Anti-pinhole agent, nickel plating solution, nickel plating method and nickel-plated part
The anti-pin hole agent prepared by the synergistic action of alcohol defoaming agents, thiourea compounds, sodium naphthalene disulfonate and leveling agents in a specific proportion has solved the needle under the influence of the stability and impurities of nickel plating solution. The hole problem achieves the effect of efficiently preventing pinholes and improving the leveling of nickel plating layer.
Patent Information
- Application Number
- CN202411090618.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing pinhole anti-pin hole agent has a great impact on the stability of nickel plating solutions, and cannot effectively prevent the generation of pinholes when there are many impurities.
The anti-pin pore agent prepared by using the synergistic action of alcohol defoaming agents, thiourea compounds, sodium naphthalene disulfonate, sodium phenyldithiopropane sulfonate and leveling agent with specific ratios, to control the nickel plating rate , improve the leveling of the nickel plating layer and use it without traditional surfactants, to improve the stability and recycling performance of the nickel plating solution.
In the case of impurities, the generation of pinholes is prevented, the flatness of the nickel plating layer and the stability of the nickel plating solution are improved, the service life of the nickel plating solution is extended, and a high-quality nickel plating layer is formed.
Smart Images

Figure CN118639221B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical nickel plating, and in particular relates to an anti-pinhole agent, a nickel plating solution, a nickel plating method and a nickel-plated part. Background Art
[0002] The most commonly used reducing agent for chemical nickel plating is hypophosphite. The principle is to use the catalytic effect of the catalyst to reduce the hypophosphite (H 2 PO 2- ) catalytically dehydrogenates on the catalytic surface to form active hydrides, which are oxidized to phosphites; the active hydrides undergo a reduction reaction with nickel ions in the solution to deposit nickel, which itself is oxidized to hydrogen, namely:
[0003] 2H 2 PO 2- +2H 2 O+Ni 2+ →Ni0+H 2 ↑+4H + +2HPO 3 2-
[0004] At the same time, part of the hypophosphite in the solution is reduced by hydride to elemental phosphorus and enters the coating, namely:
[0005] H 2 PO 2- +[H + ](catalytic surface)→P+H 2 O+OH - , forming a chemical plating layer of NiP alloy, which has an amorphous thin film structure.
[0006] Pinholes are the most common faults in the nickel plating process. Pinholes are tiny holes that can be seen by the naked eye. Pinholes are caused by bubbles left on the cathode surface, which cause insulation and prevent metal from being deposited there. The area around the bubbles continues to thicken. Later, the bubbles escape or burst, leaving a concave mark there, thus forming pinholes.
[0007] Pinhole failure is a rather complicated problem. If the pinhole is caused by non-standard operating conditions or solution composition, it is easy to remedy. It can usually be solved by adjusting the operating conditions or solution composition to meet the requirements. However, if the pinhole is caused by contamination of the solution with impurities (metallic impurities or organic impurities), or the viscosity of the plating solution is too high, the root cause must be found and the right remedy must be prescribed to solve it.
[0008] In the prior art, in the absence of impurities, one of the most commonly used methods is to add an anti-pinhole agent. In glossy nickel plating, a wetting agent such as sodium dodecyl sulfate can be added in an amount of 0.01 to 0.05 g / L. In ordinary nickel plating, 0.1 ml / L of hydrogen peroxide can be added after work is completed every day. However, excessive use of such an anti-pinhole agent can easily cause instability of the chemical nickel plating solution, making it easy for nickel particles to deposit on the wall of the reaction vessel and causing the self-decomposition of the plating solution. If the plating solution contains too many impurities, the effect of the above method will also be affected, or even ineffective.
[0009] Therefore, an anti-pinhole agent that has little effect on the stability of the nickel plating solution and has a good anti-pinhole effect even when containing impurities has not yet been developed. Summary of the invention
[0010] The invention provides an anti-pinhole agent, which is used to solve the problem that the anti-pinhole agent in the prior art has a great influence on the stability of a nickel plating solution and cannot improve the pinhole situation when there are many impurities.
[0011] The invention provides a nickel plating solution, comprising the above-mentioned anti-pinhole agent, which has good stability, long cycle service life and good anti-pinhole effect.
