Lithium metal battery negative electrode and preparation method thereof and battery
By adopting a two-layer lithium-philic layer structure in a lithium metal battery, the potential difference is used to deposit lithium metal between the two layers, the dendrite growth and battery safety problems are solved, and the cycle stability and safety performance are improved.
Patent Information
- Application Number
- CN202411103535.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The growth of dendrite of metal lithium in lithium metal batteries leads to battery safety problems and degradation of cycling performance, which is difficult to effectively solve in the existing technology.
A two-layer lithium-philic layer structure is adopted, in which the metal elements of the first lithium-philic layer and the second lithium-philic layer have different standard electrode potentials. The lithium metal is deposited between the two layers through the potential difference, reducing the risk of dendrites' growth and short circuit.
It significantly improves the cycle stability and safety performance of lithium metal batteries, achieves more uniform lithium deposition, and extends the service life of the battery.
Smart Images

Figure CN118645585B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a lithium metal battery negative electrode and a preparation method thereof, and a battery. Background Art
[0002] In recent years, electrochemical energy storage devices represented by rechargeable batteries have attracted more and more attention due to their advantages such as high energy conversion efficiency, environmental friendliness and ease of use. Among them, lithium-ion batteries have been used in many fields due to their advantages such as high rate, long life and low cost. For example, they have been widely used in various electronic products, electric vehicles and power systems. However, with higher requirements for various technical indicators of batteries, the energy density of lithium-ion batteries with carbon-based materials as negative electrodes can only reach 250Wh·Kg -1 The current level of rechargeable batteries can no longer meet the needs of various fields for high energy density energy storage systems. Therefore, it is necessary to continue to develop a new generation of rechargeable batteries to meet and support the long-term development of related industries.
[0003] In recent years, lithium-sulfur and lithium-air battery systems have attracted great interest from researchers due to their high theoretical capacity density. Metallic lithium has been paid attention to as an important component. Therefore, metallic lithium anode is considered to be one of the important breakthroughs in the development of the next generation of high-energy-density secondary batteries. However, since the surface of metallic lithium is very active, a solid electrolyte interface (SEI) will inevitably form in the atmosphere and electrolyte, and dendrites are easily generated during the charge and discharge cycle. The continuous growth of dendrites can cause short circuits, which in turn leads to battery safety issues. Therefore, solving problems such as the growth of metallic lithium dendrites and improving its stability as anode are important issues in the current research of lithium metal battery systems. Summary of the invention
[0004] In view of this, the present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, the present invention provides a lithium metal battery negative electrode and a preparation method thereof and a battery, which can alleviate the problem of dendrite growth of metal lithium.
[0005] In order to solve the above technical problems, this application is implemented as follows:
[0006] According to one aspect of the present application, an embodiment of the present application provides a negative electrode for a lithium metal battery, the negative electrode for the lithium metal battery comprising:
[0007] substrate;
[0008] a first lithium-philic layer, disposed on at least one surface of the substrate along a thickness direction, wherein the first lithium-philic layer comprises a first lithium-philic material; and
[0009] A second lithium-philic layer is disposed on a surface of the first lithium-philic layer away from the substrate, wherein the second lithium-philic layer comprises a second lithium-philic material;
[0010] The first lithiophilic material contains a metal element, and the metal formed by the metal element and the metal included in the second lithiophilic material have different standard electrode potentials.
[0011] In addition, the lithium metal battery negative electrode according to the present application may also have the following additional technical features:
[0012] In some embodiments, the first lithiophilic material includes one or more of metal oxides, metal nitrides, or metal sulfides, and the second lithiophilic material includes a metal element capable of alloying with lithium.
[0013] In some embodiments, the standard electrode potential difference between the metal formed by the metal element in the first lithiophilic material and the metal included in the second lithiophilic material is in the range of 0.05V to 3.6V.
[0014] In some embodiments, the first lithiophilic material includes at least one of cobalt oxide, calcium oxide, copper oxide, zinc oxide, nickel oxide, magnesium oxide, copper sulfide, silver sulfide, nickel nitride or copper nitride.
[0015] In some embodiments, the second lithiophilic material includes at least one of indium, strontium, gold, silver, zinc, tin, magnesium, cobalt, molybdenum, aluminum, germanium, antimony, zirconium, cerium or yttrium, and the metal element in the second lithiophilic material is different from the metal element in the first lithiophilic material.
[0016] In some embodiments, the substrate includes at least one of carbon paper, carbon cloth, carbon fiber, carbon nanotube, graphene, copper foam, nickel foam or aluminum foam.
[0017] In some embodiments, the substrate has a thickness of 6 μm to 20 μm.
[0018] In some embodiments, the thickness of the first lithium-philic layer is 20 μm to 40 μm.
[0019] In some embodiments, the thickness of the second lithium-philic layer is 10 μm to 30 μm.
[0020] In some embodiments, the first lithiophilic layer further includes a binder and a conductive agent, and the mass ratio of the first lithiophilic material, the binder and the conductive agent is (7.5-8.5): (0.5-1): (0.5-2).
[0021] According to another aspect of the present application, an embodiment of the present application provides a method for preparing a negative electrode of a lithium metal battery as described above, the method comprising the following steps:
[0022] forming a first lithium-philic layer on a substrate;
[0023] The second lithium-philic layer is compounded with the substrate to which the first lithium-philic layer is attached to obtain the negative electrode of the lithium metal battery.
[0024] In some of the embodiments, the forming of the first lithium-philic layer on the substrate specifically includes: mixing a first lithium-philic material precursor, a binder and a conductive agent, and dispersing them in a solvent, mixing them evenly to obtain a slurry, coating the slurry on the substrate, and forming the first lithium-philic layer on the substrate after drying.
[0025] In some embodiments, the first lithium-philic material precursor includes at least one of cobalt oxide, calcium oxide, copper oxide, zinc oxide, nickel oxide, magnesium oxide, copper sulfide, silver sulfide, nickel nitride or copper nitride.
