding pipe is a pipe made of polypropylene (PP) as the main raw material, adding appropriate amounts of polyethylene, reinforcing materials, modifying additives and filling auxiliary materials, and made through advanced winding molding process. The pipe molding process includes extrusion molding and winding molding. First, the polypropylene resin and other auxiliary materials are extruded into a rectangular tube blank by an extruder, and then wound and welded on a special winding machine. Due to its unique molding process, the pipe has a uniform wall thickness and a high-strength ring structure. As a new type of chemical building material, polypropylene hollow wall winding pipe has the advantages of light weight, high strength and high rigidity, corrosion resistance, smooth pipe wall, and large flow capacity, so it has been widely used in municipal engineering, agricultural irrigation, industrial sewage, communication cable protection and other fields.
[0004] Chinese patent CN112793117A discloses a high modulus impact-resistant hollow wall winding tube and its preparation method. The winding tube is made of the following materials by weight: 0.5-15 parts of copolymer, 10-20 parts of reinforcing masterbatch, 1-3 parts of coloring masterbatch, 15-20 parts of melt adhesive material and 60-99 parts of matrix material; the matrix material is made of polyethylene, block copolymer polypropylene, polypropylene, and antioxidant materials after being mixed and then extruded and granulated by a single screw. In the impact performance test, the hollow wall winding tube provided by the invention has a real impact rate of less than or equal to 5%, and the ring stiffness is increased by 1 level. Although the hollow wall winding tube has excellent impact resistance, its heat resistance stability is poor and the cost is high. Summary of the invention
[0005] In view of the above-mentioned defects of the prior art, the present invention provides a nano-ceramic reinforced polypropylene hollow wall winding tube, which overcomes the shortcomings of the existing polypropylene hollow wall winding tube by rationally proportioning the raw material formula of the polypropylene hollow wall winding tube and strictly debugging the preparation process conditions, significantly improves the heat resistance stability and ring rigidity of the polypropylene hollow wall winding tube, and improves the impact resistance and compression resistance of the product. The preparation method of the polypropylene hollow wall winding tube of the present invention is simple, low in cost, short in preparation cycle, has no special requirements for equipment, and is very suitable for industrial production.
[0006] The present invention provides a method for preparing a nano-ceramic reinforced polypropylene hollow wall winding tube, comprising the following steps:
[0007] (1) Mix polypropylene, high-density polyethylene, modification additives, and antioxidants in a high-speed mixer at 1000-1500 r / min for 5-10 minutes; then add the filling auxiliary materials and continue to mix and stir for 5-10 minutes; then add the nano-ceramics and continue to mix and stir for 3-8 minutes to obtain a mixture;
[0008] (2) placing the mixed material obtained in step (1) in a single screw extruder, and extruding it through a special mold at a temperature of 190-220° C. to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube blank; and vacuum cooling the obtained blank to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube;
[0009] (3) The nano-ceramic reinforced polypropylene hollow rectangular tube obtained in step (2) is sent into a winding device for spiral winding, and hot air with a temperature of 330-350° C. is delivered to the winding fusion position by a blower for heating, and the fusion connection is extruded at the same time; then the nano-ceramic reinforced polypropylene hollow rectangular tube after the fusion connection is cooled by cooling water with a temperature of 15-20° C. to obtain a semi-finished wound tube; the semi-finished wound tube is cut to a fixed length to obtain a finished wound tube.
[0010] Preferably, the modification aid is a cucurbituril-diacid complex, and the preparation method thereof comprises the following steps, calculated by weight:
[0011] 0.2-0.5 parts of cucurbituril hydrate and 0.1-0.3 parts of dibasic acid are added to 10-20 parts of water, and then stirred at room temperature for 10-12 hours to obtain a mixed solution; the mixed solution is allowed to stand for 22-24 hours, and then filtered to collect the precipitate, and the precipitate is vacuum dried to obtain a cucurbituril-dibasic acid complex.
[0012] More preferably, the dibasic acid is selected from one of suberic acid, pimelic acid and oxalic acid.