[0012] The present invention provides a nickel plating method, which allows the anti-pinhole agent or the nickel plating solution to participate in chemical nickel plating treatment, thereby effectively preventing the generation of pinholes.
[0013] The invention provides a nickel-plated part, comprising a workpiece to be plated and a nickel-plated layer located on at least a part of the surface of the workpiece to be plated. The nickel-plated layer is obtained by the nickel-plating method and has good molding.
[0014] In a first aspect, the present invention provides an anti-pinhole agent, comprising the following components in parts by mass: 0.5 to 5 parts of an alcohol defoamer, 0.001 to 0.05 parts of a semicarbazide compound, 0.0005 to 0.6 parts of sodium naphthalene disulfonate, 0.0004 to 0.006 parts of sodium phenyl disulfide propane sulfonate, and 0.0005 to 0.025 parts of a leveler.
[0015] Further, the invention comprises 0.0004-0.005 parts by mass of sodium phenyl disulfide propane sulfonate; and / or,
[0016] The leveling agent is included in an amount of 0.0005 to 0.02 parts by mass.
[0017] Furthermore, the alcohol defoaming agent contains no more than 3 carbon atoms.
[0018] Furthermore, the alcohol defoaming agent includes at least one of isopropyl alcohol, ethylene glycol or glycerol.
[0019] Furthermore, the semicarbazide compound includes at least one of semicarbazide, N-methyl semicarbazide and phenyl semicarbazide.
[0020] Furthermore, the leveler includes at least one of copper sulfate or bismuth chloride.
[0021] In a second aspect, the present invention provides a nickel plating solution, comprising the anti-pinhole agent of the first aspect.
[0022] Furthermore, the mass percentage of the anti-pinhole agent in the nickel plating solution is 0.06-0.48%.
[0023] In a third aspect, the present invention provides a nickel plating method, wherein the anti-pinhole agent of the first aspect or the nickel plating solution of the second aspect participates in a chemical nickel plating process.
[0024] Further, the temperature of the chemical nickel plating treatment is 80-85° C.; and / or,
[0025] The chemical nickel plating treatment time is 60-90 minutes; and / or,
[0026] The pH value of the chemical nickel plating treatment is 5-7.
[0027] In a fourth aspect, the present invention provides a nickel-plated part, comprising a workpiece to be plated and a nickel-plated layer located on at least a portion of the surface of the workpiece to be plated, wherein the nickel-plated layer is obtained by the nickel plating method described in the third aspect.
[0028] The anti-pinhole agent provided by the present invention can control the nickel plating rate through the synergistic effect of alcohol defoamers, semicarbazide compounds, sodium naphthalene disulfonate, sodium phenyl disulfide propane sulfonate and a leveling agent in a specific ratio, thereby achieving a good anti-pinhole effect and improving the leveling property of the nickel plating layer in the presence of impurities; and the anti-pinhole agent does not contain traditional surfactants, can be used in a wider range, and improves the stability and recycling performance of the nickel plating solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is an appearance diagram of the nickel-plated part obtained in Example 1;
[0030] Figure 2 This is the appearance of the nickel-plated part obtained in Comparative Example 1;
[0031] Figure 3 This is the appearance of the nickel-plated part prepared in Comparative Example 2. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In a first aspect, the present invention provides an anti-pinhole agent, comprising the following components in parts by mass: 0.5 to 5 parts of an alcohol defoamer, 0.001 to 0.05 parts of a semicarbazide compound, 0.0005 to 0.6 parts of sodium naphthalene disulfonate, 0.0004 to 0.006 parts of sodium phenyl disulfide propane sulfonate, and 0.0005 to 0.025 parts of a leveler.
