Binder and preparation method thereof, pole piece and battery

By using a modified polycarboxylic acid binder in the cathode coating layer of lithium battery, the problem of insufficient conductivity and adhesion is solved, and the cycle life and electrochemical performance of the battery are significantly improved.

CN118638497BActive Publication Date: 2024-12-03JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411124075.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-03
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The existing lithium battery cathode coating adhesive is insufficient in conductivity and adhesion, which leads to an increase in polarization of lithium iron phosphate positive electrode material during the cycle, affecting the cycle life of the battery.

Method used

Using a modified polycarboxylic acid binder consisting of a carboxylic acid polymer and a modified polypyrrole grafted on the carboxylic acid polymer, the conductivity and adhesion of the polypyrrole is enhanced by the introduction of polypyrrole, and the It is used in the coating layer to enhance the bonding force between the positive electrode active material layer and the coating layer.

Benefits of technology

The conductivity and adhesion of the coating layer are significantly improved, the bonding force between the positive electrode active material layer and the coating layer is enhanced, the cycle life of the battery is extended, and the electrochemical performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the field of battery technology, and in particular to a binder and a preparation method thereof, a pole piece and a battery. A binder comprises a modified polycarboxylic acid; the modified polycarboxylic acid comprises a carboxylic acid polymer and a modified polypyrrole grafted on the carboxylic acid polymer. A method for preparing a binder is also provided, comprising the following steps: reacting a modifier and polypyrrole under a catalyst condition to obtain a modified polypyrrole; mixing the modified polypyrrole as a modified monomer with a carboxyl monomer to obtain a mixed monomer; mixing the mixed monomer with an initiator to initiate a polymerization reaction to obtain the binder. The present invention introduces polypyrrole (heterocyclic conjugated conductive polymer) into the molecular chain of polycarboxylic acid, which can improve the conductivity, dispersibility and swelling property of the binder in a solvent, and can alleviate the problem of poor adhesion or poor conductivity between the current primer slurry and the foil material and the positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an adhesive and a preparation method thereof, a pole piece and a battery. Background Art

[0002] Generally, the main components of batteries (such as lithium batteries, etc.) include positive electrodes, negative electrodes, electrolytes and separators. Binders are a key component of batteries. For example, they can tightly adhere the active materials, conductive agents and other additives in the active material layer of the positive or negative electrode to the current collector, thereby ensuring the structural stability and good point contact of the electrode; or some positive or negative electrodes will be provided with an intermediate coating containing a binder to improve the relevant electrochemical properties of the positive or negative electrode.

[0003] In lithium batteries, lithium iron phosphate positive electrode materials have become the mainstream positive electrode materials because of their advantages such as low cost, environmental friendliness, and good safety. However, lithium iron phosphate has problems such as poor conductivity. Its polarization will continue to increase during the cycle, which will affect the cycle life of the battery. In order to improve its electronic conductivity and reduce ohmic impedance, lithium iron phosphate positive electrode coating generally requires the use of carbon-coated aluminum foil, that is, a carbon-coated layer is set in the positive electrode, which can tightly bond the positive electrode active material to the aluminum foil, and the particles are embedded in each other, thereby improving the conductivity of the positive electrode sheet and ultimately reducing the internal resistance of the battery.

[0004] At present, the binder used in the carbon coating layer of carbon-coated aluminum foil is mostly polyacrylic acid binder. However, since the solvent in the positive electrode slurry has no swelling property for the existing polyacrylic acid binder, the binder in the positive electrode slurry (such as polyvinylidene fluoride) cannot penetrate into the carbon coating layer, which leads to a very weak peeling force between the positive electrode active material layer and the carbon coating layer, that is, the existing carbon coating layer has poor adhesion; in addition, the conductivity of the existing carbon coating layer is also poor. Therefore, it is necessary to provide an improved binder to improve the adhesion of the carbon coating layer and improve the adhesion between the positive electrode active material layer and the carbon coating layer.

[0005] Therefore, the prior art is still to be improved and developed. Summary of the invention

[0006] In view of this, the present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the present invention provides a binder and a preparation method thereof, a pole piece and a battery, which can alleviate the problem of poor bonding between the current positive electrode active material layer and the carbon coating layer, effectively improve the bonding property of the carbon coating layer, and also improve the conductivity of the carbon coating layer.

[0007] In order to solve the above technical problems, this application is implemented as follows:

[0008] According to one aspect of the present application, an embodiment of the present application provides a binder, wherein the binder includes a modified polycarboxylic acid; the modified polycarboxylic acid includes a carboxylic acid polymer and a modified polypyrrole grafted onto the carboxylic acid polymer.

[0009] In the present application, the binder can be applied to the carbon coating layer (also called conductive coating) of the positive electrode sheet.

[0010] In addition, the adhesive according to the present application may also have the following additional technical features:

[0011] In some embodiments, the modified polypyrrole includes a modifier containing a reactive group or a modifier containing a reactive group in the hydrolysis product, and a polypyrrole having a functional group that reacts or interacts with the reactive group; wherein the reactive group includes at least one of an epoxy group or a silanol group, and the functional group includes an imine group.

[0012] In some embodiments, the modifier includes at least one of vinyl siloxane or glycidyl methacrylate, and the hydrolysis product of the vinyl siloxane contains silanol groups, wherein the vinyl siloxane includes at least one of vinyl trimethoxy silane, vinyl triethoxy silane or γ-methacryloxy trimethoxy silane.

[0013] In some embodiments, the viscosity of the binder is 700-1500 mPa·s.

[0014] In some embodiments, the solid content of the binder is 20-30%.

[0015] In some embodiments, the pH value of the binder is 3-5.

[0016] According to another aspect of the present application, an embodiment of the present application provides a method for preparing a binder, the method comprising the following steps:

[0017] The modifier and polypyrrole are reacted under a catalyst condition to obtain modified polypyrrole;

[0018] Mixing the modified polypyrrole as a modified monomer with a carboxyl monomer to obtain a mixed monomer;

[0019] The mixed monomer is mixed with an initiator to initiate a polymerization reaction to obtain the binder.

[0020] In some embodiments, the step of obtaining modified polypyrrole satisfies at least one of the following features (1) to (6): (1) the modifier includes at least one of vinyl siloxane or glycidyl methacrylate, wherein the vinyl siloxane includes at least one of vinyl trimethoxy silane, vinyl triethoxy silane or γ-methacryloxy trimethoxy silane; (2) the mass ratio of the modifier to the polypyrrole is (0.5-1): (100-200); (3) the number average molecular weight of the polypyrrole is 2000-5000; (4) the catalyst includes at least one of concentrated sulfuric acid, tetrafluoroboric acid, perchloric acid or fluoroacetic acid; (5) the mass of the catalyst is 0.05%-0.1% of the mass of the polypyrrole; (6) the reaction temperature is 75°C-85°C and the reaction time is 120 min-180 min.