[0013] Cucurbituril has a specific cavity structure, and dibasic acid can interact with cucurbituril through non-covalent bonds to form a stable inclusion complex, namely cucurbituril-dibasic acid complex. This structural feature helps dibasic acid to form an orderly arrangement in the cavity of cucurbituril, thereby providing a template for the crystallization of polypropylene molecules, which may guide the polypropylene molecular chains to be arranged more orderly around the cucurbituril-dibasic acid complex, thereby facilitating the formation of polymer crystals with β-crystal form. In addition, the formation of cucurbituril-dibasic acid complex provides active sites for polypropylene molecules, increases the heterogeneous nucleation points of polypropylene, and promotes the formation of β-crystal form of polypropylene. Compared with the α-crystal form of polypropylene, the β-crystal form has a higher melting point and a tighter molecular arrangement, which can increase the energy required for thermal decomposition and is beneficial to improving the thermal stability of polypropylene. At the same time, the β-crystal form has better mechanical properties, which may enhance the impact performance of polypropylene hollow winding tubes by improving the local deformation ability and energy absorption ability of the material. Therefore, the introduction of cucurbituril-dibasic acid complex can effectively improve the ring rigidity, impact resistance, compressive resistance and heat stability of polypropylene hollow winding tubes. Compared with pimelic acid and oxalic acid, suberic acid has a longer carbon chain. During the mixing process with cucurbituril, the carbon chain length of suberic acid may provide the best balance between flexibility and rigidity, helping to form a more stable complex, thereby more effectively promoting the formation of β-crystal.
[0014] Preferably, the weight ratio of each raw material component is:
[0015] 60-80 parts of polypropylene, 55-65 parts of high-density polyethylene, 5-8 parts of nano-ceramics, 2-5 parts of modification aids, 1-3 parts of antioxidants, and 10-20 parts of filling auxiliary materials.
[0016] Preferably, the nano-ceramic is modified nano-silicon carbide, and its preparation method comprises the following steps, measured by weight:
[0017] Add 3-5 parts of zinc stearate to 50-80 parts of ethanol aqueous solution with a volume concentration of 25-35%, then add 20-30 parts of nano-silicon carbide, mix and stir for 1-2 hours at 70-90°C and 200-300r / min, filter and dry to obtain modified nano-silicon carbide.
[0018] Nano silicon carbide has heterogeneous nucleation activity, which can effectively improve the crystallization performance of polypropylene molecules, and is conducive to improving the ring rigidity, impact resistance and compressive resistance of polypropylene hollow winding tubes. However, due to its high surface energy, it is easy to produce agglomeration phenomenon, which makes it impossible to be evenly dispersed in the polymer matrix. Excessive introduction is easy to cause disordered crystal growth, affecting the crystallization of polypropylene. The application uses zinc stearate to modify the surface of nano silicon carbide. The long-chain molecules of zinc stearate grafted to the surface of nano silicon carbide can act as "steric hindrance" to reduce the direct contact between nano silicon carbide particles, thereby reducing the agglomeration phenomenon. At the same time, the carboxyl group of zinc stearate can form a chemical bond or hydrogen bond with the hydroxyl group on the surface of nano silicon carbide, which helps to enhance the interfacial bonding force between nano silicon carbide and polypropylene, making it easier for the polymer matrix to wrap nano particles, improve the dispersibility of nano silicon carbide in the polypropylene matrix, and form a more uniform dispersion system. In addition, the introduction of zinc stearate may also prevent the polymer from thermal degradation during processing, thereby maintaining the molecular weight and performance of the polymer, which is conducive to improving the thermal stability of the polymer matrix. Therefore, using zinc stearate to modify nano-silicon carbide is beneficial to reducing agglomeration, improving the uniform dispersion of nano-silicon carbide in the polymer matrix, promoting the crystallization of polypropylene, and thus helping to improve the ring rigidity, impact resistance and compression resistance of polypropylene hollow winding tubes.
[0019] Preferably, the antioxidant is selected from one or more combinations of hindered phenol antioxidants, phosphite antioxidants, and sulfur-containing antioxidants; the hindered phenol antioxidant is selected from antioxidants with models 1010 and 1076; the phosphite antioxidant is selected from antioxidants with models 168, 626, and 618; the sulfur-containing antioxidant is selected from antioxidants with models DLTDP, DSTDP, DMTDP, and DTDTP.
[0020] Preferably, the filling auxiliary material is selected from one of montmorillonite, calcium carbonate, talc and mica.
