A POY / FDY universal production equipment and its application
By installing and optimizing the drafting and setting device and main network controller on the POY production equipment, the problem of POY equipment being difficult to produce FDY has been solved, efficient production of FDY products has been achieved, and product quality and production stability have been improved.
Patent Information
- Application Number
- CN202411112515.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Existing POY production equipment lacks a drafting and setting device and a main network controller, making it difficult to produce FDY products. It is also difficult to install a drafting and setting device in FDY equipment on POY equipment due to space constraints and reduced operating efficiency.
A kind of POY/FDY general production equipment is designed. By installing the drafting and setting device and the main network controller on the POY production equipment, and optimizing the specifications, arrangement and rotation of the heat roller and dividing roller, the size of the equipment is reduced to adapt to the POY equipment. space while ensuring adequate heating and shaping of the tow.
Alternate production of POY and FDY products is realized, the structure and layout of the drafting and setting device are optimized, the drafting and setting effect of the tow and product quality are improved, the excessive activity and wear of the fiber molecular chains are reduced, and the production stability is improved and fiber properties.
Smart Images

Figure CN118639374B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of spinning equipment and relates to POY / FDY universal production equipment and application. Background Art
[0002] In the textile industry, fully drawn yarn (FDY) and pre-oriented yarn (POY) are the two main varieties of polyester filaments, each playing an indispensable role in many fields such as textiles, clothing, and industrial fabrics. FDY is widely used in high-end textiles and special functional materials due to its high orientation, medium crystallinity, and excellent physical properties; while POY has become one of the widely used raw materials in the textile industry due to its good processing performance and low cost. The two not only have their own advantages in performance, but also show a complementary trend in market demand, jointly supporting the prosperity and development of the chemical fiber market.
[0003] However, the existing technology has encountered insurmountable obstacles in this field. Specifically, there are significant differences in the production process of FDY and POY. The production process of FDY requires more complex drafting and networking treatment to ensure the final performance of the product. This process complexity makes it difficult to use FDY equipment (such as FDY production equipment in the existing technology). Figure 2 It is relatively easy to transform the FDY equipment to spin POY products (such as patent application CN112458580B, patent application CN102660786A), because the FDY equipment itself has all the necessary conditions for producing high-quality products. Figure 1 Trying to produce FDY on a 200-meter-high (0.1-meter) surface becomes extremely difficult.
[0004] The core of the problem is that the POY production equipment was not designed with the drafting and shaping device and main network device required for FDY production in mind. These two devices are indispensable components of the FDY production process, and they play a decisive role in the heating, drafting and shaping of the tow. Since the POY equipment lacks these key devices, it cannot be directly used to produce FDY products.
[0005] In order to overcome this problem, in theory, the production of FDY can be achieved by adding a drafting and shaping device and a main network device to the POY equipment. However, there are many challenges in actual operation. First, the drafting and shaping device in the FDY production equipment is large in size, and the spatial layout of the POY production equipment is often compact, which makes it difficult to accommodate such a large additional equipment. Secondly, even if the drafting and shaping device is barely installed on the POY equipment through technical transformation, the operating efficiency of the equipment will be greatly reduced due to space limitations.
[0006] What is more serious is that if the specifications of the GR1 and GR2 groups are reduced in order to adapt to the space of the POY equipment (the GR1 and GR2 groups are key components in the drafting and shaping device, responsible for heating and drawing the tow), it will directly lead to a significant reduction in the number of windings of the tow on the GR1 and GR2 groups. This change will seriously affect the heating effect of the tow, making it impossible for the tow to be fully heated and shaped during the drafting process, thereby affecting the quality of the final product. Summary of the invention
[0007] The purpose of the present invention is to solve the problems existing in the prior art and to provide a POY / FDY universal production equipment and application.
[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] A POY / FDY general production equipment A1, comprising a spinning assembly, a cooling bellows, an oiling device, a pre-netting device, a godet a, a godet b and a winding machine, which are all POY production equipment, and also comprises a drafting and shaping device and a main netting device;
[0010] The drafting and shaping device is located below the pre-network device and at the upper left of the godet roller a;
[0011] The drafting and setting device consists of a heat box and a GR1 group and a GR2 group located in the heat box at the same time. The GR1 group consists of a heat roller a and a wire separation roller a, and the GR2 group consists of a heat roller b and a wire separation roller b.
[0012] The central axes of the heat roller a, heat roller b, wire separation roller a and wire separation roller b are parallel to the front-rear direction;
[0013] The upper surfaces of the hot roller a and the hot roller b are flush, the hot roller a is located on the left side of the hot roller b, the two are arranged at a distance of 100-140 mm, the wire separation roller a is located below the hot roller a and the two are arranged at a distance, and the wire separation roller b is located below the hot roller b and the two are arranged at a distance;
[0014] The rightmost vertical plane of the hot roller a passes through the fiber outlet of the pre-network device;
[0015] Both hot roller a and hot roller b rotate clockwise;
[0016] The diameter of the hot roller a and the hot roller b is 150-190 mm, and the length is 180-200 mm; the diameter of the wire separation roller a and the wire separation roller b is 75-95 mm, and the length is 180-200 mm;
[0017] The main network device is located between the wire roller a and the wire roller b.