[0021] In some embodiments, the step of obtaining a mixed monomer satisfies at least one of the following characteristics (1) to (2): (1) the mass ratio of the modified monomer to the carboxyl monomer is 1:(5-9); (2) the carboxyl monomer includes at least one of sodium styrene sulfonate, acrylic acid, methacrylic acid or carboxyethyl acrylate.

[0022] In some embodiments, the step of obtaining the binder satisfies at least one of the following features (1) to (6): (1) the mass of the initiator is 1% to 5% of the mass of the mixed monomer; (2) the initiator comprises at least one of sodium persulfate, ammonium persulfate or potassium persulfate; (3) the mixed monomer and the initiator are mixed to initiate a polymerization reaction, specifically comprising: adding water to a reaction device and heating the temperature to 80°C to 90°C, and simultaneously dripping the mixed monomer and the initiator into the reaction device, the dripping time being 180 min to 240 min, and after the dripping is completed, keeping the temperature at 85°C to 95°C for 60 min to 80 min; (4) the viscosity of the binder is 700 to 1500 mPa•s; (5) the solid content of the binder is 20 to 30%; (6) the pH value of the binder is 3 to 5.

[0023] According to another aspect of the present application, an embodiment of the present application provides a pole piece, the pole piece comprising:

[0024] current collector;

[0025] A conductive coating is disposed on at least one side of the current collector along the thickness direction; the conductive coating comprises the aforementioned binder or the binder prepared according to the aforementioned method; and

[0026] The active material layer is arranged on the surface of the conductive coating layer which is away from the current collector.

[0027] In some embodiments, the conductive coating further comprises a conductive material, that is, the conductive coating comprises a conductive material and the binder.

[0028] In some embodiments, the conductive material includes at least one of conductive carbon black, conductive graphite, carbon nanotubes, carbon nanofibers or graphene.

[0029] In some of the embodiments, the mass ratio of the binder to the conductive material is (4-6): (6-4).

[0030] In some embodiments, the active material layer includes an active material, and the active material includes lithium iron phosphate.

[0031] According to another aspect of the present application, an embodiment of the present application provides a battery, which includes the aforementioned pole piece.

[0032] Implementing the technical solution of the present invention has at least the following beneficial effects:

[0033] In an embodiment of the present application, the binder provided includes a modified polycarboxylic acid, and the modified polycarboxylic acid includes a carboxylic acid polymer and a modified polypyrrole grafted on the carboxylic acid polymer. The present application obtains a modified polycarboxylic acid by modifying the polycarboxylic acid with modified polypyrrole. Thus, the modified polycarboxylic acid is applied to a conductive coating, and by introducing polypyrrole (a heterocyclic conjugated conductive polymer) into the molecular chain of the polycarboxylic acid, the conductivity of the obtained modified polycarboxylic acid is optimized by utilizing the good conductivity of the polypyrrole, and the dispersibility of the modified polycarboxylic acid can be improved by utilizing the good dispersibility of the polycarboxylic acid structure to the conductive carbon; and polypyrrole has a high swelling property in a solvent (such as N-methylpyrrolidone), which can improve the swelling property of the modified polycarboxylic acid, and then the binder (such as polyvinylidene fluoride) in the positive electrode slurry can be penetrated into the conductive coating, which greatly improves the bonding force between the positive electrode coating, that is, the positive electrode active material layer and the conductive coating. Therefore, the present application can improve the conductivity, dispersibility and swelling property of the binder in the solvent, and can effectively alleviate the problems of weak conductivity and poor adhesion of the existing conductive coating.

[0034] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION

[0035] The present application is further described below in conjunction with specific embodiments. It should be understood that these embodiments of the present application are only used to illustrate the present application and are not used to limit the scope of the present application.

[0036] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0037] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0038] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0039] As analyzed in the background technology, lithium iron phosphate itself has poor conductivity, and lacks a bridge for transmitting electrons between the current collector such as aluminum foil. After carbon coating on the surface of the aluminum foil, the carbon coating layer can be used as a bridge to tightly bond the positive electrode active material to the aluminum foil, and the particles are embedded in each other, thereby improving the conductivity of the positive electrode sheet and ultimately reducing the internal resistance of the battery. However, the current carbon coating layer formula mostly adopts the method of conductive carbon plus polyacrylic acid dispersant (binder). Since polyacrylic acid itself is not conductive, it will affect the conductivity of the carbon coating layer; and when polyacrylic acid is used as a carbon coating aluminum foil dispersant, since the positive electrode slurry solvent such as N-methylpyrrolidone (NMP) has no swelling property for the existing polyacrylic acid binder, the binder polyvinylidene fluoride (PVDF) in the positive electrode slurry cannot penetrate into the carbon coating layer, which leads to a weak peeling force between the positive electrode active material layer and the carbon coating layer, that is, the bonding force between the positive electrode active material layer and the carbon coating layer is poor, and the bonding property of the existing carbon coating layer is poor; in addition, the conductivity of the existing carbon coating layer is also poor. Therefore, it is urgent to provide a new type of binder to improve the adhesion and conductivity of the carbon coating layer. Based on this problem, how to continue to increase the conductivity of the carbon coating layer and improve the adhesion between the positive electrode active material layer and the carbon coating layer has become a difficulty in the relevant industry.

[0040] In view of this, the inventors of the present application have improved the binder in the carbon coating layer from the perspective of modifying polycarboxylic acids such as polyacrylic acid, and provided a binder with high conductivity and strong adhesion that can be used in the carbon coating layer (conductive coating), so as to increase the conductivity of the carbon coating layer and improve the adhesion (or bonding force) between the positive electrode active material layer and the carbon coating layer, thereby improving the electrochemical performance of the battery. The present application is described in detail below.

[0041] [Binder]

[0042] In some embodiments, the present application provides a binder, which includes a modified polycarboxylic acid; the modified polycarboxylic acid includes a carboxylic acid polymer and a modified polypyrrole grafted on the carboxylic acid polymer.

[0043] In the present application, the binder adopts modified polycarboxylic acid, which introduces polypyrrole (heterocyclic conjugated conductive polymer) into the molecular chain of polycarboxylic acid to obtain a polypyrrole-grafted carboxylic acid polymer.

[0044] The modified polycarboxylic acid can be obtained by polymerizing a modified monomer and a carboxyl monomer, wherein the modified monomer includes polypyrrole modified by a modifier. That is, the raw materials for preparing the modified polycarboxylic acid may include a modified monomer and a carboxyl monomer. The carboxyl monomer can have a good bonding effect, and the carboxyl group can produce a physical interaction with the active material and the current collector, improve the bonding performance to the active material, and also have a good dispersion of conductive carbon, or the carboxyl group can be treated by lithiation to increase the ion migration rate. The polypyrrole modified by the modifier has good conductivity, that is, due to the unique chemical structure of pyrrole, a large delocalized bond is formed in the polypyrrole, which can play the role of conducting electrons; in addition, polypyrrole has a high swelling property in a solvent (such as NMP), which is conducive to improving the bonding force between the positive electrode active material layer and the carbon coating layer.