[0021] Preferably, the step (1) can also be: mixing the nanocellulose with an ethanol aqueous solution having a volume concentration of 25-35% at a mass ratio of nanocellulose to ethanol aqueous solution of 1:5, then adding a modification aid, mixing and stirring at 80-90°C and 200-300r / min for 1-2h; then drying at 50-60°C for 1-2h to obtain a mixture; then mixing and stirring the mixture, polypropylene, high-density polyethylene, and an antioxidant in a high-speed mixer at 1000-1500 r / min for 5-10min; then adding a filling auxiliary material and continuing to mix and stir for 5-10min; then adding nanoceramics and continuing to mix and stir for 3-8min to obtain a mixture.
[0022] Further preferably, the weight ratio of each raw material component is:
[0023] 60-80 parts of polypropylene, 55-65 parts of high-density polyethylene, 5-8 parts of nano-ceramics, 2-5 parts of modification aids, 8-15 parts of nano-fibers, 1-3 parts of antioxidants, and 10-20 parts of filling auxiliary materials.
[0024] The present invention also provides a nano-ceramic reinforced polypropylene hollow wall winding tube, which is prepared by the above method.
[0025] In the present invention, the addition of high-density polyethylene can improve the flexibility and environmental stress cracking resistance of the pipe, and after being blended with polypropylene and modified nano-silicon carbide, the rigidity and deformation resistance of the pipe can be improved, thereby optimizing the comprehensive performance of the pipe.
[0026] In the present invention, antioxidant 1076 can improve the heat resistance stability and oxidation resistance of the pipe, extend the service life of the pipe, and the coordinated use with modified nano silicon carbide and cucurbituril-suberic acid composite is beneficial to further improve the heat resistance stability of the pipe.
[0027] In the present invention, talcum powder is used as a filler to reduce costs, and its flaky structure helps to improve the rigidity and pressure resistance of the pipe. The coordinated use with modified nano silicon carbide is conducive to further improving the compressive strength of the pipe.
[0028] Beneficial effects of the present invention:
[0029] 1. Compared with the prior art, the present invention uses polypropylene, high-density polyethylene, modified nano-silicon carbide, cucurbituril-diacid complex, nano-cellulose, antioxidant and talcum powder as raw materials to prepare polypropylene hollow wall wound tubes. By reasonably proportioning the raw materials and optimizing the production process conditions, the prepared hollow wall wound tubes have excellent ring rigidity, impact resistance, compression resistance and heat stability.
[0030] 2. Compared with the prior art, the present invention modifies nano silicon carbide by zinc stearate to reduce its agglomeration phenomenon, improves the uniform dispersion of nano silicon carbide in the polymer matrix, is conducive to promoting the crystallization of polypropylene, and enhances the filler to improve the ring rigidity and compression resistance of the pipe. Suberic acid and cucurbituril are mixed to form a stable cucurbituril-suberic acid complex as a modification aid to promote the crystallization of polypropylene, improve crystallinity and thermal stability, thereby increasing the heat resistance stability of the pipe. At the same time, nano cellulose is introduced to mix with the cucurbituril-suberic acid complex, and the hydroxyl group in the nano cellulose can interact with the carboxyl group in the cucurbituril-suberic acid complex to form a hydrogen bond, thereby improving the dispersibility of the cucurbituril-diacid complex in the polypropylene matrix, which is conducive to improving the impact resistance, compression resistance and heat resistance stability of the polypropylene hollow winding tube. The present invention uses zinc stearate modified nano silicon carbide, cucurbituril-suberic acid complex and nano cellulose in a coordinated manner to jointly promote the improvement of the ring rigidity, impact resistance, compression resistance and heat resistance stability of the hollow wall winding tube. DETAILED DESCRIPTION
[0031] Parameters for specific chemical substances used, sources.
[0032] Polypropylene, grade 4220, brand: Yanshan Petrochemical;
[0033] High-density polyethylene, grade 5000S, brand: Yangzi Petrochemical;
[0034] Nano silicon carbide, purity: 99%, manufacturer: Shanghai Myrel Biochemical Technology Co., Ltd., item number: M16310, particle size: 40nm;
[0035] Nanocellulose, purity: 99.5%, produced by Wuhan Huaxiang Kejie Biotechnology Co., Ltd., particle size: 40nm;
[0036] Talc, purity: 99%, 325 mesh, manufacturer: Shanghai Myril Biochemical Technology Co., Ltd., item number: C0500540023.