[0034] The invention provides an anti-pinhole agent, which comprises the following components by mass: 0.5-5 parts of an alcohol defoamer, 0.001-0.05 parts of a semicarbazide compound, 0.0005-0.6 parts of sodium naphthalene disulfonate, 0.0004-0.006 parts of sodium phenyl disulfide propane sulfonate and 0.0005-0.025 parts of a leveler. The inventor speculates that, through the synergistic effect of the alcohol defoamer, the semicarbazide compound, the sodium naphthalene disulfonate, the sodium phenyl disulfide propane sulfonate and the leveler in a specific ratio, some components in the anti-pinhole agent can be adsorbed on the surface of the coating, so that bubbles are prevented from being generated and staying, and bubbles are more easily diffused and broken, so that the nickel plating rate can be controlled, and a good anti-pinhole effect is achieved in the presence of impurities, and the leveling property of the nickel plating layer is improved. In addition, the anti-pinhole agent does not contain a traditional surfactant, so that the anti-pinhole agent can be used in a larger range, the stability of the nickel plating solution is improved, and the recycling performance of the nickel plating solution is improved.
[0035] The anti-pinhole agent provided by the present invention can control the nickel plating rate through the synergistic effect of alcohol defoamers, semicarbazide compounds, sodium naphthalene disulfonate, sodium phenyl disulfide propane sulfonate and a leveling agent in a specific ratio, thereby achieving a good anti-pinhole effect and improving the leveling property of the nickel plating layer in the presence of impurities; and the anti-pinhole agent does not contain traditional surfactants, can be used in a wider range, and improves the stability and recycling performance of the nickel plating solution.
[0036] Furthermore, the solution comprises 0.0004-0.005 parts of sodium disulfide propane sulfonate and 0.0005-0.02 parts of a leveler by mass; this can further achieve efficient defoaming, and can further improve the stability of the nickel plating solution and the pinhole effect of the nickel plating layer.
[0037] Furthermore, the alcohol defoaming agent contains no more than 3 carbon atoms.
[0038] The inventors have found that the use of an alcohol defoaming agent with no more than 3 carbon atoms can better cooperate with other components in the anti-pinhole agent to achieve a synergistic effect, further defoam efficiently, and further improve the stability of the nickel plating solution and improve the pinhole effect of the nickel plating layer.
[0039] In a specific embodiment, the alcohol defoaming agent includes at least one of isopropyl alcohol, ethylene glycol or glycerol.
[0040] When the alcohol defoaming agent includes at least one of isopropyl alcohol, ethylene glycol or glycerol, it can further improve the solubility of organic impurities in the nickel plating solution, reduce the adsorption of impurities on the metal surface, further reduce the viscosity of the metal surface, and further diffuse and rupture the bubbles.
[0041] In a specific embodiment, the semicarbazide compound includes at least one of semicarbazide, N-methyl semicarbazide, and phenyl semicarbazide.
[0042] When the semicarbazide compound includes at least one of semicarbazide, N-methyl semicarbazide and phenyl semicarbazide, the reaction rate can be further controlled, the dense generation of bubbles can be reduced, and the anti-pinhole effect can be further improved.
[0043] In one embodiment, the leveler includes at least one of copper sulfate or bismuth chloride.
[0044] The inventors found that when the leveling agent is selected from at least one of copper sulfate or bismuth chloride, it can better cooperate with other components in the anti-pinhole agent to play a synergistic role, further improve the leveling of the nickel plating layer, and reduce the generation of pinholes.
[0045] In a second aspect, the present invention provides a nickel plating solution, comprising the anti-pinhole agent of the first aspect.
[0046] The nickel plating solution provided by the present invention comprises the anti-pinhole agent of the first aspect. The anti-pinhole agent can control the nickel plating reaction rate through the synergistic effect of alcohol defoaming agent, semicarbazide compound, sodium naphthalene disulfonate, sodium phenyl disulfide propane sulfonate and leveling agent in a specific ratio, so as to achieve good anti-pinhole effect and improve the leveling property of the nickel plating layer in the presence of impurities; and the anti-pinhole agent does not contain traditional surfactants, so that the anti-pinhole agent can be used in a wider range, thereby improving the stability of the nickel plating solution and the recycling performance of the nickel plating solution.
[0047] Furthermore, the mass percentage of the anti-pinhole agent in the nickel plating solution is 0.06-0.48%.
[0048] By further limiting the mass percentage of the anti-pinhole agent in the nickel plating solution, the nickel plating effect of the nickel plating solution can be further improved, the anti-pinhole effect can be further improved, and the leveling of the nickel plating layer can be improved. The mass percentage of the anti-pinhole agent in the nickel plating solution can be further limited to 0.1-1%.
