Damping rubber strip for railway metal sound barrier and its preparation process and application

By using damping rubber strips with an inner and outer structure in the railway metal sound barrier, combined with copolymers and filler modification technologies with different melt indexes, the problem of insufficient toughness and aging resistance of the damping rubber strips is solved, and a higher service life is achieved. and adaptability.

CN118638368BActive Publication Date: 2024-10-22HEBEI XINGCHEN ENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411102802.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-22
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The damping rubber used for railway metal sound barriers has poor toughness and aging resistance, causing it to be easily damaged and have a short lifespan during use.

Method used

It adopts a foam rubber layer and a solid rubber layer structure from the inside to the outside, introduces acrylonitrile-styrene-acrylate copolymers with different melt indexes, and modifies the filler with 4-vinyl benzoic acid to improve the filler's performance. The degree of dispersion and bonding can produce damping rubber strips with high toughness and aging resistance.

Benefits of technology

The toughness and aging resistance of the damping rubber strips are significantly improved, the service life is extended, and it is suitable for arbitrary-shaped connections in railway metal sound barriers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the field of damping rubber technology, and proposes a damping rubber strip for railway metal sound barrier and its preparation process and application. The damping rubber strip includes a foamed rubber layer and a solid rubber layer arranged in sequence from the inside to the outside; the raw material of the solid rubber layer includes the following components in parts by weight: ethylene propylene rubber, a first copolymer, polyethylene glycol, a filler, a vulcanizing agent, an antioxidant, a vulcanizing aid, a plasticizer, and a defoaming agent; the raw material of the foamed rubber layer includes the following components in parts by weight: ethylene propylene rubber, a second copolymer, polyethylene glycol, a filler, a foaming agent, a vulcanizing agent, an antioxidant, a vulcanizing aid, and a plasticizer; the first copolymer and the second copolymer are each independently acrylonitrile-styrene-acrylate copolymer. Through the above technical scheme, the problem of poor toughness and aging resistance of the damping rubber strip in the related art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of damping rubber, and in particular to a damping rubber strip for a railway metal sound barrier and a preparation process and application thereof. Background Art

[0002] With the rapid development of my country's high-speed railways, sound barriers have been widely used on railways and roads in various countries around the world. Railway metal sound barriers can greatly reduce the noise hazards caused by the pulsating force and high noise generated by high-speed trains to residents near the railway. Most sound barriers use elastic connections, that is, rubber parts are added between the sound absorbing and insulating units of the sound barriers. The shock-absorbing, buffering and damping properties of rubber are used to absorb the pulsating force generated by high-speed train travel, prevent the resonance of the sound barrier wall, and increase the service life of the sound barrier. However, the damping rubber used for railway metal sound barriers still has the problems of insufficient toughness and poor aging resistance.

[0003] Therefore, obtaining a high-toughness, aging-resistant damping rubber strip will be of great significance for the application of rubber products in railway metal sound barriers. Summary of the invention

[0004] The present invention provides a damping rubber strip for a railway metal sound barrier and a preparation process and application thereof, which solves the problem of poor toughness and aging resistance of the damping rubber strip in the related art.

[0005] The technical solution of the present invention is as follows:

[0006] The present invention provides a damping rubber strip for a railway metal sound barrier, comprising a foam rubber layer and a solid rubber layer arranged in sequence from the inside to the outside;

[0007] The raw materials of the solid rubber layer include the following components in parts by weight: 80-90 parts of EPDM rubber, 6-10 parts of the first copolymer, 4-8 parts of polyethylene glycol, 10-15 parts of filler, 2-4 parts of vulcanizer, 1-1.5 parts of antioxidant, 2-4 parts of vulcanizing aid, 2-4 parts of plasticizer, and 1-3 parts of defoaming agent;

[0008] The raw materials of the foam rubber layer include the following components in parts by weight: 80-90 parts of EPDM rubber, 8-12 parts of the second copolymer, 4-8 parts of polyethylene glycol, 10-15 parts of filler, 4-8 parts of foaming agent, 2-4 parts of vulcanizing agent, 1-1.5 parts of antioxidant, 2-4 parts of vulcanizing aid, and 2-4 parts of plasticizer;

[0009] The first copolymer and the second copolymer are each independently an acrylonitrile-styrene-acrylate copolymer.