[0018] It is difficult to produce FDY with the POY production equipment of the prior art because the POY production equipment has no drafting and shaping device and main interlacing device. The production of FDY requires drafting and shaping and interlacing treatment, so it is necessary to install a drafting and shaping device and a main interlacing device on the POY production equipment. However, it is difficult to directly add the drafting and shaping device in the FDY production equipment to the POY production equipment for the following reasons:
[0019] The drafting and shaping device in the FDY production equipment is relatively large in size, and there is not enough space in the POY production equipment to accommodate the drafting and shaping device in the FDY production equipment. At this time, it is necessary to reduce the size of the drafting and shaping device in the FDY production equipment. For this purpose, the present invention reduces the specifications of the GR1 group and the GR2 group (the diameter of the hot roller a and the hot roller b in the prior art is 220 mm, and the length is 350-400 mm, while the diameter of the hot roller a and the hot roller b in the present invention is 150-190 mm, and the length is 180-200 mm; the wire separation roller a and the wire separation roller b in the prior art are 220 mm, and the length is 350-400 mm, respectively. The diameter of the FDY production equipment is 110 mm, and the length is 350-400 mm. In the present invention, the diameter of the filament separation roller a and the filament separation roller b is 75-95 mm, and the length is 180-200 mm). However, this has created a new problem - the specifications of the GR1 group and the GR2 group are reduced, and the number of windings of the filament bundle on the GR1 group and the GR2 group will be significantly reduced. The filament bundle cannot be fully heated, and thus cannot be effectively drawn and shaped. Therefore, it is necessary to change the layout of the drawing and shaping device in the FDY production equipment so that the filament bundle can be effectively drawn and shaped. The principle of the present invention is as follows:
[0020] (1) In the drafting and shaping device of the present invention, "the separating roller a is located below the hot roller a and the two are arranged at a distance", and "the vertical surface of the hot roller a at the rightmost side passes through the fiber outlet of the pre-network device". This allows the filament bundle to run along the shortest route to contact the hot roller a after leaving the pre-network device, making full use of the residual heat of the filament bundle to reduce the power load of the hot roller a, thereby improving the heating effect of the filament bundle on the hot roller, and further facilitating the effective drafting and shaping of the filament bundle;
[0021] (2) In the drafting and shaping device of the FDY production equipment, the hot roller a rotates counterclockwise, and the hot roller b rotates clockwise. During the high-speed rotation of the hot roller a and the hot roller b, a certain amount of airflow is generated, forming two airflows in different directions. If the drafting is carried out in the same insulation box, the two airflows will interfere with each other, causing the filament bundle to shake greatly, affecting the production stability. Therefore, in the drafting and shaping device of the FDY production equipment, the hot roller a and the filament separator a are located in one insulation box, and the hot roller b and the filament separator b are located in another insulation box, which causes the filament bundle between the hot roller a and the hot roller b to shake. When exposed to the outside of the heat preservation box, the temperature of the filament bundle will escape, the molecular chain part of the fiber will be in a frozen state, and uneven stretching will occur during the stretching process, thus affecting the uniformity of the stretching; the present invention changes the layout of the stretching and shaping device in the FDY production equipment, making it possible for "the hot roller a and the hot roller b to rotate in the same direction", thereby making it possible for "the entire stretching and shaping device to be located in the same heat preservation box", so that the filament bundle is located in the heat preservation box during the entire stretching and shaping process, reducing heat loss, and thus facilitating the effective stretching and shaping of the filament bundle;
[0022] (3) In the stretching and shaping device in the FDY production equipment, the lengths of the filaments at different positions from the hot roller a to the hot roller b are different (the larger the angle of the filaments from the hot roller a to the hot roller b, the longer the distance, and vice versa), resulting in uneven stretching and the risk of horizontal stripes in the subsequent dyeing process. In the stretching and shaping device of the present invention, "the upper surfaces of the hot roller a and the hot roller b are flush, the hot roller a is located on the left side of the hot roller b, and the two are arranged at a distance of 100-140 mm", the filaments at different positions are stretched in parallel between the hot roller a and the hot roller b, and the lengths of the filaments at different positions from the hot roller a to the hot roller b are the same, which can avoid uneven stretching and reduce the risk of horizontal stripes in the subsequent dyeing process. At the same time, the stretching distance of the filaments is short, which can improve the utilization rate of the hot roller a and the hot roller b, thereby facilitating the effective stretching and shaping of the filaments.
[0023] The present invention also provides a POY / FDY universal production equipment A2, which is different from the POY / FDY universal production equipment A1 only in that: the wire separation roller a is replaced by a hot roller c, and the central axis of the hot roller c is parallel to the front-to-back direction; the distance between the hot roller a and the hot roller c is 120-150 mm; the vertical planes where the rightmost sides of the hot roller a and the hot roller c are located are coplanar; the diameter of the hot roller c is 150-190 mm, and the length is 180-200 mm.
[0024] The present invention replaces the filament separation roller in the drawing and shaping device of the prior art with a hot roller C, which can shorten the residence time of the filament bundle on each hot roller when the same degree of crystallization is achieved. It is also beneficial to reduce the volume of the hot roller and make its arrangement more compact. The matching hot roller insulation box is also reduced accordingly to ensure the uniformity of the ambient temperature around the hot roller. The temperature distribution on the surface of the hot roller is more stable than that of the original process, which is beneficial to maintain consistent heating and drawing of the fiber.
[0025] The present invention also provides a method for producing POY yarn, using a POY / FDY universal production equipment A1 or A2 as described in any of the above items, and the specific process is: after the polyester melt is extruded through a spinning assembly, it is cooled by a cooling bellows to form a yarn bundle, and the yarn bundle passes through an oiling device, a pre-network device, a guide roller a, and a guide roller b in sequence, and is then wound by a winder to obtain POY yarn.
[0026] As the preferred technical solution:
[0027] The process parameters of the POY yarn production method as described above include: spinning assembly temperature 288-293°C, cooling bellows pressure 30-40Pa, pre-network pressure 0.5-0.7bar, guide roller a speed 2730-3350m / min, guide roller b speed 2740-3360m / min, and winding speed 2730-3350m / min.
[0028] A production method for POY yarn as described above, the specification of POY yarn is 100-300D / 36-576F, the linear density deviation rate is ±0.2%, the linear density CV%≤0.1%, the breaking strength is ≥2.32cN / dtex, the breaking strength CV%≤2.88%, the breaking elongation is 129.8±0.4%, the breaking elongation CV%≤2.89%, the yarn unevenness CV%≤1.28%, the yarn unevenness half suppression value ≤0.46%, the thermal stress CV%≤1.54%, and the oil content is 0.30-0.31wt%.
[0029] The present invention also provides a method for producing FDY yarn, using the POY / FDY universal production equipment A1 as described above, and the specific process is: after the polyester melt is extruded through a spinning assembly, it is cooled by a cooling bellows to form a tow, and the tow is successively passed through an oiling device, a pre-netting device, a drafting and shaping device, a godet a, a main netting device, and a godet b, and then wound by a winder to obtain FDY yarn;
[0030] The winding method of the tow on the drafting and setting device is as follows: the tow first contacts the right side of the hot roller a, and then is wound 3.5 times clockwise on the GR1 group until it contacts the upper side of the hot roller a, and then runs horizontally to the right until it contacts the upper side of the hot roller b, and then is wound 3.5 times clockwise on the GR2 group; when the tow is wound clockwise on the GR1 group, the right side of the hot roller a is taken as the starting position, and it returns to the starting position for the first time at the end of winding one circle, and returns to the starting position for the second time at the end of winding the second circle, and returns to the starting position for the second time at the end of winding the third circle. The filament bundle returns to the starting position for the third time, and the remaining 0.5 turns are an incomplete turn formed by the filament bundle continuing to be wound clockwise from the starting position to the upper side of the hot roller a; when the filament bundle is wound clockwise on the GR2 group, the upper side of the hot roller b is taken as the starting position, and it returns to the starting position for the first time when winding one turn is completed, and returns to the starting position for the second time when winding the second turn is completed, and returns to the starting position for the third time when winding the third turn is completed. The remaining 0.5 turns are the length of the filament bundle in contact with the hot roller b when it leaves the GR2 group;
[0031] During the stretching and shaping process, hot roller a is used for stretching and heating, and the filament bundle is wound around the GR1 group for multiple turns. The movement of macromolecules in the fiber is intensified, so that the fiber can be smoothly stretched. The stretching is mainly completed between the two hot rollers, hot roller a and hot roller b. Hot roller b is used for shaping and heating, and the filament bundle is wound around the GR2 group for multiple turns, so that the changes in the internal structure of the fiber during the stretching process can be stabilized, thereby improving the dimensional stability of the fiber.
[0032] As the preferred technical solution:
[0033] The process parameters of the FDY yarn production method as described above include: spinning assembly temperature 289-293°C, cooling bellows pressure 20-35Pa, pre-network pressure 0.2-0.25bar, hot roller a temperature 89-95°C, hot roller b temperature 140-148°C, hot roller a rotation speed 1460-2000m / min, hot roller b rotation speed 3600-4500m / min, guide roller a rotation speed 1460-2000m / min, main network pressure 3-4bar, guide roller b rotation speed 3600-4500m / min, winding speed 3600-4500m / min.