[0049] In a third aspect, a nickel plating method is provided, wherein the anti-pinhole agent of the first aspect or the nickel plating solution of the second aspect is involved in chemical nickel plating treatment.
[0050] The nickel plating method provided by the present invention allows the anti-pinhole agent of the first aspect or the nickel plating solution of the second aspect to participate in chemical nickel plating treatment, and the nickel plating rate can be controlled through the synergistic effect of alcohol defoamers, semicarbazide compounds, sodium naphthalene disulfonate, sodium phenyl disulfide propane sulfonate and leveling agents in specific proportions in the anti-pinhole agent, so as to achieve a good anti-pinhole effect and improve the leveling property of the nickel plating layer in the presence of impurities; and the anti-pinhole agent does not contain traditional surfactants, can be used in a wider range, and improves the stability and recycling performance of the nickel plating solution.
[0051] The present invention does not specifically limit the steps and process parameters of the nickel plating method, and it can be carried out using methods commonly used in the art; optionally, the chemical nickel plating process may include: directly contacting the workpiece to be plated with a nickel plating solution, performing a chemical nickel plating process, and obtaining a nickel-plated part.
[0052] As is common knowledge among those skilled in the art, in order to improve the bonding strength of the aluminum alloy nickel plating layer, the method also includes the step of pre-treating the workpiece to be plated before the chemical nickel plating treatment; optionally, the pre-treatment includes degreasing, corrosion, descaling, zinc precipitation, zinc stripping, zinc immersion and pre-plating treatment, and multiple water washings can be performed after each treatment step.
[0053] The present invention does not specifically limit the relevant process parameters in the above-mentioned pretreatment. In one embodiment, the degreasing liquid in the degreasing treatment includes at least one of a neutral degreasing liquid, a weak alkaline degreasing liquid, and a weak acidic degreasing liquid. The degreasing treatment adopts ultrasonic degreasing. The degreasing treatment time is 5 to 10 minutes and the temperature is 30 to 60°C.
[0054] The corrosion solution in the corrosion treatment includes at least one of sodium carbonate, sodium pyrophosphate, and sodium bicarbonate, the pH value of the corrosion solution is 11-12, the corrosion treatment time is 60-90 seconds, and the temperature is 15-35°C;
[0055] The descaling liquid in the descaling treatment includes at least one of nitric acid and hydrofluoric acid, and the descaling treatment time is 40-70 seconds and the temperature is 15-35°C;
[0056] The zinc precipitation solution in the zinc precipitation treatment includes at least one of sodium hydroxide, zinc oxide, corrosion inhibitor, complexing agent and surfactant. The zinc precipitation treatment time is 40-60 seconds and the temperature is 15-22°C.
[0057] The zinc stripping solution in the zinc stripping treatment includes at least one of nitric acid, and the zinc stripping treatment time is 20-40 seconds and the temperature is 15-35°C;
[0058] The zinc stripping solution in the zinc immersion treatment includes at least one of sodium hydroxide, zinc oxide, a corrosion inhibitor, a complexing agent, and a surfactant. The zinc immersion treatment time is 40 to 60 seconds and the temperature is 15 to 22°C.
[0059] The pre-plating treatment is carried out using the nickel plating solution provided by the present invention, or a nickel plating solution commonly used in the art. The pH value of the nickel plating solution is 8-9, the pre-plating treatment time is 6-10 minutes, and the temperature is 30-40°C.
[0060] As is common knowledge among those skilled in the art, the nickel plating method may further include a step of drying the nickel-plated parts; wherein the drying may be carried out by natural air drying or by hot air drying at 70-90°C, but is not limited thereto.
[0061] Optionally, the chemical nickel plating treatment temperature is 80-85° C., the time is 60-90 min, and the pH value is 5-7.
[0062] It can be understood that by limiting the temperature, time and pH value of the chemical nickel plating process, the effect of the nickel plating method can be further improved, the flatness of the nickel plating layer can be improved, and the generation of pinholes can be further reduced.