[0037] Example 1
[0038] A method for preparing a nano-ceramic reinforced polypropylene hollow wall winding tube comprises the following steps:
[0039] (1) 10 parts by weight of nanocellulose and 30% ethanol aqueous solution were mixed in a mass ratio of nanocellulose to ethanol aqueous solution of 1:5, and then 3 parts by weight of a modification aid were added, and the mixture was mixed and stirred at 85°C and 300 r / min for 1.5 hours; then dried at 55°C for 2 hours to obtain a mixture; then the mixture, 75 parts by weight of polypropylene, 60 parts by weight of high-density polyethylene, and 1.5 parts by weight of antioxidant 1076 were mixed and stirred in a high-speed mixer at 1300 r / min for 8 minutes; then 18 parts by weight of talc was added and the mixture was continued to be mixed and stirred for 8 minutes; then 6 parts by weight of modified nano silicon carbide was added and the mixture was continued to be mixed and stirred for 5 minutes to obtain a mixture;
[0040] (2) placing the mixed material obtained in step (1) in a single screw extruder, and extruding it through a special mold at a temperature of 210° C. to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube blank; and vacuum cooling the obtained blank to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube;
[0041] (3) The nano-ceramic reinforced polypropylene hollow rectangular tube obtained in step (2) is sent into a winding device for spiral winding, and hot air at a temperature of 335° C. is delivered to the winding fusion position by a blower for heating, and the fusion connection is extruded at the same time; then the nano-ceramic reinforced polypropylene hollow rectangular tube after the fusion connection is cooled by cooling water at a temperature of 16° C. to obtain a semi-finished wound tube; the semi-finished wound tube is cut to a fixed length to obtain a finished wound tube.
[0042] The modification aid is a cucurbituril-suberic acid complex, and its preparation method comprises the following steps:
[0043] 0.25 parts by weight of cucurbituril hydrate and 0.12 parts by weight of suberic acid were added to 15 parts by weight of water, and then stirred at room temperature for 11 hours to obtain a mixed solution; the mixed solution was allowed to stand for 23 hours, and then filtered to collect the precipitate, and the precipitate was vacuum dried to obtain a cucurbituril-suberic acid complex.
[0044] The preparation method of the modified nano-silicon carbide comprises the following steps:
[0045] 4 parts by weight of zinc stearate were added to 60 parts by weight of 30% ethanol aqueous solution, and then 22 parts by weight of nano-silicon carbide were added. The mixture was mixed and stirred at 80° C. and 250 r / min for 1.5 h, filtered, and dried to obtain modified nano-silicon carbide.
[0046] Example 2
[0047] A method for preparing a nano-ceramic reinforced polypropylene hollow wall winding tube, which is different from Example 1 in that the modification auxiliary agent is a cucurbituril-pimelic acid complex, and the preparation method comprises the following steps:
[0048] 0.25 parts by weight of cucurbituril hydrate and 0.12 parts by weight of pimelic acid were added to 15 parts by weight of water, and then stirred at room temperature for 11 hours to obtain a mixed solution; the mixed solution was allowed to stand for 23 hours, and then filtered to collect the precipitate, and the precipitate was vacuum dried to obtain a cucurbituril-pimelic acid complex.
[0049] Example 3
[0050] A method for preparing a nano-ceramic reinforced polypropylene hollow wall winding tube, which is different from Example 1 in that the modification auxiliary agent is a cucurbituril-oxalic acid complex, and the preparation method comprises the following steps:
[0051] 0.25 parts by weight of cucurbituril hydrate and 0.12 parts by weight of oxalic acid were added to 15 parts by weight of water, and then stirred at room temperature for 11 hours to obtain a mixed solution; the mixed solution was allowed to stand for 23 hours, and then filtered to collect the precipitate, and the precipitate was vacuum dried to obtain a cucurbituril-oxalic acid complex.