[0034] The production method of FDY yarn as described above, the single yarn linear density of FDY yarn is 0.57-1.39 dtex, the linear density deviation rate is ±0.2%, the linear density CV%≤0.54%, the breaking strength is ≥4.4 cN / dtex, the breaking strength CV%≤2.21%, the breaking elongation is 30.3±0.5%, the breaking elongation is ≤4.32%, the oil content is 1.01±0.01wt%, the network degree is 16-19 pieces / m, the boiling water shrinkage is 7.9±0.1%, and the boiling water shrinkage CV%≤3.2%.
[0035] It is difficult to produce FDY yarn with excellent performance and a single yarn density of less than 1.5 dtex in the existing technology for the following reasons:
[0036] ① In the production process of FDY yarn in the prior art, the tow is wound around the GR1 group for 6.5-7.5 turns, the diameter of the hot roller a is 220 mm, the length is 400 mm, the residence time of the tow on the hot roller a is 0.067-0.128 seconds, and the contact length is 225-259 cm; the hot roller a is a stretching hot roller, which is used to mechanically stretch the polymer chain and microcrystals to a certain extent. The increase in the orientation degree of the fiber during stretching is mainly caused by the further orderly arrangement of the amorphous region. By increasing the orientation degree and crystallinity, the strength of the fiber is improved;
[0037] The tow is wound around the GR2 group for 5.5-6.5 turns. The diameter of the hot roller b is 220 mm and the length is 350 mm. The residence time of the tow on the hot roller b is 0.025-0.037 seconds and the contact length is 190-225 cm. The hot roller b is a setting hot roller. During the heat setting process, the activity of the polymer chain is enhanced due to the increase in temperature, and the low-order molecular chain tends to crystallize. The temperature of the hot roller b is 140-150°C, which is suitable for the formation and growth of crystals. Therefore, the crystallinity of the fiber is further increased after heat setting. The large amount of internal stress generated by the fiber in the heat stretching stage is released in the heat setting stage, so that the molecular chain structure of the fiber remains stable.
[0038] In the above process, the residence time of the tow on the hot roller and the contact length between the tow and the hot roller are both relatively long, which is suitable for spinning FDY yarns with a relatively large single-filament linear density, that is, FDY yarns with a single-filament linear density of 1.5-5 dtex; when producing FDY yarns with a single-filament linear density of less than 1.5 dtex, the movement of the fiber molecular chains will be intensified, the cracks between the molecular chains will become larger, and the ester bonds in the supramolecular structure will be destroyed, thereby losing a certain degree of crystal orientation, resulting in changes in the physical properties of the fiber;
[0039] ② In the production process of FDY yarn in the prior art, hot roller a rotates counterclockwise and hot roller b rotates clockwise. The hot rollers will generate a certain amount of airflow during high-speed rotation. The two hot rollers form two airflows in different directions, which will interfere with each other, causing the yarn bundle to shake greatly and affecting the production stability. Therefore, a staggered arrangement is adopted when designing the position of the hot rollers; the stretching length of the yarn bundle from hot roller a to hot roller b is 130-150cm, and there is a stretching angle of about 45° (oblique stretching). When the speed of hot roller a is 1200-2000m / min and the speed of hot roller b is 3600-4500m / min, the speed difference between the two hot rollers is used to quickly extend the yarn, and the polymer chains and microcrystals inside the fiber are mechanically stretched. First, the macromolecular chains are straightened in the non-crystalline region, and then these macromolecular chains are subjected to the tensile force and arranged parallel to the axial direction of the fiber. The molecular chain tension produces an effective impedance in the axial direction of the fiber, so the fiber has a certain breaking strength and breaking elongation;
[0040] In the above process, the stretching length of the tow between the hot rollers is 130-150cm, which is suitable for spinning FDY yarns with a coarser single-filament linear density, that is, FDY yarns with a single-filament linear density of 1.5-5dtex; when producing FDY yarns with a single-filament linear density less than 1.5dtex, since the total denier of the tow and the single-filament denier are both small, compared with the coarse-denier fiber, the fine-denier fiber has a higher oriented microcrystalline structure. When stretched and deformed, the internal stress of the fine-denier fiber develops rapidly. If the stretching distance of the tow between the hot rollers reaches 130-150cm and there is a stretching angle of about 45°, on the one hand, the yarn will Large stress is generated, and some macromolecular chains are pulled out of the crystallization area. In some cases, the main chain of the macromolecular chain may even be broken, resulting in single filament breakage and affecting production stability. On the other hand, since fine denier fibers have a larger specific surface area, they heat or lose temperature faster, and the tow is stretched too long between the hot rollers, which will cause the tow to rise and fall rapidly repeatedly. Under the same stretching ratio, the fiber orientation and crystal structure between different spindles will be different. Therefore, the fiber elongation at break between different spindles fluctuates greatly, and the elongation at break CV% is about 5.43%.
[0041] ③ In the production process of FDY yarn in the prior art, after the yarn bundle is oiled by the oiling device, the yarn bundle goes down the channel through the porcelain part to form an angle of about 140° and enters the hot roller a. The yarn bundle will be subjected to a large friction force, resulting in the FDY yarn with a single yarn density less than 1.5dtex easily causing single yarn breakage.
[0042] The present invention can produce FDY yarn with excellent performance and a single yarn density of less than 1.5 dtex, for the following reasons:
[0043] ① According to the calculation of fiber stretching mechanism, at the same spinning speed, when producing FDY yarn with a single yarn density of less than 1.5dtex, the contact length between the yarn bundle and the hot roller a and the hot roller b reaches 82-104cm, which can obtain a higher degree of orientation and crystallinity; this is because the fine denier fiber has a larger specific surface area, and the relative area in contact with the hot roller and the heat transfer rate inside the yarn bundle are significantly better than those of medium and coarse denier yarns, so the contact length between the yarn bundle and the hot roller can be shortened;
[0044] In the present invention, the diameter of the hot roller a and the hot roller b is 150-190 mm, and the length is 180-200 mm. According to the required contact length between the filament bundle and the hot roller, the residence time of the filament bundle on the hot roller a needs to be 0.024-0.052 seconds, and the residence time on the hot roller b needs to be 0.011-0.017 seconds. The filament bundle only needs to be wound around the GR1 group and the GR2 group for 3.5 turns to achieve the corresponding orientation degree and crystallinity.
[0045] Compared with the FDY production process of the prior art, the residence time of the filament bundle on the hot roller is shortened by 35%-45%, which reduces the activity of the fiber molecular chain and avoids the destruction of the crystal orientation degree, resulting in the loss of fiber elasticity. On the other hand, the contact length between the filament bundle and the hot roller is reduced, reducing the quality damage caused by wear.