[0026] In some embodiments, the mass ratio of the first lithium-philic material precursor, the binder and the conductive agent is (7.5-8.5): (0.5-1): (0.5-2).
[0027] In some embodiments, the drying temperature is 80° C. to 100° C., and the drying time is 10 h to 24 h.
[0028] In some embodiments, the second lithium-philic layer is composited with the substrate to which the first lithium-philic layer is attached by a pair of rollers; the pressure of the pair of rollers is in the range of 0.1 MPa to 1 MPa.
[0029] According to another aspect of the present application, an embodiment of the present application provides a battery, which includes a positive electrode and a lithium metal battery negative electrode as described above or a lithium metal battery negative electrode prepared according to the above method.
[0030] Implementing the technical solution of the present invention has at least the following beneficial effects:
[0031] In the embodiment of the present application, the provided lithium metal battery negative electrode has a first lithium-philic layer disposed on the surface of the substrate, and a second lithium-philic layer disposed on the surface of the first lithium-philic layer, and the standard electrode potential of the metal formed by the metal element in the first lithium-philic material and the metal included in the second lithium-philic material are different, that is, two different lithium-philic layers are used for coordinated arrangement. Thus, by making the potential of the first lithium-philic layer and the second lithium-philic layer different, and utilizing the potential difference between the first lithium-philic layer and the second lithium-philic layer, during the charge and discharge process, lithium metal will be deposited between the first lithium-philic layer and the second lithium-philic layer, that is, lithium metal will utilize the potential difference between the two lithium-philic layers to penetrate into the middle, providing a spatial structure for the generation of dendrites, reducing the chance of battery short circuit caused by contact with the positive electrode, and thus facilitating the improvement of the battery cycle performance.
[0032] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Shown is a schematic structural diagram of a negative electrode of a lithium metal battery provided in some embodiments of the present invention.
[0034] Description of reference numerals:
[0035] 10-base;
[0036] 20-first lithium-philic layer;
[0037] 30-Second lithium-philic layer. DETAILED DESCRIPTION
[0038] The present application is further described below in conjunction with specific embodiments. It should be understood that these embodiments of the present application are only used to illustrate the present application and are not used to limit the scope of the present application.
[0039] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0040] Hereinafter, the embodiments of the lithium metal battery negative electrode, the method for preparing the lithium metal battery negative electrode, the battery, etc. of the present application are specifically disclosed with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0041] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0042] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0043] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0044] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0045] During the use of lithium metal batteries, the uneven deposition of lithium ions on the negative electrode of the lithium metal battery will cause the growth of lithium dendrites. Generally, a negative electrode-free battery refers to a battery "without negative electrode active material". By not using negative electrode active materials, the negative electrode-free battery can improve the energy density of the battery. The technical principle of a negative electrode-free battery is to deposit the lithium in the positive electrode on the negative electrode collector (negative electrode current collector of a negative electrode-free lithium metal battery) through formation charging or during the first charging of the battery. However, the interaction between the negative electrode structure of the negative electrode-free lithium metal battery or the negative electrode current collector and lithium in the related art is weak, resulting in uneven lithium deposition, and uncontrollable lithium deposition will form dendrites, deteriorate performance, and cause safety hazards. That is, the existing negative electrode of lithium metal batteries, especially negative electrode-free lithium metal batteries, mainly has the problem of lithium dendrite growth, which causes safety hazards to the battery or affects the cycle life of the battery.
[0046] In view of this, the technical solution of the embodiment of the present application provides a lithium metal battery negative electrode, which can be used in a negative electrode-free lithium metal battery. The technical solution of the embodiment of the present application can alleviate the problem of lithium dendrite growth in the existing negative electrode-free lithium metal battery, improve its stability as a negative electrode, and thus achieve the purpose of improving the safety performance and cycle life of the battery. The description of the specific technical solution is as follows.
[0047] like Figure 1 As shown, in some embodiments, the present application provides a lithium metal battery negative electrode, the lithium metal battery negative electrode comprising:
[0048] Base 10;
[0049] A first lithium-philic layer 20 is disposed on at least one side of the substrate 10 along the thickness direction, and the first lithium-philic layer 20 includes a first lithium-philic material; and
[0050] A second lithium-philic layer 30 is disposed on a surface of the first lithium-philic layer 20 away from the substrate 10 , and the second lithium-philic layer 30 includes a second lithium-philic material;
[0051] The first lithiophilic material contains a metal element, and the standard electrode potential of the metal formed by the metal element is different from that of the metal included in the second lithiophilic material.
[0052] The above “the first lithium-philic layer 20 is disposed on at least one side surface of the substrate 10 along the thickness direction” means that the first lithium-philic layer 20 can be disposed on one surface of the substrate 10 along its own thickness direction, or on two surfaces of the substrate 10 along its own thickness direction. The “surface” here can be the entire area of the substrate 10, or a partial area of the substrate 10, and the present application has no particular limitation on this, as long as the purpose of the present application can be achieved.
[0053] As an example, the substrate 10 has two surfaces opposite to each other in the thickness direction thereof, and the first lithium-philic layer 20 is disposed on the two opposite surfaces of the substrate 10. Further, the second lithium-philic layer 30 is formed on the surfaces of the first lithium-philic layer 20 on both sides. For example, the substrate 10 has a first surface and a second surface in the thickness direction thereof, and the first lithium-philic layer 20 and the second lithium-philic layer 30 are sequentially disposed on the first surface, and the first lithium-philic layer 20 and the second lithium-philic layer 30 are sequentially disposed on the second surface.
[0054] It is understandable that, in other embodiments, the first lithium-philic layer 20 may also be stacked on any one of the two surfaces of the substrate 10 .