[0052] Example 4
[0053] A method for preparing a nano-ceramic reinforced polypropylene hollow wall winding tube comprises the following steps:
[0054] 75 parts by weight of polypropylene, 60 parts by weight of high-density polyethylene, 3 parts by weight of a modifying aid, and 1.5 parts by weight of an antioxidant 1076 were mixed and stirred in a high-speed mixer at 1300 r / min for 8 minutes; then 18 parts by weight of talcum powder were added and the mixture was continued to be mixed and stirred for 8 minutes; then 6 parts by weight of modified nano-silicon carbide were added and the mixture was continued to be mixed and stirred for 5 minutes to obtain a mixture;
[0055] (2) placing the mixed material obtained in step (1) in a single screw extruder, and extruding it through a special mold at a temperature of 210° C. to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube blank; and vacuum cooling the obtained blank to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube;
[0056] (3) The nano-ceramic reinforced polypropylene hollow rectangular tube obtained in step (2) is sent into a winding device for spiral winding, and hot air at a temperature of 335° C. is delivered to the winding fusion position by a blower for heating, and the fusion connection is extruded at the same time; then the nano-ceramic reinforced polypropylene hollow rectangular tube after the fusion connection is cooled by cooling water at a temperature of 16° C. to obtain a semi-finished wound tube; the semi-finished wound tube is cut to a fixed length to obtain a finished wound tube.
[0057] The modification aid is a cucurbituril-suberic acid complex, and its preparation method is the same as that in Example 1.
[0058] The preparation method of the modified nano-silicon carbide is consistent with that of Example 1.
[0059] Comparative Example 1
[0060] A method for preparing a polypropylene hollow wall wound tube comprises the following steps:
[0061] (1) 10 parts by weight of nanocellulose and 30% ethanol aqueous solution were mixed in a mass ratio of nanocellulose to ethanol aqueous solution of 1:5, and then 3 parts by weight of a modification aid were added, and the mixture was mixed and stirred at 85°C and 300 r / min for 1.5 hours; then dried at 55°C for 2 hours to obtain a mixture; then the mixture, 75 parts by weight of polypropylene, 60 parts by weight of high-density polyethylene, and 1.5 parts by weight of antioxidant 1076 were mixed and stirred in a high-speed mixer at 1300 r / min for 8 minutes; then 18 parts by weight of talc were added and the mixture was mixed and stirred for 8 minutes to obtain a mixture;
[0062] (2) placing the mixed material obtained in step (1) in a single screw extruder, and extruding it through a special mold at a temperature of 210° C. to obtain a polypropylene hollow rectangular tube blank; and vacuum cooling the obtained blank to obtain a polypropylene hollow rectangular tube;
[0063] (3) The polypropylene hollow rectangular tube obtained in step (2) is sent to a winding device for spiral winding, and hot air at a temperature of 335° C. is sent to the winding fusion position by a blower for heating, and the fusion connection is extruded at the same time; then the polypropylene hollow rectangular tube after the fusion connection is cooled by cooling water at a temperature of 16° C. to obtain a semi-finished wound tube; the semi-finished wound tube is cut to a fixed length to obtain a finished wound tube.
[0064] The modification aid is a cucurbituril-suberic acid complex, and its preparation method is the same as that in Example 1.
[0065] Comparative Example 2
[0066] A method for preparing a nano-ceramic reinforced polypropylene hollow wall winding tube comprises the following steps:
[0067] (1) 75 parts by weight of polypropylene, 60 parts by weight of high-density polyethylene, 10 parts by weight of nanocellulose, and 1.5 parts by weight of antioxidant 1076 were mixed and stirred in a high-speed mixer at 1300 r / min for 8 minutes; then 18 parts by weight of talc were added and the mixture was continued to be mixed and stirred for 8 minutes; then 6 parts by weight of modified nano-silicon carbide were added and the mixture was continued to be mixed and stirred for 5 minutes to obtain a mixture;
[0068] (2) placing the mixed material obtained in step (1) in a single screw extruder, and extruding it through a special mold at a temperature of 210° C. to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube blank; and vacuum cooling the obtained blank to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube;
[0069] (3) The nano-ceramic reinforced polypropylene hollow rectangular tube obtained in step (2) is sent into a winding device for spiral winding, and hot air at a temperature of 335° C. is delivered to the winding fusion position by a blower for heating, and the fusion connection is extruded at the same time; then the nano-ceramic reinforced polypropylene hollow rectangular tube after the fusion connection is cooled by cooling water at a temperature of 16° C. to obtain a semi-finished wound tube; the semi-finished wound tube is cut to a fixed length to obtain a finished wound tube.
[0070] The preparation method of the modified nano-silicon carbide is consistent with that of Example 1.
[0071] Comparative Example 3
[0072] A method for preparing a nano-ceramic reinforced polypropylene hollow wall winding tube, which differs from Example 1 in that 6 parts by weight of modified nano-silicon carbide in step (1) is replaced by 6 parts by weight of nano-silicon carbide.