[0046] ② In the present invention, the hot roller a and the hot roller b are arranged in parallel and both rotate clockwise, so as to avoid the interference of the opposite airflow generated by the hot rollers during the high-speed rotation, reduce the shaking amplitude of the tow, and improve the production stability. Since the arrangement and rotation modes of the hot rollers are changed, the silk path of the tow also needs to be improved; the present invention changes the existing method of stretching the tow from the hot roller a to the hot roller b at an angle of about 45° (oblique stretching), and changes it to stretching the tow from the hot roller a to the hot roller b in parallel, and the stretching distance is the shortest. The tow enters the hot roller b from the hot roller a in parallel and closely at an angle of 0, and there is no tension difference before and after, which reduces the stress generated by the tow from the hot roller a to the hot roller b, avoids the breakage of the silk strips, and improves the production stability;
[0047] The distance between the hot roller a and the hot roller b is set to 100-140mm. Compared with the prior art, the stretching distance of the tow between the hot rollers is shortened by 15-30%. On the one hand, the short stretching distance between the hot rollers can reduce the tension of the filaments during the stretching process as much as possible, solve the problem of rapid development of internal stress when the fine denier fiber is stretched and deformed, and make more macromolecules arranged parallel to the axial direction of the fiber; on the other hand, the short stretching distance between the hot rollers can reduce the influence of the external environment, and avoid repeated rapid temperature rise and fall processes, so that the elongation at break of the tow between different spindle positions fluctuates little, and the elongation at break CV% is about 4.08%;
[0048] ③ In the present invention, a pre-network device is installed in the middle position of the tunnel to replace the porcelain part, so as to achieve the effect of fixing the direction of the silk path and improve the bundling and oiling uniformity of the yarn bundle. The yarn bundle passes through the pre-network device through the tunnel and enters the drawing and shaping device at the shortest route of 0 angle, which avoids the yarn bundle from being subjected to large friction. FDY yarn with a single yarn density of less than 1.5dtex is not prone to single yarn breakage.
[0049] By comparing the prior art with the present invention, it can be seen that the FDY yarn of the present invention with a single yarn density of less than 1.5 dtex has better performance, which supports the above viewpoints, for example:
[0050] In the paper "Process Development of Polyester Fine Denier (138dtex / 144f) Fully Drawn Yarn", the breaking strength of FDY yarn with a specification of 138dtex / 144f is 4.04cN / dtex, and the breaking strength and breaking elongation indexes fluctuate greatly between different spindle positions, with the breaking strength CV% being 2.43% and the breaking elongation CV% being 5.43%;
[0051] In the present invention, the breaking strength of the FDY yarn with a specification of 138dtex / 144f is 4.4cN / dtex, and the breaking strength and breaking elongation indexes fluctuate little between different spindle positions, the breaking strength CV% is 2.21%, and the breaking elongation CV% is 4.08%.
[0052] The production method of FDY yarn as described above, the process parameters include: spinning assembly temperature 290-291°C, cooling bellows pressure 22-30Pa, pre-network pressure 0.25bar, hot roller a temperature 90-95°C, hot roller b temperature 143-148°C, hot roller a speed 1460-1680m / min, hot roller b speed 4300-4500m / min, godet a speed 1460-1680m / min, main network pressure 4bar, godet b speed 4200-4500m / min, winding speed 4200-4500m / min;
[0053] The single yarn linear density of FDY yarn is ≤1.25dtex, the linear density deviation rate is ±0.2%, the linear density CV%≤0.54%, the breaking strength is ≥4.4cN / dtex, the breaking strength CV%≤2.21%, the breaking elongation is 29.7±0.4%, the breaking elongation CV%≤4.32%, the oil content is 1.01±0.01wt%, the network density is 16-19 pieces / m, the boiling water shrinkage is 7.9±0.1%, and the boiling water shrinkage CV%≤3.2%.
[0054] The present invention also provides a method for producing FDY yarn, using the POY / FDY universal production equipment A2 as described above, and the specific process is: after the polyester melt is extruded through a spinning assembly, it is cooled by a cooling bellows to form a tow, and the tow passes through an oiling device, a pre-netting device, a drafting and shaping device, a godet a, a main netting device, and a godet b in sequence, and is then wound by a winder to obtain FDY yarn;
[0055] The winding method of the tow on the drafting and setting device is as follows: the tow first contacts the right side of the hot roller a, and then is wound 3.5 times clockwise on the GR1 group until it contacts the upper side of the hot roller a, and then runs horizontally to the right until it contacts the upper side of the hot roller b, and then is wound 3.5 times clockwise on the GR2 group; when the tow is wound clockwise on the GR1 group, the right side of the hot roller a is taken as the starting position, and it returns to the starting position for the first time at the end of winding one circle, and returns to the starting position for the second time at the end of winding the second circle, and returns to the starting position for the second time at the end of winding the third circle. The filament bundle returns to the starting position for the third time, and the remaining 0.5 turns are an incomplete turn formed by the filament bundle continuing to be wound clockwise from the starting position to the upper side of the hot roller a; when the filament bundle is wound clockwise on the GR2 group, the upper side of the hot roller b is taken as the starting position, and it returns to the starting position for the first time when winding one turn is completed, and returns to the starting position for the second time when winding the second turn is completed, and returns to the starting position for the third time when winding the third turn is completed. The remaining 0.5 turns are the length of the filament bundle in contact with the hot roller b when it leaves the GR2 group;
[0056] During the stretching and shaping process, hot rollers a and c are used for stretching and heating, and the movement of macromolecules in the fiber is intensified, so that the fiber can be stretched smoothly. The stretching is mainly completed between hot rollers a and b. Hot roller b is used for shaping and heating. The filament bundle is wound around the GR2 group for multiple turns, so that the changes in the internal structure of the fiber during the stretching process can be stabilized, thereby improving the dimensional stability of the fiber.
[0057] As the preferred technical solution:
[0058] The process parameters of the FDY yarn production method as described above include: spinning assembly temperature 288-293°C, cooling bellows pressure 33-40Pa, pre-network pressure 0.2-0.4bar, hot roller a temperature 89-95°C, hot roller b temperature 145-150°C, hot roller c temperature 89-95°C, hot roller a rotation speed 1200-1800m / min, hot roller b rotation speed 3600-4500m / min, hot roller c rotation speed 1200-1800m / min, guide roller a rotation speed 3600-4500m / min, main network pressure 3.5-4bar, guide roller b rotation speed 3600-4500m / min, winding speed 3600-4500m / min.
[0059] The production method of FDY yarn as described above, the single yarn linear density of FDY yarn is 1.52-4.64dtex, the linear density deviation rate is ±0.2%, the linear density CV%≤0.57%, the breaking strength is ≥4.48cN / dtex, the breaking strength CV%≤1.91%, the breaking elongation is 30.1±0.7%, the breaking elongation CV%≤4.9%, the oil content is 1±0.02wt%, the network degree is 14-15 pieces / m, the boiling water shrinkage is 7.4±0.2%, and the boiling water shrinkage CV%≤1.85%.
[0060] Beneficial effects:
[0061] (1) The present invention solves the problem that existing POY production equipment is difficult to produce FDY, realizes the alternating production of the two products, and better adapts to market changes.
[0062] (2) The present invention optimizes the structure and layout of the drafting and shaping device, reduces its size to fit the space of the POY equipment, and at the same time ensures the drafting and shaping effect of the filament bundle and the product quality by improving the specifications, arrangement and rotation mode of the hot roller and the wire separation roller.
[0063] (3) For the production of FDY yarn with a single yarn density of less than 1.5 dtex, the present invention reduces the excessive activity of the fiber molecular chain and reduces wear and quality damage by reasonably designing the contact length and residence time between the yarn bundle and the hot roller.