[0055] In the present application, the negative electrode of the lithium metal battery is provided with a first lithium-philic layer 20 on the surface of the substrate 10, and a second lithium-philic layer 30 is provided on the surface of the first lithium-philic layer 20, wherein the first lithium-philic layer 20 includes a first lithium-philic material, and the second lithium-philic layer 30 includes a second lithium-philic material, the first lithium-philic material includes a metal element, and the second lithium-philic material includes a metal, that is, the first lithium-philic material and the second lithium-philic material can be different, especially the metal elements in the first lithium-philic material and the second lithium-philic material are different, so that the standard electrode potential of the metal formed by the metal element in the first lithium-philic material and the metal included in the second lithium-philic material are different. In this way, by loading two layers of lithium-philic layers with lithium-philic metal elements with different standard electrode potentials on the substrate 10, lithium ion transmission can be stabilized, lithium dendrite growth can be suppressed, and uniform lithium deposition can be achieved. It is used as the negative electrode of a negative electrode-free lithium metal battery, which can significantly improve the cycle stability and safety performance of the negative electrode-free lithium metal battery. In detail:
[0056] The present invention selects at least two metal elements with lithium affinity, and preferably, at least one of the lithium affinity materials, such as the second lithium affinity material, is a lithium affinity material that can alloy with lithium to form a lithium alloy. By loading two lithium affinity layers containing lithium affinity metal elements with different potentials on the substrate 10, the two different lithium affinity layers are used for coordination, that is, by making the potentials of the first lithium affinity layer 20 and the second lithium affinity layer 30 different, the potential difference between the first lithium affinity layer 20 and the second lithium affinity layer 30 is used. During the charge and discharge process, lithium metal will be deposited between the first lithium affinity layer 20 and the second lithium affinity layer 30, that is, lithium metal will use the potential difference between the two lithium affinity layers to penetrate into the middle, providing a spatial structure for the generation of dendrites, reducing the chance of contacting the positive electrode to cause a short circuit in the battery, and thus helping to improve the cycle performance of the battery.
[0057] In addition, the second lithium-philic material of the present invention is preferably a lithium-philic material that can alloy with lithium to form a lithium alloy. The second lithium-philic material is used to contact lithium to form a lithium alloy. The presence of the second lithium-philic material can slow down the diffusion of lithium. Under a smaller stripping current, the lithium alloy in the second lithium-philic layer 30 can extract more lithium, which indicates that the alloy can maintain a more stable diffusion path, thereby improving the effective lithium diffusion rate.
[0058] Therefore, based on the above configuration, the coordinated configuration of the first lithium-philic layer 20 and the second lithium-philic layer 30 with different potentials can effectively inhibit the growth of lithium dendrites, facilitate uniform lithium deposition, reduce the safety hazards caused by the presence of lithium dendrites, and help improve the cycle stability of the battery, which is suitable for lithium metal battery applications.
[0059] The inventors have found through in-depth research that when the negative electrode of the lithium metal battery of the present application satisfies the above-mentioned design conditions and optionally satisfies one or more of the following conditions, the performance of the negative electrode of the lithium metal battery can be further improved.
[0060] In some embodiments, the first lithiophilic material includes one or more of a metal oxide, a metal nitride, or a metal sulfide, and the second lithiophilic material includes a metal element capable of alloying with lithium.
[0061] In the present application, the first lithiophilic material may be a lithium-insertable compound, such as a compound containing a metal element such as a metal oxide, a metal nitride, or a metal sulfide, and the compound has a lithiophilic property. The second lithiophilic material may be a metal element, especially a lithiophilic material that can alloy with lithium to form a lithium alloy. Moreover, the metal element of the second lithiophilic material is different from the metal element in the first lithiophilic material, so that the standard electrode potential of the metal formed by the metal element in the first lithiophilic material and the metal in the second lithiophilic material are different.
[0062] In some embodiments, the standard electrode potential difference between the metal formed by the metal element in the first lithiophilic material and the metal included in the second lithiophilic material is in the range of 0.05 V to 3.6 V. As an example, the standard electrode potential difference between the two can be 0.05 V, 0.06 V, 0.08 V, 0.1 V, 02 V, 0.4 V, 0.5 V, 0.6 V, 0.8 V, 1 V, 1.2 V, 1.5 V, 2 V, 2.2 V, 2.5 V, 3 V, 3.5 V, 3.6 V or in the range of any two of the above values.
[0063] It should be pointed out that the standard electrode potential difference can be a value obtained by subtracting the standard electrode potential of the metal formed by the metal element in the first lithiophilic material from the standard electrode potential of the metal single substance of the second lithiophilic material, or it can be a value obtained by subtracting the standard electrode potential of the metal formed by the metal element in the first lithiophilic material from the standard electrode potential of the metal single substance of the second lithiophilic material.
[0064] It should be understood that when the material types of the first lithiophilic material and the second lithiophilic material are determined, the potential difference between the two is a constant value. As long as a potential difference is generated, lithium ions can be deposited using the potential difference. Therefore, the above-mentioned potential difference value range is a preferred range. The first lithiophilic material and the second lithiophilic material selectable within this preferred range are more practical and more conducive to obtaining a lithium metal battery negative electrode with excellent comprehensive performance, but it is not limited to this. For example, when the potential difference between the two is less than 0.05V or greater than 3.6V, lithium ion deposition can also be achieved, and there is no special restriction on this.
[0065] In some embodiments, the first lithium-philic material includes, but is not limited to, any one or a combination of at least two of cobalt oxide (CoO), calcium oxide (CaO), copper oxide (CuO), zinc oxide (ZnO), nickel oxide (NiO), magnesium oxide (MgO), copper sulfide (CuS), silver sulfide (Ag2S), nickel nitride (Ni3N2) or copper nitride (Cu(N3)2), and the combinations can be arbitrarily matched, and the combinations within the above range are no longer listed one by one.
[0066] Using the above-mentioned lithiophilic metal oxide, metal sulfide or metal nitride as the first lithiophilic material is beneficial to making the lithium deposited on the negative electrode of the lithium metal battery more uniform, has a good effect in inhibiting lithium dendrites, helps to inhibit the formation of lithium dendrites, and improves the safety performance and cycle life of the battery.