[0045] It can be understood that the binder provided in the present application can be used in the positive electrode sheet, especially in the conductive coating (also called carbon coating layer) of the positive electrode sheet, which is more preferred, and can alleviate the problem of weak conductivity and poor adhesion of the existing conductive coating. Of course, in addition to this, the binder can also be used in other structures or scenarios, providing adhesion to any scenario or layered structure with similar requirements. The embodiments of the present application do not impose specific restrictions on the specific use scenarios and working conditions of the binder.

[0046] Thus, the modified polycarboxylic acid binder provided by the embodiment of the present invention is used to modify the polycarboxylic acid by using modified polypyrrole to obtain the modified polycarboxylic acid, that is, to obtain the polypyrrole-grafted carboxylic acid polymer. The modified polycarboxylic acid is applied to the conductive coating, and the good conductivity of polypyrrole is introduced into the molecular chain of the polycarboxylic acid, and the conductivity of the obtained modified polycarboxylic acid is optimized by using the good dispersibility of the polycarboxylic acid structure to the conductive carbon, so as to improve the dispersibility of the modified polycarboxylic acid; and polypyrrole has a high swelling property in the solvent (such as NMP), which can improve the swelling property of the modified polycarboxylic acid, and then the binder (such as PVDF) in the positive electrode slurry can penetrate into the conductive coating, which greatly improves the bonding force between the positive electrode coating, that is, the active material layer and the conductive coating. In summary, the binder provided by the present invention can play a role of strong bonding performance and conductive electrons / ions, and improve the conductivity, dispersibility and swelling property of the binder in the solvent. Therefore, the present application can effectively alleviate the problems of weak conductivity and poor adhesion of existing conductive coatings.

[0047] The inventors have found through in-depth research that when the adhesive of the present application satisfies the above-mentioned design conditions and optionally satisfies one or more of the following conditions, the performance of the adhesive can be further improved.

[0048] In some specific embodiments, the modified polycarboxylic acid can be obtained by two-step polymerization. In the first step, polypyrrole is modified by a modifier to obtain modified polypyrrole. In the second step, the prepared modified polypyrrole is used as a modified monomer to polymerize with a carboxyl monomer to form a modified polycarboxylic acid, i.e., a binder.

[0049] In some embodiments, the modified polypyrrole includes a modifier containing a reactive group or a modifier containing a reactive group in the hydrolysis product, and a polypyrrole having a functional group that reacts or interacts with the reactive group; wherein the reactive group includes at least one of an epoxy group or a silanol group, and the functional group includes an imine group.

[0050] In the present application, the unsaturated group is introduced into the polypyrrole to obtain the modified polypyrrole by reacting the reactive group such as epoxy group or silanol group with the functional group of the polypyrrole such as imine group to form a covalent bond, and the modified monomer is obtained. In this way, it is convenient to polymerize with the subsequent carboxyl monomer, that is, to introduce the polypyrrole into the molecular chain of the polycarboxylic acid to form the modified polycarboxylic acid.

[0051] In some embodiments, the modifier includes, but is not limited to, at least one of vinyl siloxane or glycidyl methacrylate; the hydrolysis product of the vinyl siloxane contains silanol groups, wherein the vinyl siloxane includes at least one of vinyl trimethoxy silane, vinyl triethoxy silane, or γ-methacryloxy trimethoxy silane. As an example, the modifier can be vinyl trimethoxy silane, vinyl triethoxy silane, γ-methacryloxy trimethoxy silane, glycidyl methacrylate, or a mixture of any two or more of the above substances.

[0052] It should be understood that among the above-mentioned modifiers, vinyl siloxanes such as vinyl trimethoxysilane, vinyl triethoxysilane, and γ-methacryloxy trimethoxysilane contain reactive groups in the hydrolysis products obtained after hydrolysis, and the reactive groups are silanol groups, which react with the imine groups in polypyrrole to form covalent bonds. Glycidyl methacrylate contains reactive groups such as epoxy groups, which react with the imine groups in polypyrrole to form covalent bonds.

[0053] It should be noted that the modifier is not limited to the substances listed above, and can be used to react with the imine group in polypyrrole to form a covalent bond and introduce an unsaturated group into polypyrrole. This does not limit the purpose of the present invention, and other similar modifiers can also be used in the present invention.

[0054] In some embodiments, the viscosity of the binder is 700 to 1500 mPa·s. As an example, the viscosity of the binder is 700 mPa·s, 800 mPa·s, 900 mPa·s, 1000 mPa·s, 1100 mPa·s, 1200 mPa·s, 1300 mPa·s, 1500 mPa·s, etc. Of course, it can also be other values ​​within the above range, which are not limited here. If the viscosity of the binder is too large, such as greater than 1500 mPa·s, the viscosity of the slurry containing it will be too large, and the slurry cannot be applied; if the viscosity of the binder is too small, such as less than 700 mPa·s, the stability of the slurry containing it will be poor, and the dispersion effect will also be poor. Therefore, by controlling the viscosity of the binder within the above range, the stability and dispersion effect of the slurry can be improved, and the slurry can be applied smoothly.

[0055] In some embodiments, the solid content of the binder is 20-30%, that is, the solid content concentration of the binder composition is 20wt%-30wt%. As an example, the solid content of the binder can be 20%, 22%, 24%, 25%, 26%, 28%, 30%, etc., and of course it can also be other values ​​within the above range, which are not limited here. If the solid content of the binder is too large, such as greater than 30%, it will make it impossible to achieve polymerization and explosion during the preparation process; if the solid content of the binder is too small, such as less than 20%, it will increase the preparation cost.

[0056] In addition, when the solid content of the above-mentioned binder is 20-30%, the viscosity of the binder can reach 700-1500mPa·s, which means that the solid components such as adhesive polymers contained in the binder can show high viscosity in the solvent. When the viscosity of the binder is too small, the adhesion between the active material layer and the conductive coating cannot be effectively ensured, and the cycle performance of the battery will be reduced. In addition, the conductive coating obtained by using the binder cannot be effectively prevented from peeling off during roller pressing. Thus, by making the viscosity of the binder within the above range, a good bonding effect can be achieved.

[0057] In some embodiments, the pH value of the binder is 3 to 5. As an example, the pH value of the binder can be 3, 3.4, 4, 4.5 or 5. If the pH value of the binder is too high, such as greater than 5, the coating containing the binder will have almost no adhesion; if the pH value of the binder is too low, such as less than 3, it will be too acidic and easily corrode the equipment.

[0058] [Method for preparing adhesive]

[0059] In some embodiments, the present application provides a method for preparing a binder, the method comprising the following steps:

[0060] The modifier and polypyrrole are reacted under a catalyst condition to obtain modified polypyrrole;

[0061] Mixing the modified polypyrrole as a modified monomer with a carboxyl monomer to obtain a mixed monomer;

[0062] The mixed monomers are mixed with an initiator to initiate a polymerization reaction to obtain a binder.