[0064] (4) The present invention adopts a method in which the hot rollers are arranged in parallel and rotate in the same direction, and the yarn paths are stretched in parallel, which reduces the shaking and stress of the yarn bundle, shortens the stretching distance, improves the production stability, and reduces the fluctuation of the fiber performance indicators between different spindle positions.
[0065] (5) The entire drawing and shaping device can be placed in an insulation box, which avoids the temperature loss of the yarn bundle and ensures the temperature stability during drawing and shaping. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 It is a schematic diagram of a POY production device in the prior art;
[0067] Figure 2 It is a schematic diagram of FDY production equipment in the prior art;
[0068] Figure 3 This is a schematic diagram of producing FDY yarn using the POY / FDY universal production equipment of Example A1 of the present invention;
[0069] Figure 4 This is a schematic diagram of producing FDY yarn using the POY / FDY universal production equipment of Example A2 of the present invention;
[0070] Figure 5This is a schematic diagram of producing POY yarn using the POY / FDY universal production equipment of Example A1 of the present invention;
[0071] Among them, 1-spinning assembly, 2-cooling bellows, 3-oiling device, 4-pre-network device, 5-heat roller a, 6-heat roller b, 7-filament separation roller a, 8-filament separation roller b, 9-wire guide roller a, 10-main network device, 11-wire guide roller b, 12-winding machine, 13-ceramic parts, 14-heat roller c. DETAILED DESCRIPTION
[0072] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0073] The following are the test methods for the relevant performance indicators in each embodiment:
[0074] Line density deviation rate, line density CV%: measured in accordance with GB / T 14343-2008 standard.
[0075] Breaking strength, breaking strength CV%, breaking elongation, breaking elongation CV%: measured in accordance with GB / T 14344-2008; when testing FDY yarn, the gauge length is 500mm, and the dynamic clamp speed is 500mm / min; when testing POY yarn, the gauge length is 250mm, and the dynamic clamp speed is 1000mm / min.
[0076] Strip unevenness CV%, strip unevenness half inhibition value: measured in accordance with GB / T 14346-2015 standard, with a sample speed of 200m / min and a test time of 2.5min.
[0077] Thermal stress CV%: measured in accordance with FZ / T 50051-2020 standard, the test speed is 100m / min, the draft ratio is 1.65, the test length is 100m, and the heating temperature is selected according to the product specifications.
[0078] Oil content: measured in accordance with GB / T 6504-2017 standard.
[0079] Network degree: measured in accordance with FZ / T 50001-2016 standard.
[0080] Boiling water shrinkage, boiling water shrinkage CV%: measured in accordance with GB / T 6505-2017.
[0081] In the following examples, the intrinsic viscosity of the polyester melt is 0.650±0.006 dl / g.
[0082] Example A1
[0083] A POY / FDY general production equipment, such as Figure 3 As shown, the POY production equipment includes a spinning assembly 1, a cooling air box 2, an oiling device 3, a pre-network device 4, a godet roller a 9, a godet roller b 11, a winder 12, a drafting and shaping device and a main network device 10;
[0084] The drafting and shaping device is located below the pre-network device 4 and at the upper left of the godet roller a 9;
[0085] The drafting and setting device consists of a heat box and a GR1 group and a GR2 group located in the heat box at the same time. The GR1 group consists of a heat roller a 5 and a wire separation roller a 7, and the GR2 group consists of a heat roller b 6 and a wire separation roller b 8.
[0086] The central axes of the heat roller a 5, the heat roller b 6, the wire separation roller a 7, and the wire separation roller b 8 are all parallel to the front-rear direction;
[0087] The upper surfaces of the hot roller a5 and the hot roller b6 are flush, the hot roller a5 is located on the left side of the hot roller b6, the two are arranged at a distance of 100-140 mm, the wire separation roller a7 is located below the hot roller a5 and the two are arranged at a distance, and the wire separation roller b8 is located below the hot roller b6 and the two are arranged at a distance;
[0088] The rightmost vertical plane of the hot roller a 5 passes through the fiber outlet of the pre-network device 4;
[0089] Both the hot roller a 5 and the hot roller b 6 rotate clockwise;
[0090] The diameter of the hot roller a5 and the hot roller b6 is 150-190 mm, and the length is 180-200 mm; the diameter of the wire separation roller a7 and the wire separation roller b8 is 75-95 mm, and the length is 180-200 mm;
[0091] The main networker 10 is located between the godet roller a 9 and the godet roller b 11.
[0092] Example A2
[0093] A POY / FDY universal production equipment is basically the same as that of embodiment A1, except that: Figure 4As shown, the filament separation roller a is replaced by the hot roller c 14, and the central axis of the hot roller c 14 is parallel to the front-to-back direction; the spacing between the hot roller a 5 and the hot roller c 14 is 120-150mm; the vertical planes where the hot roller a 5 and the rightmost side of the hot roller c 14 are located are coplanar; the diameter of the hot roller c 14 is 150-190mm, and the length is 180-200mm.
[0094] Example B1
[0095] A method for producing POY yarn, using the POY / FDY general production equipment of Example A1, such as Figure 5 As shown, the specific process is as follows: the polyester melt is extruded through the spinning assembly 1, and then cooled by the cooling bellows 2 to form a tow, and the tow passes through the oiling device 3, the pre-network device 4, the godet roller a 9, the godet roller b 11 in sequence, and then is wound by the winder 12 to obtain the POY yarn;
[0096] The relevant process parameters are: spinning assembly temperature 288°C, cooling bellows air pressure 30Pa, pre-network pressure 0.7bar, godet roller a speed 3350m / min, godet roller b speed 3360m / min, winding speed 3350m / min.
[0097] The final specification of the POY yarn is 100D / 36F, the linear density deviation rate is 0.2%, the linear density CV% is 0.1%, the breaking strength is 2.49cN / dtex, the breaking strength CV% is 2.05%, the breaking elongation is 129.4%, the breaking elongation CV% is 1.99%, the yarn unevenness CV% is 1.23%, the yarn unevenness half-suppression value is 0.34%, the thermal stress CV% is 1.37%, and the oil content is 0.30wt%.
[0098] Example B2
[0099] A method for producing POY yarns, using the POY / FDY universal production equipment of Example A2, wherein the specific process is as follows: a polyester melt is extruded through a spinning assembly, and then cooled by a cooling bellows to form a tow, and the tow is successively passed through an oiling device, a pre-netting device, a godet a, and a godet b, and then wound by a winder to obtain POY yarns;
[0100] The relevant process parameters are: spinning assembly temperature 293°C, cooling bellows air pressure 40Pa, pre-network pressure 0.5bar, godet roller a speed 2730m / min, godet roller b speed 2740m / min, winding speed 2730m / min.
[0101] The final specification of the POY yarn is 300D / 576F, the linear density deviation rate is -0.2%, the linear density CV% is 0.06%, the breaking strength is 2.32cN / dtex, the breaking strength CV% is 2.88%, the breaking elongation is 130.2%, the breaking elongation CV% is 2.89%, the yarn unevenness CV% is 1.28%, the yarn unevenness half-suppression value is 0.46%, the thermal stress CV% is 1.54%, and the oil content is 0.31wt%.