[0010] As a further technical solution, the melt index of the acrylonitrile-styrene-acrylate copolymer is 5-21 g / 10 min.

[0011] As a further technical solution, the melt index of the first copolymer is 5-15 g / 10 min.

[0012] As a further technical solution, the melt index of the second copolymer is greater than 15 g / 10 min.

[0013] In the present invention, by introducing acrylonitrile-styrene-acrylate copolymers with different melting indexes into the foamed rubber layer and the solid rubber layer respectively, the toughness and aging resistance of the damping rubber strip are further improved.

[0014] As a further technical solution, the filler is a 4-vinylbenzoic acid modified filler.

[0015] In the present invention, 4-vinyl benzoic acid is used to modify the filler, thereby improving the dispersion and bonding degree of the filler in the matrix, and further improving the toughness and aging resistance of the damping rubber strip.

[0016] As a further technical solution, the mass ratio of 4-vinylbenzoic acid to filler in the 4-vinylbenzoic acid modified filler is 1:9-14.

[0017] In the present invention, the mass ratio of 4-vinylbenzoic acid to filler is limited to 1:9-14, which further improves the toughness and aging resistance of the damping rubber strip.

[0018] As a further technical solution, the preparation method of the 4-vinylbenzoic acid modified filler comprises the following steps: mixing 4-vinylbenzoic acid and a filler to obtain a 4-vinylbenzoic acid modified filler.

[0019] As a further technical solution, the mixing is wet mixing, that is, 4-vinylbenzoic acid is dissolved and then mixed with the filler, and then dried to obtain a 4-vinylbenzoic acid modified filler.

[0020] As a further technical solution, the model of the EPDM rubber is one or both of 4869 and 5890; the vulcanizing agent is one or both of sulfur and DCP; the antioxidant is one or more of antioxidant RD, antioxidant 4020, and antioxidant 2246; the foaming agent is one or more of AC foaming agent, OBSH foaming agent, and TSH foaming agent; the filler is one or more of carbon black and calcium carbonate powder; the plasticizer is one of white oil and paraffin oil; the defoaming agent includes calcium oxide; the vulcanization aid includes a vulcanization activator and a vulcanization accelerator; the vulcanization activator includes one or more of stearic acid and zinc oxide; the vulcanization accelerator includes one or more of accelerator CZ, accelerator M, accelerator BZ, and accelerator TMTD.

[0021] The present invention also proposes a preparation process of a damping rubber strip for a railway metal sound barrier, comprising the following steps:

[0022] S1, mixing the components of the solid rubber layer to obtain a mixed rubber A;

[0023] S2, mixing the components of the foamed rubber layer to obtain a mixed rubber B;

[0024] S3, extruding the rubber mix B into the rubber mix A, and vulcanizing to obtain a damping rubber strip.

[0025] The present invention also proposes the use of the damping rubber strip for railway metal sound barriers or the damping rubber strip prepared by the preparation process in railway metal sound barriers, which can be made into damping rubber strips of any shape or any shapes interconnected with each other, including but not limited to damping rubber strips with circular, square or triangular cross-sections.

[0026] The working principle and beneficial effects of the present invention are:

[0027] In the present invention, acrylonitrile-styrene-acrylate copolymer is introduced into the foamed rubber layer and the solid rubber layer based on EPDM rubber respectively, so that the toughness and aging resistance of the damping rubber strip are significantly improved. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In the following examples, the model of acrylonitrile-styrene-acrylate copolymer having a melt index of 3.5 g / 10 min is TW25;

[0030] The model of acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min is E210;

[0031] The model of acrylonitrile-styrene-acrylate copolymer with a melt index of 21 g / 10 min is WR-9120;

[0032] The model of acrylonitrile-styrene-acrylate copolymer with a melt index of 5 g / 10 min is SS1070U;

[0033] The model of acrylonitrile-styrene-acrylate copolymer with a melt index of 11 g / 10 min is ASA003L;

[0034] The test conditions for the melt index are all 220°C / 10.0kg.