[0063] The preparation process of the binder is simple, easy to control, highly feasible, and has little pollution to the environment, and is suitable for industrial-scale production.

[0064] It should be understood that all the features and advantages described above for the “binder” are also applicable to the “method for preparing the binder” and will not be described in detail here.

[0065] In some specific embodiments, the preparation method of the provided binder specifically comprises the following steps:

[0066] (a) Preparation of modified polypyrrole.

[0067] In step (a), the modifier and polypyrrole are reacted under catalyst conditions to obtain modified polypyrrole.

[0068] Specifically, in some embodiments, step (a) specifically includes:

[0069] The polypyrrole is dissolved in the modifier, a catalyst is added, and the mixture is stirred, heated to a certain temperature, and reacted for a certain period of time so that the epoxy group or silanol group in the modifier reacts with the imine group in the polypyrrole to form a covalent bond, and the unsaturated group is introduced into the polypyrrole to obtain a modified polypyrrole intermediate.

[0070] Optionally, in step (a), the modifier includes, but is not limited to, at least one of vinyl siloxane or glycidyl methacrylate; wherein the vinyl siloxane includes at least one of vinyl trimethoxy silane, vinyl triethoxy silane or γ-methacryloxy trimethoxy silane.

[0071] Optionally, in step (a), the number average molecular weight of polypyrrole is 2000-5000; as an example, the number average molecular weight of polypyrrole can be 2000, 2500, 3000, 3500, 4000, 4500, 5000, etc., and of course it can also be other values ​​within the above range, which is not limited here.

[0072] By controlling the molecular weight of polypyrrole within the above range, a modified polypyrrole having suitable conductivity and reactivity can be obtained. If the number average molecular weight of polypyrrole is too low, such as less than 2000, its conductivity is poor, which is not conducive to improving the conductivity of the binder; if the number average molecular weight of polypyrrole is too high, such as more than 5000, the reactivity of the obtained modified polypyrrole is low, which is not conducive to the subsequent polymer reaction with the carboxyl monomer.

[0073] Optionally, in step (a), the mass ratio of the modifier to the polypyrrole is (0.5-1):(100-200), preferably 1:(100-200). As an example, the mass ratio of the modifier to the polypyrrole can be 0.75:100, 1:100, 1:120, 1:140, 1:150, 1:160, 1:180, 1:200, etc., and of course it can be other values ​​within the above range, which is not limited here.

[0074] By controlling the mass ratio of the modifier to the polypyrrole within the above range, the reactivity of the obtained modified polypyrrole can be guaranteed and the destruction of the structure of the polypyrrole can be avoided. If the amount of the modifier added is too little, the reactivity of the obtained modified polypyrrole intermediate is insufficient; if the amount of the modifier added is too much, the conductive structure of the polypyrrole itself may be destroyed.

[0075] Optionally, in step (a), the catalyst may be an anhydrous protonic acid, such as a catalyst including, but not limited to, at least one of concentrated sulfuric acid, tetrafluoroboric acid, perchloric acid or fluoroacetic acid. As an example, the catalyst may be concentrated sulfuric acid, tetrafluoroboric acid, perchloric acid, fluoroacetic acid, or a mixture of any two or more of the above substances.

[0076] Among the above-mentioned catalysts, concentrated sulfuric acid is preferred because the raw materials are easily available and the use effect is better.

[0077] It should be noted that the catalyst is not limited to the substances listed above. The acid catalyst that can be used to catalyze the reaction between the modifier and polypyrrole does not limit the purpose of the present invention. Other anhydrous protonic acids can also be used in the present invention.

[0078] Optionally, in step (a), the mass of the catalyst is 0.05% to 0.1% of the mass of the polypyrrole. As an example, the mass of the catalyst can be 0.05%, 0.06%, 0.08%, 0.1%, etc. of the mass of the polypyrrole, and of course can be other values ​​within the above range, which are not limited here.

[0079] By controlling the amount of catalyst added within the above range, the cost can be reduced while ensuring the catalytic effect. If the amount of catalyst added is too high, the preparation cost will be increased without significantly improving the catalytic effect. If the amount of catalyst added is too low, the catalytic effect will be weakened and the reaction rate will be reduced.

[0080] Optionally, in step (a), the reaction temperature is 75°C to 85°C, and the reaction time is 120min to 180min. That is, after adding the catalyst, stirring and heating to 75°C to 85°C are carried out for 120min to 180min. As an example, the reaction temperature can be 75°C, 76°C, 78°C, 80°C, 82°C, 84°C, 85°C, etc., and the reaction time can be 120min, 130min, 140min, 150min, 160min, 170min, 180min, etc.

[0081] Therefore, at the above reaction temperature and time, the modifier and polypyrrole can be fully reacted to obtain modified polypyrrole with excellent performance.

[0082] (b) Preparation of mixed monomers.

[0083] In step (b), the modified polypyrrole obtained in step (a) is mixed with a carboxyl monomer as a modified monomer to obtain a mixed monomer.

[0084] Optionally, in step (b), the mass ratio of the modified monomer to the carboxyl monomer is 1:(5-9). As an example, as an example, the mass ratio of the modified monomer to the carboxyl monomer can be 1:5, 1:6, 1:7, 1:8, 1:9, etc., and of course it can also be other values ​​within the above range, which is not limited here.

[0085] In practical applications, the dosage of the above two types of monomers can be adjusted as needed. In this embodiment, by controlling the dosage of the modified monomer and the carboxyl monomer, the content of polypyrrole and carboxyl in the binder can be controlled, thereby better achieving the effect of improving conductivity and adhesion.

[0086] Optionally, in step (b), the carboxyl monomer includes, but is not limited to, at least one of sodium styrene sulfonate, acrylic acid, methacrylic acid or carboxyethyl acrylate.

[0087] It should be noted that the carboxyl monomer is not limited to the above-listed substances and can be used for polymerization reaction with the modified monomer, which does not limit the purpose of the present invention. Other similar carboxyl monomers can also be used in the present invention.

[0088] (c) Preparation of binder.

[0089] In step (c), the mixed monomer obtained in step (b) is mixed with an initiator to initiate a polymerization reaction to obtain a binder.

[0090] Specifically, in some embodiments, step (c) specifically includes:

[0091] Add water (such as deionized water) to a reaction device (such as a reactor) and heat it to 80°C to 90°C. Simultaneously, drop the mixed monomer and initiator into the reaction device for 180min to 240min. After the dropwise addition is completed, keep the temperature at 85°C to 95°C for 60min to 80min to obtain a binder.