[0102] Example C1
[0103] A method for producing FDY yarn, using the POY / FDY general production equipment of Example A1, such as Figure 3 As shown, the specific process is: the polyester melt is extruded through the spinning assembly, and then cooled by the cooling bellows to form a tow, and the tow passes through the oiling device, the pre-netting device, the drafting and shaping device, the godet roller a, the main netting device, the godet roller b in sequence, and then is wound by the winder to obtain the FDY yarn;
[0104] Among them, the relevant dimensional parameters of the POY / FDY general production equipment are: the distance between the hot roller a and the hot roller b is 100mm; the diameter of the hot roller a is 150mm, and the length is 180mm; the diameter of the hot roller b is 150mm, and the length is 180mm; the diameter of the wire separation roller a is 75mm, and the length is 180mm; the diameter of the wire separation roller b is 75mm, and the length is 180mm;
[0105] The winding method of the tow on the drafting and setting device is as follows: the tow first contacts the right side of the hot roller a, is wound 3.5 turns clockwise on the GR1 group to the upper side of the hot roller a, then runs horizontally to the right to the upper side of the hot roller b, and then is wound 3.5 turns clockwise on the GR2 group;
[0106] The relevant process parameters are: spinning component temperature 293°C, cooling bellows pressure 20Pa, pre-network pressure 0.2bar, hot roller a temperature 89°C, hot roller b temperature 140°C, hot roller a speed 2000m / min, hot roller b speed 3600m / min, guide roller a speed 2000m / min, main network pressure 3bar, guide roller b speed 3600m / min, winding speed 3600m / min.
[0107] The final FDY yarn consists of 144 single yarns, with a linear density of 0.57 dtex, a linear density deviation rate of -0.1%, a linear density CV% of 0.54%, a breaking strength of 4.42 cN / dtex, a breaking strength CV% of 1.5%, an elongation at break of 30.8%, an elongation at break CV% of 4.12%, an oil content of 1.02 wt%, a network density of 17 pieces / m, a boiling water shrinkage of 7.9%, and a boiling water shrinkage CV% of 2.41%.
[0108] Example C2
[0109] A method for producing FDY yarn, using the POY / FDY general production equipment of Example A1, such as Figure 3 As shown, the specific process is: the polyester melt is extruded through the spinning assembly, and then cooled by the cooling bellows to form a tow, and the tow passes through the oiling device, the pre-netting device, the drafting and shaping device, the godet roller a, the main netting device, the godet roller b in sequence, and then is wound by the winder to obtain the FDY yarn;
[0110] Among them, the relevant dimensional parameters of the POY / FDY general production equipment are: the distance between the hot roller a and the hot roller b is 120mm; the diameter of the hot roller a is 170mm, and the length is 180mm; the diameter of the hot roller b is 170mm, and the length is 180mm; the diameter of the wire separation roller a is 85mm, and the length is 180mm; the diameter of the wire separation roller b is 85mm, and the length is 180mm;
[0111] The winding method of the tow on the drafting and setting device is as follows: the tow first contacts the right side of the hot roller a, is wound 3.5 turns clockwise on the GR1 group to the upper side of the hot roller a, then runs horizontally to the right to the upper side of the hot roller b, and then is wound 3.5 turns clockwise on the GR2 group;
[0112] The relevant process parameters are: spinning component temperature 290℃, cooling bellows pressure 25Pa, pre-network pressure 0.25bar, hot roller a temperature 92℃, hot roller b temperature 146℃, hot roller a speed 1690m / min, hot roller b speed 4300m / min, guide roller a speed 1690m / min, main network pressure 4bar, guide roller b speed 4300m / min, winding speed 4300m / min.
[0113] The final FDY yarn consists of 36 single yarns, with a linear density of 1.39 dtex, a linear density deviation of -0.2%, a linear density CV% of 0.46%, a breaking strength of 4.46 cN / dtex, a breaking strength CV% of 1.8%, an elongation at break of 29.9%, an elongation at break CV% of 4.18%, an oil content of 1.02 wt%, a network density of 17 pieces / m, a boiling water shrinkage of 8%, and a boiling water shrinkage CV% of 2.2%.
[0114] Example C3
[0115] A method for producing FDY yarn, using the POY / FDY general production equipment of Example A1, such as Figure 3As shown, the specific process is: the polyester melt is extruded through the spinning assembly, and then cooled by the cooling bellows to form a tow, and the tow passes through the oiling device, the pre-netting device, the drafting and shaping device, the godet roller a, the main netting device, the godet roller b in sequence, and then is wound by the winder to obtain the FDY yarn;
[0116] Among them, the relevant dimensional parameters of the POY / FDY general production equipment are: the distance between the hot roller a and the hot roller b is 120mm; the diameter of the hot roller a is 180mm, and the length is 180mm; the diameter of the hot roller b is 180mm, and the length is 180mm; the diameter of the wire separation roller a is 90mm, and the length is 180mm; the diameter of the wire separation roller b is 90mm, and the length is 180mm;
[0117] The winding method of the tow on the drafting and setting device is as follows: the tow first contacts the right side of the hot roller a, is wound 3.5 turns clockwise on the GR1 group to the upper side of the hot roller a, then runs horizontally to the right to the upper side of the hot roller b, and then is wound 3.5 turns clockwise on the GR2 group;
[0118] The relevant process parameters are: spinning component temperature 289℃, cooling bellows pressure 35Pa, pre-network pressure 0.25bar, hot roller a temperature 95℃, hot roller b temperature 148℃, hot roller a speed 1460m / min, hot roller b speed 4500m / min, guide roller a speed 1460m / min, main network pressure 4bar, guide roller b speed 4500m / min, winding speed 4500m / min.
[0119] The final FDY yarn consists of 72 single yarns, with a linear density of 1.15 dtex, a linear density deviation of 0.1%, a linear density CV% of 0.45%, a breaking strength of 4.51 cN / dtex, a breaking strength CV% of 1.58%, an elongation at break of 30.1%, an elongation at break CV% of 4.32%, an oil content of 1wt%, a network density of 16 pieces / m, a boiling water shrinkage of 7.8%, and a boiling water shrinkage CV% of 3.2%.
[0120] Example C4
[0121] A method for producing FDY yarn, using the POY / FDY general production equipment of Example A1, such as Figure 3 As shown, the specific process is: the polyester melt is extruded through the spinning assembly, and then cooled by the cooling bellows to form a tow, and the tow passes through the oiling device, the pre-netting device, the drafting and shaping device, the godet roller a, the main netting device, the godet roller b in sequence, and then is wound by the winder to obtain the FDY yarn;
[0122] Among them, the relevant size parameters of POY / FDY general production equipment are: the distance between hot roller a and hot roller b is 140mm; the diameter of hot roller a is 190mm, and the length is 200mm; the diameter of hot roller b is 190mm, and the length is 200mm; the diameter of wire separation roller a is 95mm, and the length is 200mm; the diameter of wire separation roller b is 95mm, and the length is 200mm;
[0123] The winding method of the tow on the drafting and setting device is as follows: the tow first contacts the right side of the hot roller a, is wound 3.5 turns clockwise on the GR1 group to the upper side of the hot roller a, then runs horizontally to the right to the upper side of the hot roller b, and then is wound 3.5 turns clockwise on the GR2 group;
[0124] The relevant process parameters are: spinning component temperature 291°C, cooling bellows pressure 22Pa, pre-network pressure 0.2bar, hot roller a temperature 90°C, hot roller b temperature 143°C, hot roller a speed 2000m / min, hot roller b speed 4200m / min, guide roller a speed 2000m / min, main network pressure 3bar, guide roller b speed 4200m / min, winding speed 4200m / min.