[0035] Example 1

[0036] The damping rubber strip comprises a foam rubber layer and a solid rubber layer arranged in sequence from the inside to the outside;

[0037] The cross section of the damping rubber strip is circular, the diameter of the foam rubber layer is 4 mm and the thickness of the solid rubber layer is 1.5 mm;

[0038] The raw materials of the solid rubber layer of the damping rubber strip include the following components in parts by weight: 80 parts of EPDM rubber, 6 parts of acrylonitrile-styrene-acrylate copolymer with a melt index of 3.5 g / 10 min, 4 parts of polyethylene glycol, 10 parts of filler (carbon black N550), 2 parts of sulfur, 1 part of antioxidant RD, 0.8 parts of stearic acid, 1 part of zinc oxide, 0.2 parts of accelerator TMTD, 2 parts of white oil, and 1 part of defoaming agent (calcium oxide);

[0039] The raw materials of the foam rubber layer include the following components in parts by weight: 80 parts of EPDM rubber, 8 parts of acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min, 4 parts of polyethylene glycol, 10 parts of filler (calcium carbonate powder), 4 parts of foaming agent, 2 parts of sulfur, 1 part of antioxidant RD, 0.9 parts of stearic acid, 0.6 parts of zinc oxide, 0.2 parts of accelerator CZ, 0.1 parts of accelerator M, 0.1 parts of accelerator BZ, 0.1 parts of accelerator TMTD, and 2 parts of paraffin oil;

[0040] The preparation process of the damping rubber strip comprises the following steps:

[0041] S1, solid rubber layer: EPDM rubber, acrylonitrile-styrene-acrylate copolymer with a melt index of 3.5 g / 10 min, polyethylene glycol, carbon black N550, antioxidant RD, stearic acid, zinc oxide, accelerator TMTD, white oil, defoaming agent (calcium oxide) are mixed and then the remaining components are added and mixed to obtain a mixed rubber A;

[0042] S2, foam rubber layer: EPDM rubber, acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min, polyethylene glycol, calcium carbonate powder, antioxidant RD, stearic acid, zinc oxide, accelerator CZ, accelerator M, accelerator BZ, accelerator TMTD, and paraffin oil are mixed, and then the remaining components are added and mixed to obtain a mixed rubber B;

[0043] S3, extruding the rubber mix B into the rubber mix A, and vulcanizing to obtain a damping rubber strip;

[0044] The EPDM rubber is EPDM 4869 and EPDM 5890 in a mass ratio of 1:1, and the foaming agent is AC foaming agent and OBSH foaming agent in a mass ratio of 1:1.

[0045] Example 2

[0046] The damping rubber strip comprises a foam rubber layer and a solid rubber layer arranged in sequence from the inside to the outside;

[0047] The cross section of the damping rubber strip is circular, the diameter of the foam rubber layer is 4 mm and the thickness of the solid rubber layer is 1.5 mm;

[0048] The raw materials of the solid rubber layer of the damping rubber strip include the following components in parts by weight: 85 parts of EPDM rubber, 8 parts of acrylonitrile-styrene-acrylate copolymer with a melt index of 3.5 g / 10 min, 6 parts of polyethylene glycol, 12 parts of filler (carbon black N550), 3 parts of sulfur, 1 part of antioxidant 4020, 1 part of stearic acid, 1 part of zinc oxide, 1 part of accelerator TMTD, 3 parts of white oil, and 2 parts of defoaming agent (calcium oxide);

[0049] The raw materials of the foam rubber layer include the following components in parts by weight: 85 parts of EPDM rubber, 10 parts of acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min, 7 parts of polyethylene glycol, 13 parts of filler (calcium carbonate powder), 5 parts of foaming agent, 3 parts of sulfur, 1.5 parts of antioxidant 4020, 1 part of stearic acid, 1 part of zinc oxide, 0.2 parts of accelerator CZ, 0.2 parts of accelerator M, 0.3 parts of accelerator BZ, 0.3 parts of accelerator TMTD, and 3 parts of paraffin oil;

[0050] The preparation process of the damping rubber strip comprises the following steps:

[0051] S1, solid rubber layer: EPDM rubber, acrylonitrile-styrene-acrylate copolymer with a melt index of 3.5 g / 10 min, polyethylene glycol, carbon black N550, antioxidant 4020, stearic acid, zinc oxide, accelerator TMTD, white oil, defoaming agent (calcium oxide) are mixed and then the remaining components are added and mixed to obtain a mixed rubber A;

[0052] S2, foam rubber layer: EPDM rubber, acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min, polyethylene glycol, calcium carbonate powder, antioxidant 4020, stearic acid, zinc oxide, accelerator CZ, accelerator M, accelerator BZ, accelerator TMTD, and paraffin oil are mixed, and then the remaining components are added and mixed to obtain a mixed rubber B;

[0053] S3, extruding the rubber mix B into the rubber mix A, and vulcanizing to obtain a damping rubber strip;

[0054] The EPDM rubber is EPDM 4869 and EPDM 5890 in a mass ratio of 1:1; the foaming agent is AC foaming agent and OBSH foaming agent in a mass ratio of 1:1.