[0067] Among them, preferably, the first lithium-philic material is preferably cobalt oxide (CoO). The standard electrode potential of the +2-valent Co is -0.277V, which is a good lithium-philic material and can form a certain potential difference with the metal element of the second lithium-philic material, which is beneficial to the deposition of lithium ions and alleviates the growth problem of lithium dendrites.
[0068] In addition, in other embodiments, the first lithiophilic material is not limited to the types listed above. The first lithiophilic material can also be of other types as long as it can be used as a good lithiophilic material and is conducive to inducing uniform deposition of lithium. These types will not be described in detail one by one here.
[0069] In some embodiments, the second lithiophilic material includes, but is not limited to, any one or a combination of at least two of indium (In), strontium (Sr), gold (Au), silver (Ag), zinc (Zn), tin (Sn), magnesium (Mg), cobalt (Co), molybdenum (Mo), aluminum (Al), germanium (Ge), antimony (Sb), zirconium (Zr), cerium (Ce) or yttrium (Y), and the combination can be arbitrarily matched, and the combinations within the above range are no longer listed one by one, and the metal element in the second lithiophilic material is different from the metal element in the first lithiophilic material. For example, when the first lithiophilic material is CoO, the second lithiophilic material does not include Co; or, when the first lithiophilic material is ZnO, the second lithiophilic material does not include Zn; similarly, as long as the metal element in the first lithiophilic material is different from the metal element in the second lithiophilic material.
[0070] The selected second lithium-philic materials can alloy with lithium metal to form lithium alloys, and can form a certain potential difference with the metal elements in the first lithium-philic material, which is beneficial to the deposition of lithium ions and alleviates the growth problem of lithium dendrites.
[0071] Preferably, the second lithiophilic material is selected from indium (In). By using In (the standard electrode potential of +3-valent In is -0.342V) as the second lithiophilic material, In can form a lithium-indium alloy when in contact with lithium. The presence of In can slow down the diffusion of lithium. Under a smaller stripping current, the lithium-indium electrode can extract more lithium, which indicates that the lithium-indium alloy can maintain a more stable diffusion path, thereby facilitating the improvement of the effective lithium diffusion rate.
[0072] In addition, an indium sheet is used as the second lithium-philic layer 30. The indium sheet is a common form of the indium element and has a relatively soft texture. It is easier to realize industrial production by using a double-roll method.
[0073] In addition, in other embodiments, the second lithiophilic material is not limited to the types listed above. Under the conditions of satisfying the requirements of having good lithiophilicity, being able to alloy with lithium, and being conducive to inducing uniform deposition of lithium, the second lithiophilic material may also adopt other types, which will not be described in detail one by one here.
[0074] Optionally, in the present application, the second lithium-philic layer 30 may be a film, sheet, foil, mesh, or other structure formed by the above-mentioned metal elements, such as indium, strontium, gold, silver, zinc, tin, magnesium, cobalt, molybdenum, aluminum, germanium, antimony, zirconium, cerium, yttrium, etc. For example, the second lithium-philic layer 30 may be a sheet of indium, strontium, or the like.
[0075] In some embodiments, the first lithium-philic layer 20 further includes a binder and a conductive agent, that is, the first lithium-philic layer 20 is mainly composed of a first lithium-philic material, a conductive agent and a binder, and the second lithium-philic layer 30 is mainly composed of a second lithium-philic material.
[0076] The mass ratio of the first lithiophilic material, the binder and the conductive agent is (7.5-8.5): (0.5-1): (0.5-2). As an example, the mass ratio of the first lithiophilic material, the binder and the conductive agent can be any one of 7.5:1:1.5, 7.5:0.5:2, 7.8:1:1.2, 8:1:1, 8:0.8:1.2, 8.5:1:0.5, 8.5:0.5:1, 8.5:0.6:0.9 or a range between any two of them.
[0077] By making the mass ratio of the first lithiophilic material, the binder and the conductive agent within the above-mentioned appropriate range, it is helpful to ensure the addition amount of the first lithiophilic material while meeting the conductivity and bonding requirements, which is beneficial to improving the cycle performance.
[0078] In some embodiments, the thickness of the first lithium-philic layer 20 is 20 μm to 40 μm. Preferably, the thickness of the first lithium-philic layer 20 is 25 μm to 35 μm. As an example, the thickness of the first lithium-philic layer 20 can be 20 μm, 21 μm, 22 μm, 24 μm, 25 μm, 26 μm, 28 μm, 30 μm, 32 μm, 35 μm, 40 μm, or a range consisting of any two of the above values.
[0079] In some embodiments, the second lithium-philic layer 30 has a thickness of 10 μm to 30 μm. Preferably, the second lithium-philic layer 30 has a thickness of 15 μm to 25 μm. As an example, the thickness of the second lithium-philic layer 30 can be 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, 22 μm, 25 μm, 28 μm, 30 μm, or a range consisting of any two of the above values.
[0080] If the thickness of the first lithium-philic layer 20 or the second lithium-philic layer 30 is too thin, the mechanical properties of the negative electrode of the lithium metal battery will be reduced, and its strength will be reduced; if the thickness of the first lithium-philic layer 20 or the second lithium-philic layer 30 is too thick, the transmission rate of lithium ions will be reduced. Therefore, by making the thickness of the first lithium-philic layer 20 and the second lithium-philic layer 30 within the above range, it can be more conducive to the transmission of lithium ions while ensuring its strength, and the electrochemical performance of the negative electrode of the lithium metal battery can be improved.
[0081] In some embodiments, the substrate 10 includes, but is not limited to, any one of carbon paper, carbon cloth, carbon fiber, carbon nanotubes, graphene, copper foam, nickel foam or aluminum foam, or a combination of at least two of them. The combination can be arbitrarily matched, and the combinations within the above range are no longer listed one by one.
[0082] In the present application, the substrate 10 may be a substrate material with a porous structure, such as a carbon-based material substrate 10, or a porous metal substrate. The carbon-based material substrate may be a substrate 10 made of materials such as carbon paper, carbon cloth, carbon fiber, carbon nanotubes, graphene, etc., or a substrate 10 made of porous metal materials such as foamed copper, foamed nickel or foamed aluminum.