[0125] The final FDY yarn consists of 144 single yarns, with a linear density of 0.96 dtex, a linear density deviation of 0.2%, a linear density CV% of 0.33%, a breaking strength of 4.4 cN / dtex, a breaking strength CV% of 2.21%, an elongation at break of 29.8%, an elongation at break CV% of 4.08%, an oil content of 1.01 wt%, a network density of 19 pieces / m, a boiling water shrinkage of 7.8%, and a boiling water shrinkage CV% of 2.28%.
[0126] Example D1
[0127] A method for producing FDY yarn, using the POY / FDY general production equipment of Example A2, such as Figure 4 As shown, the specific process is: the polyester melt is extruded through the spinning assembly, and then cooled by the cooling bellows to form a tow, and the tow passes through the oiling device, the pre-netting device, the drafting and shaping device, the godet roller a, the main netting device, the godet roller b in sequence, and then is wound by the winder to obtain the FDY yarn;
[0128] Among them, the relevant dimensional parameters of the POY / FDY general production equipment are: the distance between hot roller a and hot roller b is 100mm, the distance between hot roller a and hot roller c is 120mm; the diameter of hot roller a is 150mm, and the length is 180mm; the diameter of hot roller b is 150mm, and the length is 180mm; the diameter of hot roller c is 150mm, and the length is 180mm; the diameter of wire separation roller b is 75mm, and the length is 180mm;
[0129] The winding method of the tow on the drafting and setting device is as follows: the tow first contacts the right side of the hot roller a, is wound 3.5 turns clockwise on the GR1 group to the upper side of the hot roller a, then runs horizontally to the right to the upper side of the hot roller b, and then is wound 3.5 turns clockwise on the GR2 group;
[0130] The relevant process parameters are: spinning component temperature 288℃, cooling bellows pressure 40Pa, pre-network pressure 0.4bar, hot roller a temperature 95℃, hot roller b temperature 150℃, hot roller c temperature 95℃, hot roller a speed 1200m / min, hot roller b speed 4500m / min, hot roller c speed 1200m / min, guide roller a speed 4500m / min, main network pressure 4bar, guide roller b speed 4500m / min, winding speed 4500m / min.
[0131] The final FDY yarn consists of 36 single yarns, with a linear density of 4.64 dtex, a linear density deviation of 0.2%, a linear density CV% of 0.24%, a breaking strength of 4.54 cN / dtex, a breaking strength CV% of 1.91%, an elongation at break of 29.6%, an elongation at break CV% of 4.78%, an oil content of 1.02wt%, a network density of 15 pieces / m, a boiling water shrinkage of 7.6%, and a boiling water shrinkage CV% of 1.85%.
[0132] Example D2
[0133] A method for producing FDY yarn, using the POY / FDY general production equipment of Example A2, such as Figure 4 As shown, the specific process is: the polyester melt is extruded through the spinning assembly, and then cooled by the cooling bellows to form a tow, and the tow passes through the oiling device, the pre-netting device, the drafting and shaping device, the godet roller a, the main netting device, the godet roller b in sequence, and then is wound by the winder to obtain the FDY yarn;
[0134] Among them, the relevant dimensional parameters of the POY / FDY general production equipment are: the distance between hot roller a and hot roller b is 120mm, the distance between hot roller a and hot roller c is 140mm; the diameter of hot roller a is 180mm, the length is 180mm; the diameter of hot roller b is 180mm, the length is 180mm; the diameter of hot roller c is 180mm, the length is 180mm; the diameter of wire separation roller b is 90mm, the length is 180mm;
[0135] The winding method of the tow on the drafting and setting device is as follows: the tow first contacts the right side of the hot roller a, is wound 3.5 turns clockwise on the GR1 group to the upper side of the hot roller a, then runs horizontally to the right to the upper side of the hot roller b, and then is wound 3.5 turns clockwise on the GR2 group;
[0136] The relevant process parameters are: spinning component temperature 289°C, cooling bellows air pressure 38Pa, pre-network pressure 0.3bar, hot roller a temperature 92°C, hot roller b temperature 148°C, hot roller c temperature 92°C, hot roller a speed 1290m / min, hot roller b speed 4200m / min, hot roller c speed 1290m / min, guide roller a speed 4200m / min, main network pressure 4bar, guide roller b speed 4200m / min, winding speed 4200m / min.
[0137] The final FDY yarn consists of 48 single yarns, with a linear density of 3.48 dtex, a linear density deviation rate of -0.2%, a linear density CV% of 0.57%, a breaking strength of 4.61 cN / dtex, a breaking strength CV% of 1.86%, an elongation at break of 29.4%, an elongation at break CV% of 4.9%, an oil content of 0.99wt%, a network density of 14 / m, a boiling water shrinkage of 7.4%, and a boiling water shrinkage CV% of 0.98%.
[0138] Example D3
[0139] A method for producing FDY yarn, using the POY / FDY general production equipment of Example A2, such as Figure 4 As shown, the specific process is: the polyester melt is extruded through the spinning assembly, and then cooled by the cooling bellows to form a tow, and the tow passes through the oiling device, the pre-netting device, the drafting and shaping device, the godet roller a, the main netting device, the godet roller b in sequence, and then is wound by the winder to obtain the FDY yarn;
[0140] Among them, the relevant dimensional parameters of the POY / FDY general production equipment are: the distance between hot roller a and hot roller b is 140mm, the distance between hot roller a and hot roller c is 150mm; the diameter of hot roller a is 190mm, and the length is 200mm; the diameter of hot roller b is 190mm, and the length is 200mm; the diameter of hot roller c is 190mm, and the length is 200mm; the diameter of wire separation roller b is 95mm, and the length is 200mm;
[0141] The winding method of the tow on the drafting and setting device is as follows: the tow first contacts the right side of the hot roller a, is wound 3.5 turns clockwise on the GR1 group to the upper side of the hot roller a, then runs horizontally to the right to the upper side of the hot roller b, and then is wound 3.5 turns clockwise on the GR2 group;
[0142] The relevant process parameters are: spinning component temperature 293°C, cooling bellows air pressure 33Pa, pre-network pressure 0.2bar, hot roller a temperature 89°C, hot roller b temperature 145°C, hot roller c temperature 89°C, hot roller a speed 1800m / min, hot roller b speed 3600m / min, hot roller c speed 1800m / min, guide roller a speed 3600m / min, main network pressure 3.5bar, guide roller b speed 3600m / min, winding speed 3600m / min.
[0143] The final FDY yarn consists of 36 single yarns, with a linear density of 1.52 dtex, a linear density deviation of 0.1%, a linear density CV% of 0.07%, a breaking strength of 4.48 cN / dtex, a breaking strength CV% of 1.83%, an elongation at break of 30.8%, an elongation at break CV% of 3.98%, an oil content of 0.98wt%, a network density of 15 pieces / m, a boiling water shrinkage of 7.2%, and a boiling water shrinkage CV% of 0.51%.