[0055] Example 3

[0056] The damping rubber strip comprises a foam rubber layer and a solid rubber layer arranged in sequence from the inside to the outside;

[0057] The cross section of the damping rubber strip is circular, the diameter of the foam rubber layer is 4 mm and the thickness of the solid rubber layer is 1.5 mm;

[0058] The raw materials of the solid rubber layer of the damping rubber strip include the following components in parts by weight: 90 parts of EPDM rubber, 10 parts of acrylonitrile-styrene-acrylate copolymer with a melt index of 3.5 g / 10 min, 8 parts of polyethylene glycol, 15 parts of filler (carbon black N330), 4 parts of sulfur, 1.5 parts of antioxidant RD, 1 part of stearic acid, 2 parts of zinc oxide, 1 part of accelerator TMTD, 4 parts of white oil, and 3 parts of defoaming agent (calcium oxide);

[0059] The raw materials of the foam rubber layer include the following components in parts by weight: 90 parts of EPDM rubber, 12 parts of acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min, 8 parts of polyethylene glycol, 15 parts of filler (calcium carbonate powder), 8 parts of foaming agent, 4 parts of sulfur, 1.5 parts of antioxidant RD, 2 parts of stearic acid, 1 part of zinc oxide, 0.2 parts of accelerator CZ, 0.3 parts of accelerator M, 0.3 parts of accelerator BZ, 0.2 parts of accelerator TMTD, and 4 parts of paraffin oil;

[0060] The preparation process of the damping rubber strip comprises the following steps:

[0061] S1, solid rubber layer: EPDM rubber, acrylonitrile-styrene-acrylate copolymer with a melt index of 3.5 g / 10 min, polyethylene glycol, carbon black N330, antioxidant RD, stearic acid, zinc oxide, accelerator TMTD, white oil, defoaming agent (calcium oxide) are mixed and then the remaining components are added and mixed to obtain a mixed rubber A;

[0062] S2, foam rubber layer: EPDM rubber, acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min, polyethylene glycol, calcium carbonate powder, antioxidant RD, stearic acid, zinc oxide, accelerator CZ, accelerator M, accelerator BZ, accelerator TMTD, and paraffin oil are mixed, and then the remaining components are added and mixed to obtain a mixed rubber B;

[0063] S3, extruding the rubber mix B into the rubber mix A, and vulcanizing to obtain a damping rubber strip;

[0064] The EPDM rubber is EPDM 4869 and EPDM 5890 in a mass ratio of 1:1; the foaming agent is AC foaming agent and OBSH foaming agent in a mass ratio of 1:1.

[0065] Example 4

[0066] The only difference between this embodiment and embodiment 3 is that the acrylonitrile-styrene-acrylate copolymer with a melt index of 3.5 g / 10 min in the solid rubber layer of the damping rubber strip is replaced with an acrylonitrile-styrene-acrylate copolymer with a melt index of 21 g / 10 min.

[0067] Example 5

[0068] The only difference between this embodiment and embodiment 3 is that the acrylonitrile-styrene-acrylate copolymer with a melt index of 3.5 g / 10 min in the solid rubber layer of the damping rubber strip is replaced with an acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min.

[0069] Example 6

[0070] The only difference between this embodiment and embodiment 3 is that the acrylonitrile-styrene-acrylate copolymer with a melt index of 3.5 g / 10 min in the solid rubber layer of the damping rubber strip is replaced with an acrylonitrile-styrene-acrylate copolymer with a melt index of 5 g / 10 min.

[0071] Example 7

[0072] The only difference between this embodiment and embodiment 6 is that the acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min in the foamed rubber layer of the damping rubber strip is replaced with an acrylonitrile-styrene-acrylate copolymer with a melt index of 11 g / 10 min.