[0092] Preferably, water (such as deionized water) is added to the reaction equipment (such as a reactor) and the temperature is raised to 84°C to 90°C, and the mixed monomer and initiator are added dropwise to the reaction equipment at the same time, and the dropping time is 180min to 240min. After the dropping is completed, the temperature is kept at 86°C to 92°C for 60min to 80min to obtain a binder. As an example, the above-mentioned heating temperature can be 80°C, 82°C, 84°C, 85°C, 86°C, 88°C, 90°C, etc., and the above-mentioned dropping time can be 180min, 190min, 200min, 210min, 220min, 230min, 240min, etc. The temperature of the above-mentioned reaction can be 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 92°C, 95°C, etc., and the above-mentioned reaction time can be 60min, 65min, 70min, 75min, 80min, etc.

[0093] Optionally, in step (c), the mass of the initiator is 1% to 5% of the mass of the mixed monomers. As an example, the mass of the initiator is 1%, 2%, 3%, 4%, 5%, etc. of the mass of the mixed monomers, and of course it can be other values ​​within the above range, which is not limited here.

[0094] Optionally, in step (c), the initiator includes, but is not limited to, at least one of sodium persulfate, ammonium persulfate or potassium persulfate.

[0095] It should be noted that the initiator is not limited to the substances listed above, and can be used to initiate the polymerization reaction of polymerizable monomers, which does not limit the purpose of the present invention. Other similar initiators can also be used in the present invention, which are not listed here one by one.

[0096] In this embodiment, the viscosity of the prepared adhesive is 700-1500 mPa•s, the solid content of the prepared adhesive is 20-30%, and the pH value of the prepared adhesive is 3-5.

[0097] [Pole piece]

[0098] In some embodiments, the present application provides a pole piece, the pole piece comprising:

[0099] current collector;

[0100] A conductive coating is disposed on at least one side of the current collector along the thickness direction; the conductive coating comprises the aforementioned binder or the binder prepared according to the aforementioned method; and

[0101] The active material layer is arranged on the surface of the conductive coating layer which faces away from the current collector.

[0102] Based on the same inventive concept, an embodiment of the present application also provides a pole piece, which contains the above-mentioned adhesive. It should be understood that since the pole piece contains the above-mentioned adhesive, all the features and advantages described in the previous article for the "adhesive and its preparation method" are also applicable to the "pole piece" and will not be repeated here one by one.

[0103] The above-mentioned electrode sheet can be a positive electrode sheet or a negative electrode sheet. Preferably, the electrode sheet is a positive electrode sheet.

[0104] The binder of the embodiment of the present application can be used for the preparation of positive electrode sheets / negative electrode sheets, for example, a mixture containing the above binder and a conductive material is prepared into a slurry and coated on a current collector, a conductive coating can be formed on the current collector, and then an active material layer is formed on the conductive coating, and the positive electrode sheet / negative electrode sheet is obtained after drying. Among them, the binder provided in the present application is particularly preferably used in positive electrode sheets, especially in positive electrode sheets using lithium iron phosphate active materials, because the conductive coating of the positive electrode sheet containing lithium iron phosphate active materials in the secondary battery has more significant problems caused by bonding.

[0105] As an improvement of the electrode sheet of the present application, such as the positive electrode sheet, the electrode sheet includes a current collector, a conductive coating disposed on at least one surface of the current collector along the thickness direction, and an active material layer disposed on the conductive coating. That is, the provided electrode sheet includes a stacked current collector, a conductive coating and an active material layer. Among them, the current collector can be a foil material commonly used in batteries. As an example, the current collector can be aluminum foil, copper foil, nickel foil, titanium foil, stainless steel foil, etc. Preferably, the current collector can be aluminum foil.

[0106] It should be pointed out that in the present application, in some cases, the provided pole piece includes a stacked current collector, a conductive coating and an active material layer, the conductive coating is arranged between the current collector and the active material layer, and the current collector can be various current collectors well known in the art, and there is no limitation on this. Alternatively, in other cases, the provided pole piece may also include a current collector and an active material layer, the current collector includes a foil and a conductive coating arranged on the foil, and the active material layer is arranged on the conductive coating, that is, the conductive coating may be a part of the current collector, and in the preparation process, the current collector including the conductive coating is compounded with the active material layer.

[0107] The above-mentioned "the conductive coating is disposed on at least one side surface of the current collector along the thickness direction" means that the conductive coating can be disposed on one surface of the current collector along its own thickness direction, or on two surfaces of the current collector along its own thickness direction. The "surface" here can be the entire area of ​​the current collector or a partial area of ​​the current collector. This application has no particular limitation on this, as long as the purpose of this application can be achieved.

[0108] As an example, the current collector has two surfaces opposite to each other in its thickness direction, and the conductive coating is disposed on the two opposite surfaces of the current collector. Further, an active material layer is formed on the surfaces of the conductive coatings on both sides. It is understood that in other embodiments, the conductive coating may also be stacked on any one of the two surfaces of the current collector.

[0109] Therefore, by setting the above-mentioned conductive coating and adding the adhesive provided by the embodiment of the present application to the conductive coating, the conductivity of the conductive coating can be enhanced, thereby enhancing the conductivity of the pole piece, and increasing the adhesion between the active material layer and the conductive coating, thereby improving the bonding force between the two and enhancing the structural stability of the pole piece.

[0110] In some embodiments, the conductive coating further comprises a conductive material; that is, the conductive coating is mainly composed of a binder and a conductive material. Optionally, the conductive material is preferably a conductive carbon material, which includes, but is not limited to, at least one of conductive carbon black, conductive graphite, carbon nanotubes, carbon nanofibers, or graphene.

[0111] The conductive material in the conductive coating can be any of various conductive carbon materials known in the art that can be used in batteries. It is not limited to the above-mentioned carbon materials, and other types can also be used, which is not limited to this.

[0112] In some embodiments, the mass ratio of the binder to the conductive material is (4-6): (6-4). As an example, the mass ratio of the binder to the conductive material may be 4:6, 5:5, 6:4, etc.

[0113] In some embodiments, the active material layer includes an active material, and the active material includes lithium iron phosphate.

[0114] The binder of the present application is suitable for positive electrode plates containing lithium iron phosphate active materials, but is not limited thereto. Other active materials with similar requirements can also be used in the present application. For example, the active material can also be lithium iron manganese phosphate, lithium iron aluminum phosphate, etc., which are not listed one by one here.

[0115] In addition, there is no limitation on the specific type and content of the conductive agent and the binder in the active material layer, and the components and proportions known in the art that can be used for the active material layer of the positive electrode sheet of a secondary battery can be selected.

[0116] Optionally, the thickness of the conductive coating may be 0.3 μm to 3 μm, preferably 0.5 μm to 2 μm, and more preferably 0.5 μm to 1.5 μm. If the thickness of the conductive coating is too thin, the effect of the conductive coating cannot be effectively exerted, the bonding performance and the conductive performance will be reduced, and the too thin conductive coating is prone to serious leakage, affecting the uniformity of the coating; if the thickness of the conductive coating is too thick, the cost will increase.