[0063] In a fourth aspect, the present invention provides a nickel-plated part, comprising a workpiece to be plated and a nickel-plated layer located on at least a portion of the surface of the workpiece to be plated, wherein the nickel-plated layer is obtained by the nickel plating method of the third aspect.
[0064] The present invention does not limit the specific type of the workpiece to be plated, as long as the surface of the workpiece can be plated with a metal nickel layer.
[0065] The nickel-plated part provided by the invention has a nickel-plated layer with a flat surface and a good shape.
[0066] Hereinafter, an anti-pinhole agent, a nickel plating solution, a nickel plating method and a nickel-plated part provided by the present invention are introduced in detail through specific embodiments.
[0067] Example 1
[0068] The workpiece to be plated in this embodiment is an aluminum alloy air conditioning disk.
[0069] The anti-pinhole agent in this embodiment includes: 1 g / L isopropyl alcohol, 0.002 g / L thiosemicarbazide, 0.002 g / L sodium naphthalene disulfonate, 0.002 g / L sodium phenyl disulfide propane sulfonate and 0.002 g / L copper sulfate, and the solvent is water.
[0070] The nickel plating solution in this embodiment includes: 25 g / L nickel sulfate, 15 g / L ammonium citrate, 10 g / L succinic acid, 20 g / L sodium acetate, 12 g / L lactic acid, 0.005 g / L sodium dodecylbenzene sulfonate, 0.003 g / L polyethylene glycol 2000, 0.01 g / L ferric sulfate, 22 g / L sodium hypophosphite, 0.002 g / L thiourea, 0.002 g / L potassium iodate, and 1.008 g / L anti-pinhole agent, the solvent is water, and the pH value of the nickel plating solution is 6.
[0071] The nickel plating method comprises the following steps:
[0072] (1) Soak the workpiece to be plated in a degreasing solution, perform ultrasonic degreasing treatment at 40°C for 5 minutes, and then wash it with water three times to obtain a first pre-treated workpiece;
[0073] (2) placing the first pre-treated workpiece in a corrosion solution, corroding it at 25°C for 60 seconds, and then washing it with water three times to obtain a second pre-treated workpiece;
[0074] (3) placing the second pre-treated workpiece in a descaling solution for 60 seconds at 25°C, and washing with water three times to obtain a third pre-treated workpiece;
[0075] (4) placing the moving disk into the zinc immersion solution at 25°C for 50 seconds, and then washing it with water three times to obtain the fourth pre-treated workpiece;
[0076] (5) placing the fourth pre-treated workpiece into a zinc stripping solution for zinc stripping treatment at 25° C. for 30 seconds, and then washing with water three times to obtain a fifth pre-treated workpiece;
[0077] (6) The fifth pre-treated workpiece is placed in the zinc dipping solution again and zinc-dipped for 25 seconds at 25° C., and then washed with water three times to obtain a sixth pre-treated workpiece;
[0078] (7) placing the sixth pre-treated workpiece into a pre-plating solution for pre-plating at 30° C. for 9 min, the temperature is 30° C., the pH value is 9, and then washing with water three times to obtain a pre-plated workpiece;
[0079] Wherein, the pre-plating solution adopts a nickel plating solution;
[0080] (8) The pre-plated workpiece is placed in a nickel plating solution and subjected to chemical nickel plating treatment at 83°C for 80 minutes to obtain a nickel-plated part.
[0081] Example 2
[0082] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent includes: 0.5 g / L isopropyl alcohol, 0.001 g / L thiosemicarbazide, 0.0005 g / L sodium naphthalene disulfonate, 0.0004 g / L sodium phenyl disulfide propane sulfonate, and 0.0005 g / L copper sulfate.
[0083] Example 3
[0084] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent includes: 5 g / L isopropyl alcohol, 0.05 g / L thiosemicarbazide, 0.06 g / L sodium naphthalene disulfonate, 0.005 g / L sodium phenyl disulfide propane sulfonate, and 0.02 g / L copper sulfate.
[0085] Example 4
[0086] The difference between this embodiment and embodiment 1 is that the isopropyl alcohol in the anti-pinhole agent is replaced by 1-pentanol.
[0087] Example 5
[0088] The difference between this embodiment and embodiment 1 is that the isopropyl alcohol in the anti-pinhole agent is replaced by methanol.