[0073] Example 8

[0074] The only difference between this embodiment and embodiment 6 is that the acrylonitrile-styrene-acrylate copolymer with a melt index of 15 g / 10 min in the foamed rubber layer of the damping rubber strip is replaced with an acrylonitrile-styrene-acrylate copolymer with a melt index of 21 g / 10 min.

[0075] Example 9

[0076] The only difference between this embodiment and embodiment 8 is that the fillers in the solid rubber layer and the foamed rubber layer of the damping rubber strip are 4-vinylbenzoic acid modified fillers, and the preparation method of the 4-vinylbenzoic acid modified fillers comprises the following steps: dissolving 1g of 4-vinylbenzoic acid in 50g of ethanol, mixing with 7g of fillers, and drying to obtain 4-vinylbenzoic acid modified fillers; wherein the volume fraction of ethanol is 70%.

[0077] Example 10

[0078] The only difference between this embodiment and embodiment 9 is that the fillers in the solid rubber layer and the foamed rubber layer of the damping rubber strip are 4-vinylbenzoic acid modified fillers. The preparation method of the 4-vinylbenzoic acid modified filler comprises the following steps: dissolving 1 g of 4-vinylbenzoic acid in 50 g of ethanol, mixing with 16 g of filler, and drying to obtain 4-vinylbenzoic acid modified fillers.

[0079] Embodiment 11

[0080] The only difference between this embodiment and embodiment 9 is that the fillers in the solid rubber layer and the foamed rubber layer of the damping rubber strip are 4-vinylbenzoic acid modified fillers. The preparation method of the 4-vinylbenzoic acid modified filler comprises the following steps: dissolving 1 g of 4-vinylbenzoic acid in 50 g of ethanol, mixing with 14 g of filler, and drying to obtain 4-vinylbenzoic acid modified fillers.

[0081] Example 12

[0082] The only difference between this embodiment and embodiment 9 is that the fillers in the solid rubber layer and the foamed rubber layer of the damping rubber strip are 4-vinylbenzoic acid modified fillers. The preparation method of the 4-vinylbenzoic acid modified filler comprises the following steps: dissolving 1 g of 4-vinylbenzoic acid in 50 g of ethanol, mixing with 9 g of filler, and drying to obtain 4-vinylbenzoic acid modified fillers.

[0083] Comparative Example 1

[0084] The only difference between this comparative example and Example 3 is that acrylonitrile-styrene-acrylate copolymer is not added to the solid rubber layer and the foamed rubber layer of the damping rubber strip.

[0085] The damping rubber strips prepared in Examples 1 to 12 and Comparative Example 1 were planed to obtain the foamed rubber layer and the solid rubber layer of the damping rubber strip, respectively, and then the toughness and aging resistance performance tests were performed:

[0086] Toughness: The elongation at break test is carried out in accordance with the standard GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", and is recorded as the initial elongation at break;

[0087] Aging resistance: After hot air treatment (temperature 100℃, 96h), the elongation at break test is carried out in accordance with standard GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", and the elongation at break retention rate is calculated, elongation at break retention rate = (elongation at break after hot air treatment / initial elongation at break) × 100%.

[0088] The test results are shown in Table 1 below:

[0089] Table 1 Performance test results

[0090]

[0091] Compared with Comparative Example 1, the foamed rubber layer and the solid rubber layer of the damping rubber strips prepared in Examples 1 to 12 have higher elongation at break and higher retention rate of elongation at break, indicating that the introduction of acrylonitrile-styrene-acrylate copolymer into the foamed rubber layer and the solid rubber layer based on EPDM rubber significantly improves the toughness and aging resistance of the damping rubber strip.

[0092] Compared with Examples 3 to 4, the solid rubber layer of the damping rubber strips prepared in Examples 5 to 6 has a higher elongation at break and a higher retention rate of elongation at break, indicating that the melt index of the acrylonitrile-styrene-acrylate copolymer in the solid rubber layer is 5 to 15 g / 10 min, which further improves the toughness and aging resistance of the damping rubber strip.

[0093] Compared with Examples 6 and 7, the foamed rubber layer of the damping rubber strip prepared in Example 8 has a higher elongation at break and a higher retention rate of elongation at break, indicating that the melt index of the acrylonitrile-styrene-acrylate copolymer in the foamed rubber layer is greater than 15 g / 10 min, further improving the toughness and aging resistance of the damping rubber strip.