[0117] Optionally, the thickness of the active material layer may be 80 μm to 250 μm, preferably 80 μm to 200 μm, and more preferably 100 μm to 160 μm. If the thickness of the active material layer is too thin, the energy density of the battery using it will decrease; if the thickness of the active material layer is too thick, the cost will increase and the powder will fall off seriously.

[0118] In this embodiment, the method of preparing a pole piece using the adhesive provided in this application is well known to those skilled in the art. A method of preparing a pole piece using the adhesive provided in this application is as follows:

[0119] The binder, conductive material and solvent (such as water) of the present application are evenly mixed to form a coating slurry, and the coating slurry is applied to a current collector (such as aluminum foil) to form a conductive coating (such as carbon-coated aluminum foil) on the current collector; then the positive electrode active material, conductive agent, binder (positive electrode binder, such as PVDF) are dispersed in a solvent (such as NMP) to form a positive electrode slurry; the positive electrode slurry is applied to the prepared conductive coating (carbon-coated aluminum foil), and after oven drying, roller pressing and other processes, a pole piece can be obtained.

[0120] [Battery]

[0121] In some embodiments, the present application provides a battery, the battery comprising the aforementioned pole piece. Optionally, the pole piece is a positive pole piece.

[0122] In the present application, the battery also includes a negative electrode plate, an electrolyte and a separator.

[0123] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode material. As an example, the negative electrode current collector has two surfaces opposite to each other in its own thickness direction, and the negative electrode active material layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0124] In this embodiment, the specific materials and structures of the negative electrode current collector and the negative electrode film layer in the negative electrode plate are not limited, and the negative electrode plate structure and components known in the art that can be used for secondary batteries can be selected.

[0125] In the embodiment of the present application, the electrolyte may be an electrolyte solution, and the electrolyte solution includes a lithium salt and an organic solvent. The present application has no particular limitation on the lithium salt and the organic solvent, as long as the purpose of the present application can be achieved.

[0126] The present application has no particular limitation on the isolation membrane, as long as the purpose of the present application can be achieved.

[0127] Since the battery provided in the embodiment of the present invention adopts all the technical solutions of the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.

[0128] In the embodiment of the present invention, the battery can be wound or laminated according to the actual situation, and the manufacturing method is not limited.

[0129] The shape of the outer casing of the battery is also arbitrary, and may be any of cylindrical, rectangular, laminated, button-shaped, large-sized, and the like.

[0130] In order to better understand the present invention, the specific implementation process of the present invention will be described in detail below in a specific implementation mode. The implementation methods described below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application. If no specific technology or conditions are specified in the implementation method, the technology or conditions described in the literature in the field or the product specification shall be followed.

[0131] Example 1

[0132] 1. The preparation of the binder comprises the following steps:

[0133] (a) 100 parts by mass of polypyrrole (number average molecular weight 3000) was dissolved in 0.75 parts by mass of vinylsiloxane (vinyltrimethoxysilane), 0.075 parts by mass of concentrated sulfuric acid as a catalyst was added, and the mixture was stirred and heated to 80° C. for reaction for 120 minutes to obtain modified polypyrrole.

[0134] (b) 15 parts by mass of modified polypyrrole as a modifying monomer and 100 parts by mass of acrylic acid as a carboxyl monomer are mixed to obtain a mixed monomer.

[0135] (c) 305 parts by mass of deionized water were added to the reaction kettle, and the temperature was raised to 88° C. At the same time, a mixed monomer and an initiator ammonium persulfate solution (the ammonium persulfate solution is prepared by dissolving 2.3 parts by mass of ammonium persulfate in 40 parts by mass of water) were added dropwise to the reaction kettle for 180 min. After the addition was completed, the mixture was kept at 86° C. for 60 min to obtain a binder.

[0136] 2. Preparation of positive electrode

[0137] 5 parts by mass of the prepared binder, 5 parts by mass of conductive carbon black and 90 parts by mass of deionized water were mixed, and after mixing and dispersing in a double planetary mixer for 10 hours, a slurry with a solid content of 10% and a viscosity of 20.5 cp was obtained; the slurry was coated on both sides of the current collector optical aluminum foil by a gravure roller to obtain a carbon-coated aluminum foil with a total thickness of 1.2 μm on both sides of the conductive coating;

[0138] The positive electrode active material lithium iron phosphate, the conductive agent conductive carbon black, and the binder PVDF are mixed in a mass ratio of 96:2:2, dissolved in NMP, and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry is coated on the prepared conductive coating (carbon-coated aluminum foil). After oven drying, roller pressing and other processes, a positive electrode sheet can be obtained.

[0139] Example 2

[0140] The preparation of the binder is basically the same as that in Example 1, except that:

[0141] In step (a) of Example 2, the modifier is glycidyl methacrylate.

[0142] The rest are the same as in Example 1.

[0143] Example 3

[0144] The preparation of the binder is basically the same as that in Example 1, except that:

[0145] In step (b) of Example 3, the carboxyl monomer is methacrylic acid.

[0146] The rest are the same as in Example 1.

[0147] Example 4

[0148] The preparation of the binder is basically the same as that in Example 1, except that:

[0149] In step (a) of Example 4, 100 parts by mass of polypyrrole (number average molecular weight 5000) was dissolved in 1 part by mass of vinyl siloxane (vinyl trimethoxy silane), 0.05 parts by mass of concentrated sulfuric acid as a catalyst was added, and the mixture was stirred and heated to 80° C. for 120 minutes to obtain modified polypyrrole.

[0150] The rest are the same as in Example 1.

[0151] Example 5

[0152] The preparation of the binder is basically the same as that in Example 1, except that:

[0153] In step (a) of Example 5, 200 parts by mass of polypyrrole (number average molecular weight 2000) was dissolved in 1 part by mass of vinyl siloxane (vinyl triethoxysilane), 0.2 parts by mass of concentrated sulfuric acid as a catalyst was added, and the mixture was stirred and heated to 80° C. for 120 minutes to obtain modified polypyrrole.

[0154] The rest are the same as in Example 1.

[0155] Example 6

[0156] The preparation of the binder is basically the same as that in Example 1, except that:

[0157] In step (a) of Example 6, 100 parts by mass of polypyrrole (number average molecular weight 3000) was dissolved in 0.75 parts by mass of vinyl siloxane (γ-methacryloxytrimethoxysilane), 0.075 parts by mass of concentrated sulfuric acid as a catalyst was added, and the mixture was stirred and heated to 75° C. for reaction for 180 minutes to obtain modified polypyrrole.

[0158] The rest are the same as in Example 1.

[0159] Example 7

[0160] The preparation of the binder is basically the same as that in Example 1, except that:

[0161] In step (b) of Example 7, 20 parts by mass of modified polypyrrole as a modifying monomer was mixed with 100 parts by mass of carboxyl monomer acrylic acid to obtain a mixed monomer.

[0162] The rest are the same as in Example 1.