[0089] Example 6
[0090] The difference between this embodiment and embodiment 1 is that the thiosemicarbazide in the anti-pinhole agent is replaced by thiourea.
[0091] Example 7
[0092] The difference between this embodiment and embodiment 1 is that the copper sulfate in the anti-pinhole agent is replaced by cerium sulfate.
[0093] Example 8
[0094] The difference between this embodiment and embodiment 1 is that the amount of the anti-pinhole agent added to the nickel plating solution is 0.05 g / L.
[0095] Example 9
[0096] The difference between this embodiment and embodiment 1 is that in step (8), the temperature of the chemical nickel plating treatment is 88°C.
[0097] Example 10
[0098] The difference between this embodiment and embodiment 1 is that in step (8), the time of chemical nickel plating treatment is 120 minutes.
[0099] Embodiment 11
[0100] The difference between this embodiment and embodiment 1 is that the pH value of the nickel plating solution is 7.
[0101] Example 12
[0102] The nickel plating solution in this embodiment includes: 20 g / L nickel sulfate, 10 g / L sodium citrate, 15 g / L sodium acetate, 15 g / L lactic acid, 8 g / L triethanolamine, 0.005 g / L sodium dodecyl sulfate, 22 g / L sodium hypophosphite, 0.002 g / L lead acetate, 0.002 g / L potassium iodate, and 1.008 g / L anti-pinhole agent, the solvent is water, and the pH value of the nickel plating solution is 6.
[0103] Example 13
[0104] The nickel plating solution in this embodiment includes: 27 g / L nickel sulfate, 12 g / L EDTA, 10 g / L succinic acid, 20 g / L sodium acetate, 13 g / L lactic acid, 5 g / L tartaric acid, 0.005 g / L sodium dodecylbenzene sulfonate, 0.003 g / L polyethylene glycol 2000, 0.005 g / L ceric sulfate, 25 g / L sodium hypophosphite, 0.002 g / L thiourea, 0.001 g / L sodium thiosulfate, and 1.008 g / L anti-pinhole agent, the solvent is water, and the pH value of the nickel plating solution is 6.
[0105] Comparative Example 1
[0106] The difference between this comparative example and Example 1 is that the nickel plating solution does not include an anti-pinhole agent.
[0107] Comparative Example 2
[0108] The difference between this comparative example and Example 1 is that the nickel plating solution includes: 15 g / L nickel sulfate hexahydrate, 25 g / L sodium tungstate dihydrate, 20 g / L sodium citrate dihydrate, 0.1 g / L triethanolamine, 14 g / L lactic acid, 12 g / L ammonium acetate, 25 g / L sodium hypophosphite, 1.5 mg / L isothioureapropanesulfonic acid inner salt, 6.5 mg / L potassium iodate, 3.6 mg / L sodium thiocyanate, 3.5 mg / L nonylphenol polyoxyethylene ether, 16 mg / L sodium dodecyl sulfate, 1 mg / L tellurium dioxide, 5.5 mg / L potassium antimony tartrate, and 15 mg / L sodium saccharin.
[0109] Comparative Example 3
[0110] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent only includes: 5 g / L of isopropyl alcohol.
[0111] Comparative Example 4
[0112] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent only includes: 5 g / L isopropyl alcohol and 0.05 g / L thiosemicarbazide.
[0113] Comparative Example 5
[0114] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent only includes: 0.06 g / L sodium naphthalene disulfonate, 0.005 g / L sodium phenyl disulfide propane sulfonate, and 0.02 g / L copper sulfate.
[0115] Comparative Example 6
[0116] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent only includes: 5 g / L isopropyl alcohol, 0.05 g / L thiosemicarbazide, 0.06 g / L sodium naphthalene disulfonate, and 0.005 g / L sodium phenyl disulfide propane sulfonate.
[0117] Comparative Example 7
[0118] The difference between this embodiment and embodiment 1 is that the content of isopropyl alcohol in the anti-pinhole agent is 0.3 g / L.
[0119] Comparative Example 8
[0120] The difference between this embodiment and embodiment 1 is that the content of thiosemicarbazide in the anti-pinhole agent is 0.0005 g / L.