[0073] Test Example 1
[0074] Hollow wall spiral wound pipe performance test
[0075] According to the standard of GB / T 14152-2001 Test method for external impact resistance of thermoplastic plastic pipes - clockwise rotation method, the hollow wall wound pipes prepared in Examples 1-4 and Comparative Examples 1-3 of the present invention were subjected to a drop hammer impact test, and the true impact rate TIR (%) of the hollow wall wound pipes in each Example and Comparative Example was calculated, wherein the maximum allowable value of the true impact rate TIR (%) is 10%. The calculation formula of the true impact rate TIR (%) is as follows:
[0076] True impact rate TIR = (total number of impact failures / total number of samples) × 100%
[0077] The test results are shown in Table 1.
[0078] The ring stiffness of the hollow wall wound pipes prepared in Examples 1-4 and Comparative Examples 1-3 of the present invention was tested according to the standard "GB / T9647-2015 Determination of Ring Stiffness of Thermoplastic Plastic Pipes", wherein the standard value of the ring stiffness S is not less than 8. The test results are shown in Table 1.
[0079] According to the standard "GB / T18742.2-2017 Polypropylene Pipe System for Hot and Cold Water", the hollow wall wound pipes prepared in Examples 1-4 of the present invention and Comparative Examples 1-3 were subjected to hydrostatic strength tests and thermal stability tests under hydrostatic conditions. The test results are shown in Table 2.
[0080] Table 1
[0081] True impact rate (%) <![CDATA[Ring stiffness (kN / m 2 )]]> Example 1 2 9.68 Example 2 3 9.55 Example 3 3 9.47 Example 4 5 9.11 Comparative Example 1 10 8.23 Comparative Example 2 9 8.42 Comparative Example 3 8 8.68
[0082] Table 2
[0083]
[0084] From the test results of Table 1 and Table 2, it can be seen that the true impact rate of the polypropylene hollow winding tube prepared by Examples 1-4 of the present invention is less than 10%, the ring stiffness is greater than 8, and there is no cracking or leakage in the hydrostatic strength test and the thermal stability test under the hydrostatic state, which meets the standard requirements, indicating that the polypropylene hollow winding tube prepared by Examples 1-4 has good ring stiffness, impact resistance, pressure resistance and thermal stability. Comparing Examples 1-4 and Comparative Examples 1-3, it is found that the true impact rate of the polypropylene hollow winding tube prepared by Examples 1-4 of the present invention is significantly lower than that of Comparative Examples 1-3, among which Example 1 is as low as 2%; the ring stiffness of the polypropylene hollow winding tube prepared by Examples 1-4 is significantly higher than that of Comparative Examples 1-3, among which Example 1 is as high as 9.68; Examples 1-4 show no cracking or leakage in the hydrostatic strength test and the thermal stability test under the hydrostatic state, which is significantly better than Comparative Examples 1-3.
[0085] Comparing Examples 1-4 with Comparative Example 2, it is found that the cucurbituril-diacid complex can improve the impact resistance, compression resistance and heat stability of the polypropylene hollow winding tube, among which the cucurbituril-suberic acid complex has a more obvious improvement effect on the polypropylene hollow winding tube. Comparing Examples 1-3 with Example 4, it is found that the introduction of nanocellulose and the cucurbituril-diacid complex mixed, the hydroxyl group in the nanocellulose can interact with the carboxyl group in the cucurbituril-diacid complex to form a hydrogen bond, which is beneficial to improve the dispersibility of the cucurbituril-diacid complex in the polypropylene matrix, and is beneficial to improve the impact resistance, compression resistance and heat stability of the polypropylene hollow winding tube.
[0086] By comparing Examples 1-3, Comparative Example 1 and Comparative Example 3, it was found that the introduction of nano-silicon carbide can effectively improve the ring stiffness and impact resistance of the polypropylene hollow winding tube, and on the basis of nano-silicon carbide, zinc stearate is used to modify the nano-silicon carbide to increase its compatibility with the polymer matrix, making the nano-silicon carbide easier to be wrapped by the polymer matrix, reducing the agglomeration phenomenon, and improving the dispersion of nano-silicon carbide in the polypropylene matrix. Therefore, the addition of modified nano-silicon carbide makes the ring stiffness and impact resistance of the prepared polypropylene hollow winding tube significantly better than those of the polypropylene hollow winding tube using unmodified nano-silicon carbide.