[0083] Preferably, the substrate 10 is made of materials such as foam copper, foam nickel, carbon fiber, and carbon nanotubes.
[0084] The selected substrate 10 is a three-dimensional substrate with a porous structure, has a certain conductivity, and may have a three-dimensional microstructure, which is beneficial to improving the electrochemical performance of the negative electrode of the lithium metal battery.
[0085] In some embodiments, the thickness of the substrate 10 is 6 μm to 20 μm. As an example, the thickness of the substrate 10 may be 6 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, or a range consisting of any two of the above values.
[0086] By controlling the thickness of the substrate 10 within the above range, it is helpful to reduce the thickness as much as possible while meeting a certain mechanical strength, thereby reducing costs and improving the overall energy density of the battery.
[0087] Accordingly, in some embodiments, a method for preparing a negative electrode of a lithium metal battery is provided, the method comprising the following steps:
[0088] forming a first lithium-philic layer 20 on a substrate 10;
[0089] The second lithium-philic layer 30 is compounded with the substrate 10 to which the first lithium-philic layer 20 is attached to obtain a negative electrode for a lithium metal battery.
[0090] It should be understood that all the features and advantages described above for the “lithium metal battery negative electrode” are also applicable to the “method for preparing the lithium metal battery negative electrode” and will not be described one by one here.
[0091] In the present application, the second lithium-philic layer 30 can adopt a self-supporting structural form, such as a sheet-shaped, mesh-shaped or film-shaped metal material with lithium affinity. In the preparation process, the first lithium-philic layer 20 can be formed on the substrate 10 first, and then the second lithium-philic layer 30 can be directly compounded with the substrate 10 attached with the first lithium-philic layer 20. The preparation method of the negative electrode of the lithium metal battery is simple in process, easy to operate, and has strong feasibility. It is easy to implement in process, such as directly implementing it through existing negative electrode preparation process equipment, and the prepared lithium metal battery negative electrode has excellent performance and low cost, and is easy to realize industrial production.
[0092] In some specific embodiments, the method for preparing the negative electrode of a lithium metal battery comprises the following steps (a) and (b):
[0093] Step (a), preparing a first lithium-philic layer 20.
[0094] In step (a), a first lithium-philic layer 20 is formed on the substrate 10, specifically comprising: mixing a first lithium-philic material precursor, a binder and a conductive agent, and dispersing them in a solvent, mixing them evenly to obtain a slurry, coating the slurry on the substrate 10, and drying to form the first lithium-philic layer 20 on the substrate 10.
[0095] In the present application, a first lithium-philic material such as metal oxide, metal nitride or metal sulfide can be coated on a substrate 10 such as carbon cloth (or a porous material substrate such as foam copper, foam nickel, carbon fiber, carbon nanotube, etc.) by a doctor blade coating method to prepare a first lithium-philic layer 20. Alternatively, a conventional preparation method can be used to first prepare a first lithium-philic material precursor, and then mix the first lithium-philic material precursor, a binder and a conductive agent, and disperse them in a solvent for preparation.
[0096] Optionally, the preparation of the first lithium-philic material precursor may include: heating the lithium-philic raw material to a certain temperature and then keeping it warm for a period of time, cooling and grinding, and then obtaining the first lithium-philic material precursor. As an example, the lithium-philic raw material is heated to 500°C to 600°C (such as 500°C, 520°C, 550°C, 580°C, 600°C or any range between them) at a heating rate of 1 to 8°C / min (such as 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 8°C / min, or any range between them), keeping it warm for 2h to 5h (such as 2h, 3h, 4h, 5h, or any range between them), cooling to room temperature, and then grinding to obtain the first lithium-philic material precursor.
[0097] Among them, optionally, the lithium-philic raw materials can be cobalt-containing raw materials, calcium-containing raw materials, copper-containing raw materials, zinc-containing raw materials, nickel-containing raw materials, magnesium-containing raw materials, copper-containing raw materials, silver-containing raw materials, nickel-containing raw materials, copper-containing raw materials, etc.
[0098] In some embodiments, the first lithiophilic material precursor includes at least one of cobalt oxide, calcium oxide, copper oxide, zinc oxide, nickel oxide, magnesium oxide, copper sulfide, silver sulfide, nickel nitride, or copper nitride.
[0099] In some embodiments, the mass ratio of the first lithium-philic material precursor, the binder, and the conductive agent is (7.5-8.5): (0.5-1): (0.5-2).
[0100] It should be noted that the present application does not limit the specific types of the binder and the conductive agent in the first lithium-philic layer 20, and the conventional binder and conductive agent used in the battery in the art can be used. As an example, the conductive agent can be a conventional conductive agent known in the art, such as one or more selected from conductive carbon black (Super-P), conductive graphite, carbon nanotubes, graphene, conductive carbon fiber, etc., wherein the conductive carbon black includes Ketjen black, acetylene black, etc. The binder can be a conventional binder known in the art, such as polytetrafluoroethylene, polyvinylidene fluoride, polyacrylic acid ethylene-tetrafluoroethylene copolymer, carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, polyvinyl alcohol, etc.
[0101] It should be understood that the present application is not limited to these conductive agents and binders. The present application may also use other known materials that can be used as positive conductive agents and binders in battery electrodes. The combination can be arbitrarily matched and will not be listed here one by one.
[0102] In some embodiments, in step (a), the drying temperature is 80°C to 100°C, and the drying time is 10h to 24h. As an example, the drying temperature can be any one of 80°C, 85°C, 90°C, 95°C, 100°C, or a range between any two of them; the drying time can be any one of 10h, 12h, 15h, 20h, 24h, or a range between any two of them.