[0163] Example 8

[0164] The preparation of the binder is basically the same as that in Example 1, except that:

[0165] In step (b) of Example 8, 11.1 parts by mass of modified polypyrrole as a modifying monomer was mixed with 100 parts by mass of carboxyl monomer acrylic acid to obtain a mixed monomer.

[0166] The rest are the same as in Example 1.

[0167] Example 9

[0168] The preparation of the binder is basically the same as that in Example 1, except that:

[0169] In step (c) of Example 9, 305 parts by mass of deionized water were added to the reactor, and the temperature was raised to 84° C., and the mixed monomer and initiator ammonium persulfate solution (the ammonium persulfate solution was prepared by dissolving 2.3 parts by mass of ammonium persulfate in 40 parts by mass of water) were simultaneously added dropwise to the reactor for 240 min. After the addition was completed, the mixture was kept warm at 92° C. for 80 min to obtain a binder.

[0170] The rest are the same as in Example 1.

[0171] Example 10

[0172] 1. The preparation of the binder comprises the following steps:

[0173] (a) 100 parts by mass of polypyrrole (number average molecular weight 500) was dissolved in 0.75 parts by mass of glycidyl methacrylate, 0.075 parts by mass of concentrated sulfuric acid as a catalyst was added, and the mixture was stirred and heated to 80° C. for reaction for 120 minutes to obtain modified polypyrrole.

[0174] (b) 15 parts by mass of modified polypyrrole as a modifying monomer and 100 parts by mass of methacrylic acid as a carboxyl monomer are mixed to obtain a mixed monomer.

[0175] (c) 305 parts by mass of deionized water were added to the reaction kettle, and the temperature was raised to 88° C. At the same time, a mixed monomer and an initiator ammonium persulfate solution (the ammonium persulfate solution is prepared by dissolving 2.3 parts by mass of ammonium persulfate in 40 parts by mass of water) were added dropwise to the reaction kettle for 180 min. After the addition was completed, the mixture was kept at 86° C. for 60 min to obtain a binder.

[0176] The rest are the same as in Example 1.

[0177] Embodiment 11

[0178] 1. The preparation of the binder comprises the following steps:

[0179] (a) 100 parts by mass of polypyrrole (number average molecular weight 3000) was dissolved in 7.5 parts by mass of glycidyl methacrylate, 0.075 parts by mass of concentrated sulfuric acid as a catalyst was added, and the mixture was stirred and heated to 80° C. for reaction for 120 minutes to obtain modified polypyrrole.

[0180] (b) 15 parts by mass of modified polypyrrole as a modifying monomer and 100 parts by mass of methacrylic acid as a carboxyl monomer are mixed to obtain a mixed monomer.

[0181] (c) 305 parts by mass of deionized water were added to the reaction kettle, and the temperature was raised to 88° C. At the same time, a mixed monomer and an initiator ammonium persulfate solution (the ammonium persulfate solution is prepared by dissolving 2.3 parts by mass of ammonium persulfate in 40 parts by mass of water) were added dropwise to the reaction kettle for 180 min. After the addition was completed, the mixture was kept at 86° C. for 60 min to obtain a binder.

[0182] The rest are the same as in Example 1.

[0183] Comparative Example 1

[0184] In Comparative Example 1, the binder prepared in step 1 is replaced by a conventional polyacrylic acid (PAA) binder.

[0185] Performance Testing

[0186] 1. The solid content, viscosity and pH value of the adhesives prepared in the above embodiments and comparative examples were tested respectively.

[0187] (1) Solid content test: Use a halogen moisture meter to test. Take about 1 to 1.2 g of the prepared adhesive and dry it at 130°C. If the mass change is less than 1 mg / 1 min, the solid content result of the adhesive can be obtained.

[0188] (2) Viscosity test: A rotational viscometer is used for the test. A No. 64 rotor is used. The selected rotor is installed on the instrument and placed in the obtained adhesive. The adhesive solution must be submerged in the rotor calibration scale. The test is performed at a speed of 40 rpm and the measurement time is set to 1 min. The viscosity result of the adhesive can be obtained.

[0189] (3) pH value test: Use a pH meter to test. Place the cleaned electrode into the binder to be tested to obtain the pH value of the binder.

[0190] The test results are shown in Table 1.

[0191] Table 1 Solid content, viscosity and pH value of the binder in each embodiment and comparative example

[0192]

[0193] 2. The peel strength, membrane resistance and discharge resistance of the positive electrode sheets prepared in the above-mentioned embodiments and comparative examples were tested respectively.

[0194] (1) Peel strength test (test of the adhesion of the conductive coating and the active material layer): The peel strength is tested by a universal tensile testing machine. During the test, take the rolled electrode and cut it into 25mm*20cm in length and width; take a flat steel plate with a size of about 50mm in width and 200mm in length, and stick a double-sided tape with a size of about 25mm*50mm in the center of one end of the steel plate. The double-sided tape needs to be smoothed so that it fits completely on the steel plate; place the cut electrode in the center of the steel plate with one end completely attached to the double-sided tape; use a universal tensile testing machine, clamp the steel plate (the side without the double-sided tape) with the bottom clamp and fix it vertically, clamp the electrode with the upper clamp (the side without the double-sided tape) so that the electrode and the steel plate are 180°, pull the electrode upward at a uniform speed of 50mm / min, and peel off the bonding surface of the electrode and the double-sided tape at a uniform speed. The peel strength obtained represents the peel strength of the electrode.

[0195] (2) Diaphragm resistance test: The diaphragm resistance is tested by a diaphragm resistance meter using the four-probe method.

[0196] (3) Discharge resistance test: At 25°C, the battery cell prepared with the obtained positive electrode sheet was allowed to stand for 30 min, charged to 3.65 V at a constant current of 1 / 2C, allowed to stand for 5 min, and then discharged to 50% SOC at a constant current of 1C. After standing for 60 min, the battery cell was discharged at a current of 2C for 10 s. The resistance value obtained is the value of 2C discharge for 10 s at 25°C and 50% SOC.

[0197] The test results are shown in Table 2.

[0198] Table 2 Peel strength, membrane resistance and discharge resistance of the electrode sheets of each embodiment and comparative example

[0199]

[0200] It can be seen from the data in Table 2 that, compared with Comparative Example 1, the electrode sheets using the adhesive of Examples 1-11 of the present application reduce the diaphragm resistance and discharge resistance, improve the conductivity of the electrode sheets, and improve the peel strength, that is, enhance the bonding force between the conductive coating and the active material layer.