Claims
1. A POY / FDY general production equipment, comprising a spinning assembly, a cooling bellows, an oiling device, a pre-netting device, a godet a, a godet b and a winder, which are all POY production equipment, characterized in that: It also includes a drafting and shaping device and a main networker; The drafting and shaping device is located below the pre-network device and at the upper left of the godet roller a; The drafting and setting device consists of a heat box and a GR1 group and a GR2 group located in the heat box at the same time. The GR1 group consists of a heat roller a and a wire separation roller a, and the GR2 group consists of a heat roller b and a wire separation roller b. The central axes of the heat roller a, heat roller b, wire separation roller a and wire separation roller b are parallel to the front-rear direction; The upper surfaces of the hot roller a and the hot roller b are flush, the hot roller a is located on the left side of the hot roller b, the two are arranged at a distance of 100-140 mm, the wire separation roller a is located below the hot roller a and the two are arranged at a distance, and the wire separation roller b is located below the hot roller b and the two are arranged at a distance; The rightmost vertical plane of the hot roller a passes through the fiber outlet of the pre-network device; Both hot roller a and hot roller b rotate clockwise; The diameter of the hot roller a and the hot roller b is 150-190 mm, and the length is 180-200 mm; the diameter of the wire separation roller a and the wire separation roller b is 75-95 mm, and the length is 180-200 mm; The main network device is located between the wire roller a and the wire roller b.
2. A POY / FDY universal production equipment according to claim 1, characterized in that: The wire separation roller a is replaced by the hot roller c, and the central axis of the hot roller c is parallel to the front-to-back direction; the distance between the hot roller a and the hot roller c is 120-150mm; the vertical planes where the rightmost sides of the hot roller a and the hot roller c are located are coplanar; the diameter of the hot roller c is 150-190mm, and the length is 180-200mm.
3. A method for producing POY yarn, characterized in that: A POY / FDY universal production equipment as described in claim 1 or 2 is used, and the specific process is: after the polyester melt is extruded through the spinning assembly, it is cooled by a cooling bellows to form a filament bundle, and the filament bundle passes through an oiling device, a pre-network device, a guide roller a, and a guide roller b in sequence, and is then wound by a winder to obtain POY yarn.
4. A method for producing POY yarn according to claim 3, characterized in that: The process parameters include: spinning assembly temperature 288-293°C, cooling air box pressure 30-40Pa, pre-network pressure 0.5-0.7bar, godet a speed 2730-3350m / min, godet b speed 2740-3360m / min, winding speed 2730-3350m / min; The specifications of POY yarn are 100-300D / 36-576F, the linear density deviation rate is ±0.2%, the linear density CV%≤0.1%, the breaking strength ≥2.32cN / dtex, the breaking strength CV%≤2.88%, the breaking elongation is 129.8±0.4%, the breaking elongation CV%≤2.89%, the yarn unevenness CV%≤1.28%, the yarn unevenness half suppression value ≤0.46%, the thermal stress CV%≤1.54%, and the oil content is 0.30-0.31wt%.
5. A method for producing FDY yarn, characterized in that: The POY / FDY universal production equipment as claimed in claim 1 is used, wherein the specific process is as follows: the polyester melt is extruded through a spinning assembly, and then cooled by a cooling bellows to form a tow, and the tow is successively passed through an oiling device, a pre-netting device, a drafting and shaping device, a godet a, a main netting device, and a godet b, and then wound by a winder to obtain FDY yarn; The winding method of the yarn bundle on the stretching and shaping device is as follows: the yarn bundle first contacts the right side of the hot roller a, is wound 3.5 times clockwise on the GR1 group until it contacts the upper side of the hot roller a, then runs horizontally to the right until it contacts the upper side of the hot roller b, and then is wound 3.5 times clockwise on the GR2 group.
6. The method for producing FDY yarn according to claim 5, characterized in that: The process parameters include: spinning assembly temperature 289-293°C, cooling bellows pressure 20-35Pa, pre-network pressure 0.2-0.25bar, hot roller a temperature 89-95°C, hot roller b temperature 140-148°C, hot roller a speed 1460-2000m / min, hot roller b speed 3600-4500m / min, guide roller a speed 1460-2000m / min, main network pressure 3-4bar, guide roller b speed 3600-4500m / min, winding speed 3600-4500m / min.
7. The method for producing FDY yarn according to claim 6, characterized in that: The single-filament linear density of FDY yarn is 0.57-1.39dtex, the linear density deviation rate is ±0.2%, the linear density CV%≤0.54%, the breaking strength ≥4.4cN / dtex, the breaking strength CV%≤2.21%, the breaking elongation is 30.3±0.5%, the breaking elongation is ≤4.32%, the oil content is 1.01±0.01wt%, the network degree is 16-19 pieces / m, the boiling water shrinkage is 7.9±0.1%, and the boiling water shrinkage CV%≤3.2%.
8. A method for producing FDY yarn, characterized in that: The POY / FDY universal production equipment as claimed in claim 2 is used, and the specific process is: the polyester melt is extruded through the spinning assembly, and then cooled by a cooling bellows to form a tow, and the tow is successively passed through an oiling device, a pre-netting device, a drafting and shaping device, a godet a, a main netting device, and a godet b, and then wound by a winder to obtain FDY yarn; The winding method of the yarn bundle on the stretching and shaping device is as follows: the yarn bundle first contacts the right side of the hot roller a, is wound 3.5 times clockwise on the GR1 group until it contacts the upper side of the hot roller a, then runs horizontally to the right until it contacts the upper side of the hot roller b, and then is wound 3.5 times clockwise on the GR2 group.
9. The method for producing FDY yarn according to claim 8, characterized in that: The process parameters include: spinning assembly temperature 288-293°C, cooling bellows pressure 33-40Pa, pre-network pressure 0.2-0.4bar, hot roller a temperature 89-95°C, hot roller b temperature 145-150°C, hot roller c temperature 89-95°C, hot roller a speed 1200-1800m / min, hot roller b speed 3600-4500m / min, hot roller c speed 1200-1800m / min, guide roller a speed 3600-4500m / min, main network pressure 3.5-4bar, guide roller b speed 3600-4500m / min, winding speed 3600-4500m / min.
10. The method for producing FDY yarn according to claim 9, characterized in that: The single yarn linear density of FDY yarn is 1.52-4.64dtex, the linear density deviation rate is ±0.2%, the linear density CV%≤0.57%, the breaking strength is ≥4.48cN / dtex, the breaking strength CV%≤1.91%, the breaking elongation is 30.1±0.7%, the breaking elongation CV%≤4.9%, the oil content is 1±0.02wt%, the network degree is 14-15 pieces / m, the boiling water shrinkage is 7.4±0.2%, and the boiling water shrinkage CV%≤1.85%.
Citation Information
Patent Citations
POY (polyester pre-oriented yarn) spinning method and device by using FDY (fully drawn yarn) spinning device
CN102660786A
A method for producing POY varieties using FDY equipment
CN112458580B
Spinning device for forming slub filament yarns in composite yarn process and method for making slub filament yarns with spinning device
CN105926101A
Production process of polyester FDY multi-roll oil-free full-draft fibers
CN107034533A
Fiber filament pulling device
CN107723816A