[0103] Exemplarily, in some specific embodiments, step (a) forms a first lithium-philic layer 20 on the substrate 10, specifically comprising: placing a lithium-philic raw material (such as CoC2O4 powder, etc.) into a high-temperature tube furnace, heating it to 500°C to 600°C at a heating rate of 1 to 8°C / min, keeping it warm for 2h to 5h, cooling it to room temperature with the furnace, and then grinding it, such as grinding the powder with an agate mortar for 40min, to obtain a first lithium-philic material precursor. The prepared first lithium-philic material precursor is then mixed with a binder and a conductive agent. The mass ratio of the first lithium-philic material precursor, the binder and the conductive agent is (7.5-8.5): (0.5-1): (0.5-2) to obtain a mixture. The mixture is dispersed in a solvent (such as N-methyl-2-pyrrolidone, NMP), mixed evenly, and ground for 30 minutes to form a slurry. The slurry is coated on a substrate 10, and dried in a drying oven at a drying temperature of 80°C to 100°C for 10h to 24h to form a first lithium-philic layer 20 on the substrate 10.
[0104] Step (b), compounding the second lithium-philic layer 30 with the first lithium-philic layer 20 .
[0105] In step (a), compounding the second lithium-philic layer 30 with the first lithium-philic layer 20 specifically includes: compounding the second lithium-philic layer 30 with the substrate 10 attached with the first lithium-philic layer 20 by means of a roller; the pressure of the roller is in the range of 0.1 MPa to 1 MPa. As an example, the pressure of the roller can be any one of 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa, 0.8 MPa, 1 MPa or any range between two of them.
[0106] In the present application, a metal sheet (such as an indium sheet, etc.) can be pasted on a release film, and then the metal indium sheet and the first lithium-philic layer 20 in the substrate 10 material attached with the first lithium-philic layer 20 are rolled together (wherein the indium sheet is a common form of the indium element and has a relatively soft texture, and the rolling method is most suitable for industrial production). After rolling, a double-layer composite metal substrate material is obtained, that is, a lithium metal battery negative electrode is obtained.
[0107] In some embodiments, a battery is provided, which includes a lithium metal battery negative electrode or a lithium metal battery negative electrode prepared according to the aforementioned method.
[0108] Preferably, the battery is a lithium metal battery. More preferably, the battery is a lithium metal solid-state battery.
[0109] Since the battery provided in the embodiment of the present invention adopts all the technical solutions of the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0110] In some embodiments, the battery further comprises a positive electrode, an electrolyte and a separator. The electrolyte can conduct ions between the positive electrode and the negative electrode of the lithium metal battery. The separator is arranged between the positive electrode and the negative electrode of the lithium metal battery, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0111] It should be pointed out that in the battery of this embodiment, there is no limitation on the specific materials and structures of the positive electrode, electrolyte and separator, and the positive electrode sheet, electrolyte, separator structure and components that are known in the art and can be used for batteries can be selected.
[0112] In the embodiments of the present application, the electrolyte may be an electrolyte or a solid electrolyte, preferably a solid electrolyte (for example, it may be one or more of a sulfide solid electrolyte, an oxide solid electrolyte, and a composite solid electrolyte, etc.); the present application has no particular limitation on the solid electrolyte, as long as the purpose of the present application can be achieved.
[0113] The present application has no particular limitation on the isolation membrane, as long as the purpose of the present application can be achieved.
[0114] In order to better understand the present invention, the specific implementation process of the present invention will be described in detail below in a specific implementation mode. The implementation methods described below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application. If no specific technology or conditions are specified in the implementation method, the technology or conditions described in the literature in the field or the product specification shall be followed.
[0115] Example 1
[0116] 1. Preparation of lithium metal battery negative electrode, including the following steps:
[0117] 3 g of CoC2O4 powder was placed in a high-temperature tube furnace, heated to 550°C at a heating rate of 5°C / min, kept warm for 3 hours, and then cooled to room temperature with the furnace. The powder was then ground with an agate mortar for 40 minutes to obtain the first lithium-philic material precursor.
[0118] The prepared first lithium-philic material precursor (cobalt oxide precursor) is then mixed with a binder (polyvinylidene fluoride PVDF) and a conductive agent (conductive carbon black) in a mass ratio of 7.5:1:1.5 to obtain a mixture, and the mixture is dispersed in a solvent N-methyl-2-pyrrolidone, mixed evenly, and ground for 30 minutes to make a slurry, which is coated on a base carbon cloth, and dried in a drying oven at a drying temperature of 80°C for 12 hours to form a first lithium-philic layer on the substrate, thereby obtaining a CoO composite substrate material.
[0119] The indium sheet is pasted on the release film, and the indium sheet and the CoO composite substrate material are rolled together with the pressure of the rollers being 0.2 MPa. After the rolling, a double-layer composite metal substrate material is obtained. After the release film is removed, the negative electrode of the lithium metal battery can be obtained.
[0120] Among them, the standard electrode potential of +2-valent Co is -0.277V; the standard electrode potential of +3-valent In is -0.342V.
[0121] 2. Preparation of batteries, including:
[0122] The negative electrode of the lithium metal battery was cut into a disc with a diameter of 12 mm as a working electrode;
[0123] A lithium sheet was used as the counter electrode;
[0124] The working electrode, counter electrode, ceramic diaphragm and lithium metal electrolyte (the electrolyte is prepared by dissolving 1 mol of LiTFSI in 1,3-dioxolane DOL+ethylene glycol dimethyl ether DME) are assembled into a 2025 button cell.
[0125] It should be pointed out that, for the convenience of testing, the embodiment of the present application uses lithium metal as the counter electrode and the negative electrode of the lithium metal battery as the working electrode for testing. In this way, without other auxiliary substances, the loss of active lithium and the lithium insertion of the double-layer lithium-philic layer can be more intuitively calculated during the charge and discharge test. In practical applications, the negative electrode of the lithium metal battery of the present application can be used in lithium metal solid-state batteries.
[0126] Example 2
[0127] The difference between Example 2 and Example 1 is that:
[0128] In the preparation of lithium metal battery negative electrode, CoC2O4 powder is replaced with CaC2O4 powder to obtain a calcium oxide precursor.