Claims
1. A method for preparing a nano-ceramic reinforced polypropylene hollow wall winding tube, It is characterized in that The following steps are involved: (1) Mix polypropylene, high-density polyethylene, modification additives, and antioxidants in a high-speed mixer at 1000-1500 r / min for 5-10 minutes; then add the filling auxiliary materials and continue to mix and stir for 5-10 minutes; then add the nano-ceramics and continue to mix and stir for 3-8 minutes to obtain a mixture; Alternatively, nanocellulose is mixed with an ethanol aqueous solution having a volume concentration of 25-35% at a mass ratio of nanocellulose to ethanol aqueous solution of 1:5, and then a modification aid is added, and the mixture is mixed and stirred at 80-90° C. and 200-300 r / min for 1-2 hours; then dried at 50-60° C. for 1-2 hours to obtain a mixture; the mixture, polypropylene, high-density polyethylene, and an antioxidant are mixed and stirred in a high-speed mixer at 1000-1500 r / min for 5-10 minutes; then a filling auxiliary material is added and the mixture is mixed and stirred for 5-10 minutes; then nano-ceramics are added and the mixture is mixed and stirred for 3-8 minutes to obtain a mixture; (2) placing the mixed material obtained in step (1) in a single screw extruder, and extruding it through a special mold at a temperature of 190-220° C. to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube blank; and vacuum cooling the obtained blank to obtain a nano-ceramic reinforced polypropylene hollow rectangular tube; (3) The nano-ceramic reinforced polypropylene hollow rectangular tube obtained in step (2) is sent into a winding device for spiral winding, and hot air at a temperature of 330-350° C. is sent to the winding fusion position by a blower for heating, and the fusion connection is extruded at the same time; then the nano-ceramic reinforced polypropylene hollow rectangular tube after the fusion connection is cooled by cooling water at a temperature of 15-20° C. to obtain a semi-finished winding tube; the semi-finished winding tube is cut to a fixed length to obtain a finished winding tube; The weight proportion of each raw material component is: Polypropylene 60-80 parts, high-density polyethylene 55-65 parts, nano-ceramics 5-8 parts, modification additives 2-5 parts, antioxidants 1-3 parts, filling auxiliary materials 10-20 parts; Or, 60-80 parts of polypropylene, 55-65 parts of high-density polyethylene, 5-8 parts of nano-ceramics, 2-5 parts of modification aids, 8-15 parts of nano-cellulose, 1-3 parts of antioxidants, and 10-20 parts of filling auxiliary materials; The nano-ceramic is modified nano-silicon carbide, and its preparation method comprises the following steps, calculated by weight: Add 3-5 parts of zinc stearate to 50-80 parts of ethanol aqueous solution with a volume concentration of 25-35%, then add 20-30 parts of nano-silicon carbide, mix and stir for 1-2 hours at 70-90° C. and 200-300 r / min, filter, and dry to obtain modified nano-silicon carbide; The modification aid is a cucurbituril-diacid complex, and its preparation method The method comprises the following steps, measured by weight: 0.2-0.5 parts of cucurbituril hydrate and 0.1-0.3 parts of dibasic acid are added to 10-20 parts of water, and then stirred at room temperature for 10-12 hours to obtain a mixed solution; the mixed solution is allowed to stand for 22-24 hours, and then filtered to collect the precipitate, and the precipitate is vacuum dried to obtain a cucurbituril-dibasic acid complex; The dibasic acid is selected from one of suberic acid, pimelic acid and oxalic acid.
2. The method for preparing the nano-ceramic reinforced polypropylene hollow wall winding tube according to claim 1, Features: The antioxidant is selected from one or more combinations of hindered phenol antioxidants, phosphite antioxidants, and sulfur-containing antioxidants; the hindered phenol antioxidant is selected from antioxidants with models 1010 and 1076; the phosphite antioxidant is selected from antioxidants with models 168, 626, and 618; the sulfur-containing antioxidant is selected from antioxidants with models DLTDP, DSTDP, DMTDP, and DTDTP.
3. The method for preparing the nano-ceramic reinforced polypropylene hollow wall winding tube according to claim 1, Features: The filling auxiliary material is selected from one of montmorillonite, calcium carbonate, talc and mica.
4. A nano-ceramic reinforced polypropylene hollow wall winding tube, Features: Prepared by the method according to any one of claims 1 to 3.