[0094] Compared with Example 8, the foamed rubber layer and the solid rubber layer of the damping rubber strips prepared in Examples 9 to 12 have higher elongation at break and higher retention rate of elongation at break, indicating that the filler is modified by 4-vinylbenzoic acid, the dispersion and bonding degree of the filler in the matrix are improved, and the toughness and aging resistance of the damping rubber strip are further improved.

[0095] Compared with Examples 9 to 10, the foamed rubber layer and the solid rubber layer of the damping rubber strips prepared in Examples 11 to 12 have higher elongation at break and higher retention of elongation at break, indicating that limiting the mass ratio of 4-vinylbenzoic acid to filler to 1:9 to 14 further improves the toughness and aging resistance of the damping rubber strip.

[0096] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A damping rubber strip for railway metal sound barrier, It is characterized in that It includes a foam rubber layer and a solid rubber layer arranged in sequence from the inside to the outside; The raw materials of the solid rubber layer include the following components in parts by weight: 80-90 parts of EPDM rubber, 6-10 parts of the first copolymer, 4-8 parts of polyethylene glycol, 10-15 parts of filler, 2-4 parts of vulcanizer, 1-1.5 parts of antioxidant, 2-4 parts of vulcanizing aid, 2-4 parts of plasticizer, and 1-3 parts of defoaming agent; The raw materials of the foam rubber layer include the following components in parts by weight: 80-90 parts of EPDM rubber, 8-12 parts of the second copolymer, 4-8 parts of polyethylene glycol, 10-15 parts of filler, 4-8 parts of foaming agent, 2-4 parts of vulcanizing agent, 1-1.5 parts of antioxidant, 2-4 parts of vulcanizing aid, and 2-4 parts of plasticizer; The first copolymer and the second copolymer are each independently an acrylonitrile-styrene-acrylate copolymer; The melt index of the acrylonitrile-styrene-acrylate copolymer is 5 to 21 g / 10 min; The test condition of the melt index is 220°C / 10.0kg.

2. A damping rubber strip for railway metal sound barrier according to claim 1, It is characterized in that The melt index of the first copolymer is 5-15 g / 10 min.

3. The damping rubber strip for railway metal sound barrier according to claim 1, It is characterized in that The second copolymer has a melt index greater than 15 g / 10 min.

4. The damping rubber strip for railway metal sound barrier according to claim 1, It is characterized in that The filler is a 4-vinylbenzoic acid modified filler.

5. The damping rubber strip for railway metal sound barrier according to claim 4, It is characterized in that The mass ratio of 4-vinylbenzoic acid to filler in the 4-vinylbenzoic acid modified filler is 1:9-14.

6. The damping rubber strip for railway metal sound barrier according to claim 5, It is characterized in that The preparation method of the 4-vinylbenzoic acid modified filler comprises the following steps: mixing 4-vinylbenzoic acid and a filler to obtain the 4-vinylbenzoic acid modified filler.

7. The damping rubber strip for railway metal sound barrier according to claim 1, It is characterized in that The model of the EPDM rubber is one or both of 4869 and 5890; the vulcanizing agent is one or both of sulfur and DCP; the antioxidant is one or more of antioxidant RD, antioxidant 4020, and antioxidant 2246; the foaming agent is one or more of AC foaming agent, OBSH foaming agent, and TSH foaming agent; the filler is one or more of carbon black and calcium carbonate powder; the plasticizer is one of white oil and paraffin oil; the vulcanization aid includes a vulcanization activator and a vulcanization accelerator; the vulcanization activator includes one or more of stearic acid and zinc oxide; the vulcanization accelerator includes one or more of accelerator CZ, accelerator M, accelerator BZ, and accelerator TMTD.

8. A process for preparing a damping rubber strip for railway metal sound barrier according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S1, mixing the components of the solid rubber layer to obtain a mixed rubber A; S2, mixing the components of the foamed rubber layer to obtain a mixed rubber B; S3, extruding the rubber mix B into the rubber mix A, and vulcanizing to obtain a damping rubber strip.

9. Application of the damping rubber strip for railway metal sound barrier according to any one of claims 1 to 7 or the damping rubber strip prepared by the preparation process according to claim 8 in railway metal sound barrier, It is characterized in that Damping rubber strips can be made into any shape or connected to each other in any shape.