[0129] Among them, the standard electrode potential of +2-valent Ca is -2.866V; the standard electrode potential of +3-valent In is -0.342V.
[0130] The rest are the same as in Example 1.
[0131] Example 3
[0132] The difference between Example 3 and Example 1 is that:
[0133] In the preparation of the negative electrode of the lithium metal battery, the indium sheet is replaced by a strontium sheet, and the strontium sheet and the CoO composite substrate material are rolled together.
[0134] Among them, the standard electrode potential of +2-valent Co is -0.277V; the standard electrode potential of +2-valent strontium (Sr) is +0.892V.
[0135] The rest are the same as in Example 1.
[0136] Example 4
[0137] The difference between Example 4 and Example 1 is that:
[0138] In the preparation of the negative electrode of the lithium metal battery, the pressure of the roller was adjusted to 0.1 MPa.
[0139] The rest are the same as in Example 1.
[0140] Example 5
[0141] The difference between Example 5 and Example 1 is that:
[0142] In the preparation of the negative electrode of the lithium metal battery, the pressure of the roller was adjusted to 0.5 MPa.
[0143] The rest are the same as in Example 1.
[0144] Example 6
[0145] The difference between Example 6 and Example 1 is that:
[0146] In the preparation of the negative electrode of the lithium metal battery, the pressure of the roller was adjusted to 1 MPa.
[0147] The rest are the same as in Example 1.
[0148] Example 7
[0149] The difference between Example 7 and Example 1 is that:
[0150] In the preparation of the negative electrode of the lithium metal battery, 3g of ZnC2O4 powder was placed in a high-temperature tube furnace and heated to 600℃ at a heating rate of 5℃ / min. After keeping warm for 4h, it was cooled to room temperature with the furnace. The powder was then ground with an agate mortar for 40min to obtain the first lithium-philic material precursor.
[0151] The prepared first lithium-philic material precursor (zinc oxide precursor) is then mixed with a binder (PVDF) and a conductive agent (conductive carbon black) in a mass ratio of 7.5:1:1.5 to obtain a mixture, and the mixture is dispersed in a solvent N-methyl-2-pyrrolidone, mixed evenly, and ground for 30 minutes to form a slurry, which is coated on a base carbon cloth and dried in a drying oven at a drying temperature of 100°C for 10 hours to form a first lithium-philic layer on the base, thereby obtaining a ZnO composite base material.
[0152] The silver sheet is pasted on the release film, and the silver sheet and the ZnO composite base material are rolled together with the pressure of the rollers being 0.2 MPa. After the rolling, a double-layer composite metal base material is obtained. After the release film is removed, the negative electrode of the lithium metal battery can be obtained.
[0153] Among them, the standard electrode potential of +2-valent Zn is -0.762V; the standard electrode potential of +1-valent Ag is +0.799V.
[0154] The rest are the same as in Example 1.
[0155] Comparative Example 1
[0156] The difference between Comparative Example 1 and Example 1 is that:
[0157] Preparation of lithium metal battery negative electrode, including:
[0158] 3 g of CoC2O4 powder was placed in a high-temperature tube furnace, heated to 550°C at a heating rate of 5°C / min, kept warm for 3 hours, and then cooled to room temperature with the furnace. The powder was then ground with an agate mortar for 40 minutes to obtain the first lithium-philic material precursor.
[0159] The prepared first lithium-philic material precursor (cobalt oxide precursor) is then mixed with a binder (PVDF) and a conductive agent (conductive carbon black) in a mass ratio of 7.5:1:1.5 to obtain a mixture, and the mixture is dispersed in a solvent N-methyl-2-pyrrolidone, mixed evenly, and ground for 30 minutes to form a slurry, which is coated on a base carbon cloth, and dried in a drying oven at a drying temperature of 80°C for 12 hours to form a first lithium-philic layer on the base, thereby obtaining a CoO composite base material, and thus obtaining a lithium metal battery negative electrode.
[0160] The main difference between Comparative Example 1 and Example 1 is that the second lithium-philic layer is omitted in Comparative Example 1; the lithium metal battery negative electrode of Comparative Example 1 only includes a substrate and a first lithium-philic layer.
[0161] Comparative Example 2
[0162] The difference between Comparative Example 2 and Example 1 is that:
[0163] Preparation of lithium metal battery negative electrode, including:
[0164] The indium sheet is pasted on the release film, and the indium sheet and the base material (carbon cloth) are rolled together with the pressure of the rolling being 0.2Mpa. After the rolling, a composite metal base material is obtained, and after removing the release film, a negative electrode of a lithium metal battery can be obtained.
[0165] The main difference between Comparative Example 2 and Example 1 is that the first lithium-philic layer is omitted in Comparative Example 2; the lithium metal battery negative electrode of Comparative Example 1 only includes a substrate and a second lithium-philic layer.
[0166] Performance Testing
[0167] The batteries obtained from the above-mentioned embodiments and comparative examples were subjected to cycle performance tests.
[0168] Cycle capacity retention rate test method: Connect the batteries of the above embodiments and comparative examples to a charging cabinet, and at a test temperature of 25°C, first charge them to 4.4V with a 0.1C constant current, then charge them at a constant voltage until the current is less than 0.05C, let them stand for 5 minutes, then discharge them to 2.8V with a 0.1C constant current, and then let them stand for 5 minutes. Repeat this process for 2 weeks to complete the formation step; charge them to 4.4V with a 0.2C constant current, then charge them at a constant voltage until the current is less than 0.05C; let them stand for 5 minutes, then discharge them to 2.8V with 0.5C, record the discharge capacity at this time as the initial discharge capacity, let them stand for another 5 minutes, cycle this step until the battery capacity retention rate is 80% of the initial discharge capacity, and complete the battery cycle test.
[0169] The test results are shown in Table 1 below.