[0201] In addition, the raw materials, proportions or operating conditions used in the preparation process of the binder provided in Examples 1-9 of the present application are all within the preferred range of the present invention, so that the binder prepared in Examples 1-9 obtains higher peel strength and lower diaphragm resistance and discharge resistance. Compared with Examples 1-9, the molecular weight of the polypyrrole used in the preparation process of the binder provided in Example 10 is lower, and its molecular weight is 500, which is not within the preferred range of the present invention, resulting in the diaphragm resistance and discharge resistance of the pole piece prepared therefrom being relatively high, and the conductivity is reduced. This shows that when the number average molecular weight of the polypyrrole used is too low, such as less than 2000, the conductivity is poor, which is not conducive to improving the conductivity of the binder. Compared with Examples 1-9, the binder provided in Example 11 increases the amount of modifier used in the preparation process, that is, increases the grafting rate of polypyrrole, resulting in the diaphragm resistance and discharge resistance of the pole piece prepared therefrom being relatively high, and the conductivity is reduced. This shows that when the amount of modifier added is too much, the conductive structure of the polypyrrole itself will be destroyed, resulting in poor conductivity of the binder.

[0202] 3. The swelling properties of the adhesives prepared in the above embodiments and comparative examples were tested respectively.

[0203] Swelling test: After drying at 80°C for 36 hours, adhesive films containing the adhesives of the above embodiments and comparative examples were prepared respectively (the adhesive films were obtained by weighing the same mass of the adhesives of the above embodiments and comparative examples in a quantitative container and drying at 105°C for 2 hours). The adhesive films were weighed and immersed in NMP solution maintained at 60°C for 24 hours, then the floating liquid was wiped dry and the weight was measured again to calculate the swelling rate.

[0204] The test results are shown in Table 3.

[0205] Table 3 Swelling rate of the binder in each embodiment and comparative example

[0206]

[0207] From the data in Table 3, it can be seen that compared with the traditional polyacrylic acid provided in Comparative Example 1, the binder provided in Examples 1-11 of the present invention, namely the modified polycarboxylic acid, has significantly increased swelling to NMP. Due to the increased swelling, the bonding force is improved, indicating that the modified polycarboxylic acid of the present invention can improve the bonding force between the conductive coating and the active material layer.

[0208] Parts of the present invention that are not described in detail are well known to those skilled in the art.

[0209] The basic principle of the present invention is described above in conjunction with specific embodiments. However, it should be pointed out that the advantages, strengths, effects, etc. mentioned in the present invention are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. must be possessed by each embodiment of the present invention. In addition, the specific details disclosed above are only for the purpose of illustration and facilitation of understanding, rather than limitation, and the above details do not limit the present invention to being implemented by adopting the above specific details.

[0210] It should be noted that the term "and / or" or " / " used in this document is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The singular forms of "a", "the" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0211] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0212] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A binder, characterized in that: The binder includes a modified polycarboxylic acid; The modified polycarboxylic acid comprises a carboxylic acid polymer and a modified polypyrrole grafted onto the carboxylic acid polymer; The preparation of the modified polycarboxylic acid comprises: The modifier and polypyrrole are reacted under a catalyst condition to obtain modified polypyrrole; Mixing the modified polypyrrole as a modified monomer with a carboxyl monomer to obtain a mixed monomer; The mixed monomers are polymerized to obtain a modified polycarboxylic acid; Wherein, the modifier includes at least one of vinyl siloxane or glycidyl methacrylate, and the hydrolysis product of the vinyl siloxane contains silanol groups, wherein the vinyl siloxane includes at least one of vinyl trimethoxy silane, vinyl triethoxy silane or γ-methacryloxy trimethoxy silane.

2. The adhesive according to claim 1, characterized in that The viscosity of the binder is 700-1500 mPa·s; And / or, the solid content of the binder is 20-30%; And / or, the pH value of the binder is 3-5.

3. The method for preparing the adhesive according to claim 1 or 2, characterized in that: The following steps are involved: The modifier and polypyrrole are reacted under a catalyst condition to obtain modified polypyrrole; Mixing the modified polypyrrole as a modified monomer with a carboxyl monomer to obtain a mixed monomer; Mixing the mixed monomer with an initiator to initiate a polymerization reaction to obtain the binder; The modifier includes at least one of vinyl siloxane and glycidyl methacrylate, and the vinyl siloxane includes at least one of vinyl trimethoxy silane, vinyl triethoxy silane or γ-methacryloxy trimethoxy silane.

4. The method for preparing the adhesive according to claim 3, characterized in that: The step of obtaining the modified polypyrrole satisfies at least one of the following characteristics (1) to (5): (1) The mass ratio of the modifier to the polypyrrole is (0.5-1): (100-200); (2) The number average molecular weight of the polypyrrole is 2000 to 5000; (3) The catalyst comprises at least one of concentrated sulfuric acid, tetrafluoroboric acid, perchloric acid or fluoroacetic acid; (4) The mass of the catalyst is 0.05% to 0.1% of the mass of the polypyrrole; (5) The reaction temperature is 75°C to 85°C, and the reaction time is 120 min to 180 min.

5. The method for preparing the adhesive according to claim 3, characterized in that: The step of obtaining the mixed monomer satisfies at least one of the following characteristics (1) to (2): (1) The mass ratio of the modified monomer to the carboxyl monomer is 1:(5-9); (2) The carboxyl monomer includes at least one of sodium styrene sulfonate, acrylic acid, methacrylic acid or carboxyethyl acrylate.

6. The method for preparing the adhesive according to any one of claims 3 to 5, characterized in that: The step of obtaining the binder satisfies at least one of the following characteristics (1) to (6): (1) The mass of the initiator is 1% to 5% of the mass of the mixed monomer; (2) The initiator includes at least one of sodium persulfate, ammonium persulfate or potassium persulfate; (3) Mixing the mixed monomer with an initiator to initiate a polymerization reaction specifically includes: Add water to the reaction device and heat it to 80°C to 90°C, and simultaneously drop the mixed monomer and the initiator into the reaction device, the dropwise addition time is 180min to 240min, and after the dropwise addition is completed, keep the temperature at 85°C to 95°C for 60min to 80min; (4) The viscosity of the binder is 700 to 1500 mPa•s; (5) The solid content of the binder is 20 to 30%; (6) The pH value of the binder is 3 to 5.

7. A pole piece, characterized in that: The pole piece comprises: current collector; A conductive coating, disposed on at least one side surface of the current collector along the thickness direction; the conductive coating comprises a conductive material and the binder according to any one of claims 1 to 2 or the binder prepared according to the method according to any one of claims 3 to 6; and The active material layer is arranged on the surface of the conductive coating layer which is away from the current collector.

8. The pole piece according to claim 7, characterized in that: The pole piece satisfies at least one of the following characteristics (1) to (3): (1) The conductive material includes at least one of conductive carbon black, conductive graphite, carbon nanotubes, carbon nanofibers or graphene; (2) The mass ratio of the binder to the conductive material is (4-6): (6-4); (3) The active material layer includes an active material, and the active material includes lithium iron phosphate.

9. A battery, characterized in that: The battery comprises the pole piece according to claim 7 or 8.

Citation Information

Patent Citations

  • Conductive binder and preparation method thereof, current collector, electrode and battery

    CN115881966A