[0121] Comparative Example 9
[0122] The difference between this embodiment and embodiment 1 is that the content of sodium naphthalene disulfonate in the anti-pinhole agent is 0.7 g / L.
[0123] Comparative Example 10
[0124] The difference between this embodiment and embodiment 1 is that the content of sodium phenyl disulfide propane sulfonate in the anti-pinhole agent is 0.007 g / L.
[0125] Comparative Example 11
[0126] The difference between this embodiment and embodiment 1 is that the content of copper sulfate in the anti-pinhole agent is 0.04 g / L.
[0127] Comparative Example 12
[0128] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent does not contain isopropyl alcohol.
[0129] Comparative Example 13
[0130] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent does not contain thiosemicarbazide.
[0131] Comparative Example 14
[0132] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent does not contain sodium naphthalene disulfonate.
[0133] Comparative Example 15
[0134] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent does not contain sodium phenyl disulfide propane sulfonate.
[0135] Comparative Example 16
[0136] The difference between this embodiment and embodiment 1 is that the anti-pinhole agent does not contain copper sulfate.
[0137] Test Example 1
[0138] The nickel-plated parts prepared in the above-mentioned embodiments and comparative examples were cleaned and the appearance of the nickel-plated layer was observed. In particular, since the nickel-plated parts need to be continuously replenished with reagents to ensure that the various components in the nickel-plating solution are always kept at the original content when the nickel-plated parts are subjected to chemical nickel plating, one cycle means that the original nickel source in the nickel-plating solution is completely consumed, that is, the replenished nickel source reaches the original content; the results are shown in Table 1.
[0139] Figure 1 This is the appearance of the nickel-plated part obtained in Example 1. Figure 2 This is the appearance of the nickel-plated part obtained in Comparative Example 1. Figure 3 This is the appearance of the nickel-plated part prepared in Comparative Example 2.
[0140] Table 1
[0141]
[0142]
[0143]
[0144] As can be seen from Table 1, the nickel-plated parts that are treated with chemical nickel plating using the anti-pinhole agent provided by the present invention can form a smooth nickel-plated layer, the nickel-plated layer has no pinholes or has one or two tiny pinholes that are difficult to find, and the nickel-plating solution is stable and has no nickel deposition, and the anti-pinhole agent and the nickel-plating solution can be recycled.
[0145] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An anti-pinhole agent, characterized in that: The invention comprises the following components by mass: 0.5-5 parts of alcohol defoamer, 0.001-0.05 parts of thiosemicarbazide compound, 0.0005-0.6 parts of sodium naphthalene disulfonate, 0.0004-0.006 parts of sodium phenyl disulfide propane sulfonate and 0.0005-0.025 parts of leveler; the leveler comprises at least one of copper sulfate or cerium sulfate.
2. The anti-pinhole agent according to claim 1, characterized in that: The sodium phenyl disulfide propane sulfonate comprises 0.0004-0.005 parts by mass; and / or, The leveling agent is included in an amount of 0.0005 to 0.02 parts by mass.
3. The anti-pinhole agent according to claim 1, characterized in that: The alcohol defoamer contains no more than 3 carbon atoms.
4. The anti-pinhole agent according to claim 1, characterized in that: The alcohol defoaming agent includes at least one of isopropanol, ethylene glycol or glycerol.
5. The anti-pinhole agent according to claim 1, characterized in that: The semicarbazide compound includes at least one of semicarbazide, N-methyl semicarbazide and phenyl semicarbazide.
6. A nickel plating solution, characterized in that The invention comprises the anti-pinhole agent according to any one of claims 1 to 5; the mass percentage of the anti-pinhole agent in the nickel plating solution is 0.06-0.48%.
7. A nickel plating method, characterized in that: The anti-pinhole agent according to any one of claims 1 to 5 or the nickel plating solution according to claim 6 is involved in chemical nickel plating treatment.
8. The nickel plating method according to claim 7, characterized in that: The temperature of the chemical nickel plating treatment is 80-85° C.; and / or, The chemical nickel plating treatment time is 60-90 minutes; and / or, The pH value of the chemical nickel plating treatment is 5-7.