[0170] Table 1 Battery performance test results of various embodiments and comparative examples
[0171]
[0172] It can be seen from the data in Table 1 that, compared with Comparative Examples 1-2, the batteries using the lithium metal battery negative electrodes provided by Examples 1-7 of the present invention play a positive role in improving the cycle performance of the batteries.
[0173] In addition, it can be seen from the data in Table 1 that when the metal materials in the first lithium-philic material and the second lithium-philic material are selected from Co and In elements, the battery cycle performance is the best when the roller pressure is 0.2Mpa. When other metal elements with potential differences are used as double-layer metals, the battery cycle performance is not much different. When all metal elements can be used as load metal materials, their cycle performance is significantly better than other groups. In addition, when preparing the second lithium-philic layer, the pressure of the roller also affects the battery. Too little pressure cannot make the second lithium-philic layer, such as the indium sheet, contact well with the metal substrate of the first lithium-philic layer, affecting the lithium metal. When the charge and discharge test is carried out, the lithium metal cannot utilize the potential difference between the two lithium-philic layers to be deposited between the two lithium-philic layers. Similarly, when the roller pressure increases, it is easy to wrinkle the pole piece and the battery cannot be prepared. In addition, it is also easy to crush the metal particles, resulting in a decrease in battery performance.
[0174] Parts of the present invention that are not described in detail are well known to those skilled in the art.
[0175] The basic principle of the present invention is described above in conjunction with specific embodiments. However, it should be pointed out that the advantages, strengths, effects, etc. mentioned in the present invention are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. must be possessed by each embodiment of the present invention. In addition, the specific details disclosed above are only for the purpose of illustration and facilitation of understanding, rather than limitation, and the above details do not limit the present invention to being implemented by adopting the above specific details.
[0176] It should be noted that the term "and / or" or " / " used in this document is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The singular forms of "a", "the" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0177] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0178] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A lithium metal battery negative electrode, characterized in that: The lithium metal battery negative electrode comprises: substrate; a first lithium-philic layer, disposed on at least one side of the substrate along the thickness direction, wherein the first lithium-philic layer is mainly composed of a first lithium-philic material, a conductive agent and a binder; the first lithium-philic material includes one or more of metal oxides, metal nitrides or metal sulfides; and A second lithium-philic layer is disposed on a surface of the first lithium-philic layer away from the substrate, the second lithium-philic layer is mainly composed of a second lithium-philic material; the second lithium-philic material includes a metal element that can alloy with lithium; the second lithium-philic layer adopts a self-supporting structure; The standard electrode potential of the metal formed by the metal element in the first lithiophilic material and the metal included in the second lithiophilic material are different.
2. The lithium metal battery negative electrode according to claim 1, characterized in that The standard electrode potential difference between the metal formed by the metal element in the first lithiophilic material and the metal included in the second lithiophilic material is in the range of 0.05V to 3.6V.
3. The negative electrode of the lithium metal battery according to claim 1, characterized in that The first lithiophilic material comprises at least one of cobalt oxide, calcium oxide, copper oxide, zinc oxide, nickel oxide, magnesium oxide, copper sulfide, silver sulfide, nickel nitride or copper nitride; And / or, the second lithiophilic material includes at least one of indium, strontium, gold, silver, zinc, tin, magnesium, cobalt, molybdenum, aluminum, germanium, antimony, zirconium, cerium or yttrium, and the metal element in the second lithiophilic material is different from the metal element in the first lithiophilic material.
4. The lithium metal battery negative electrode according to claim 1, characterized in that The substrate comprises at least one of carbon paper, carbon cloth, carbon fiber, carbon nanotube, graphene, copper foam, nickel foam or aluminum foam; And / or, the thickness of the substrate is 6 μm to 20 μm.
5. The lithium metal battery negative electrode according to any one of claims 1 to 4, characterized in that: The thickness of the first lithium-philic layer is 20 μm to 40 μm; and / or, the thickness of the second lithium-philic layer is 10 μm to 30 μm; And / or, in the first lithium-philic layer, the mass ratio of the first lithium-philic material, the binder and the conductive agent is (7.5-8.5): (0.5-1): (0.5-2).
6. The method for preparing a negative electrode for a lithium metal battery according to any one of claims 1 to 5, characterized in that: The following steps are involved: forming a first lithium-philic layer on a substrate; The second lithium-philic layer is compounded with the substrate to which the first lithium-philic layer is attached to obtain the negative electrode of the lithium metal battery.
7. The method for preparing a negative electrode for a lithium metal battery according to claim 6, characterized in that: The step of forming a first lithium-philic layer on the substrate specifically comprises: A first lithium-philic material precursor, a binder and a conductive agent are mixed and dispersed in a solvent, and after being mixed evenly, a slurry is obtained. The slurry is coated on a substrate, and after drying, a first lithium-philic layer is formed on the substrate.
8. The method for preparing a negative electrode for a lithium metal battery according to claim 7, characterized in that: The first lithium-philic material precursor includes at least one of cobalt oxide, calcium oxide, copper oxide, zinc oxide, nickel oxide, magnesium oxide, copper sulfide, silver sulfide, nickel nitride or copper nitride; and / or, the mass ratio of the first lithium-philic material precursor, the binder and the conductive agent is (7.5-8.5): (0.5-1): (0.5-2); And / or, the drying temperature is 80° C. to 100° C., and the drying time is 10 h to 24 h.
9. The method for preparing a negative electrode for a lithium metal battery according to any one of claims 6 to 8, characterized in that: The second lithium-philic layer is composited with the substrate to which the first lithium-philic layer is attached by a double-roll method; The pressure range of the pair of rollers is 0.1 MPa to 1 MPa.
10. A battery, characterized in that: The battery comprises a positive electrode and a negative electrode of the lithium metal battery according to any one of claims 1 to 5 or a negative electrode of the lithium metal battery prepared by the method according to any one of claims 6 to 9.
Citation Information
Patent Citations
Lithium-free negative pole piece as well as preparation method and application thereof
CN116190559A
Composite current collector of negative-electrode-free sodium metal battery and preparation method of composite current collector
CN117317239A