A type of high voltage stable sodium oxide positive electrode material and preparation method thereof
By using the composite structure of O3 phase and surface rock-like salt phase and high-temperature calcining process in the positive electrode material of sodium ion battery, the problem of poor cycling stability of sodium ion battery under high voltage is solved, and the high voltage stability and long life of the material are achieved , suitable for commercial applications of sodium ion batteries.
Patent Information
- Application Number
- CN202411116585.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The poor cycling stability of sodium ion battery oxide materials at high voltages leads to unstable material structure and rapid decomposition of electrolytes, limiting the development of sodium ion batteries.
The composite sodium electrooxide positive electrode material of O3 phase structure and surface rock salt phase structure is adopted, and the composite structure of the surface rock salt phase and the internal O3 phase is formed by wet grinding, drying, primary calcining and secondary high-temperature calcining. , improve the interface stability of the material at high voltages.
It realizes the air stability, high specific capacity and long cycle life of the material at high voltage, reduces the preparation cost, and is suitable for large-scale sodium ion battery industrial application.
Smart Images

Figure CN118645609B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthesis of positive electrode materials for sodium ion batteries, and in particular relates to a class of high-voltage stable sodium oxide positive electrode materials and a preparation method thereof. Background Art
[0002] Since its commercialization, lithium-ion batteries have achieved great success in portable electronic devices, new energy vehicles and other fields. However, the reserves of lithium resources in the earth's crust account for only about 0.0017%, and the distribution is uneven, which makes it expensive and the cost of raw materials is high, which seriously limits its further application in the field of large-scale energy storage. Sodium resources are relatively abundant in the earth's crust, widely distributed, and have obvious cost advantages. Therefore, sodium-ion batteries have broad application prospects in low-speed two-wheeled vehicles, four-wheeled vehicles, and energy storage fields.
[0003] The positive electrode material is responsible for providing active sodium ions and high potential reaction pairs, and occupies the highest price proportion in sodium ion batteries. Among them, O3 type nickel-based transition metal oxide positive electrode materials are mainly Ni 2+ / Ni 4+ The two-electron reaction of Ni is used as the redox active center, which has a high specific capacity and energy density. At present, the operating voltage range of sodium ion batteries is 2.0-4.0 V, which leads to the 2+ / Ni 4+ The two-electron reaction cannot fully participate in charge compensation, and the specific capacity is difficult to exert. Further expanding the working voltage range can promote the reactivity of Ni, but it will face many difficulties. On the one hand, a series of phase changes occur in the bulk structure of the material, resulting in large stress changes, leading to structural instability; on the other hand, under high voltage, the positive electrode surface is more active, and more side reactions occur with the electrolyte, resulting in continuous decomposition of the electrolyte, which leads to rapid capacity decay of the material under high voltage. Therefore, the development of high-voltage cycle-stable sodium oxide positive electrode materials is of great significance to the development of sodium-ion batteries.
[0004] Chinese patent CN117855421A discloses a gradient-doped oxide positive electrode material for sodium-ion batteries. The patent prepares a hydroxide precursor based on coprecipitation, and prepares a positive electrode material with a gradient distribution of Ni from the bulk to the surface, without the presence of special surface structures. In addition, the preparation requires strict control of solution concentration and dripping speed, which greatly increases the preparation cost. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art, solve the problem of poor cycle stability of sodium ion battery oxide materials under high pressure, and provide a class of high-voltage stable sodium oxide positive electrode materials and preparation methods thereof. The class of high-voltage stable sodium oxide positive electrode materials provided by the present invention has the characteristics of good air stability, high specific capacity and long cycle life under high voltage, and can be applied to commercial sodium ion batteries.
[0006] Based on the above purpose, the technical solution of the present invention is as follows:
[0007] The first aspect of the present invention provides a type of high-voltage stable sodium oxide positive electrode material, wherein the bulk phase structure of the material is an O3 phase structure, the surface is a rock salt phase structure, and the thickness of the rock salt phase structure is 2-3 nm; the chemical formula is Na a Ni b Cu c Fe d Mn e Ti f O2, where 0.7≤a≤1, 0.2≤b≤0.45, 0≤c≤0.1, 0≤d≤0.2, 0.2≤e≤0.5, 0≤f≤0.3,b + c + d + e + f = 1.
[0008] The second aspect of the present invention provides a method for preparing a high voltage stable sodium oxide positive electrode material, comprising the following steps:
[0009] (1) Weighing and mixing the sodium source and each transition metal source in proportion, and grinding them by wet grinding to obtain a uniformly mixed precursor slurry;
[0010] (2) placing the precursor slurry obtained in step (1) into a forced air drying oven for drying to obtain a precursor powder;
[0011] (3) calcining the precursor powder obtained in step (2) for the first time, and slowly cooling it to obtain an initial material powder;
[0012] (4) The initial material powder obtained in step (3) is subjected to a second calcination and quenching to obtain a high-voltage stable sodium oxide positive electrode material.
[0013] Preferably, the sodium source in step (1) is one of sodium carbonate, sodium bicarbonate or sodium acetate.
[0014] Preferably, the transition metal source in step (1) is a nickel source, a copper source, an iron source, a manganese source, or a titanium source, and is one of oxides, carbonates, or acetates.
[0015] Preferably, in step (1), the wet grinding method uses anhydrous ethanol as the solvent and the grinding is performed for 4-6 hours.
[0016] Preferably, in step (3), the first calcination temperature is 800-1000° C. and the calcination time is 10-15 hours.
[0017] Preferably, in step (4), the second calcination temperature is 900-1200° C., and the calcination time is 1-3 hours.
[0018] A third aspect of the present invention provides a sodium ion battery electrode sheet comprising the high voltage stable sodium oxide positive electrode material.
[0019] A fourth aspect of the present invention provides a method for preparing a sodium ion battery electrode sheet comprising the high voltage stable sodium oxide positive electrode material, the steps of which are as follows:
[0020] The high-voltage stable sodium oxide positive electrode material, conductive agent (Super P) and binder (PVDF) are evenly mixed in a mass ratio of 8:1:1, and an appropriate amount of NMP is added to make a slurry. The slurry is evenly coated on aluminum foil and placed in a vacuum oven at 80°C for drying to make a sodium ion battery electrode.
[0021] A fifth aspect of the present invention provides a sodium ion battery comprising the sodium ion battery pole piece.
[0022] The sixth aspect of the present invention provides a method for preparing a sodium ion battery including the sodium ion battery pole piece, wherein the sodium ion battery pole piece, the diaphragm, the electrolyte and the negative electrode pole piece are assembled in sequence in an argon atmosphere to finally prepare a sodium ion battery; wherein the diaphragm is glass fiber; the solute in the electrolyte is 1M NaPF6, the solvent is EMC (ethyl methyl carbonate) and PC (propylene carbonate), and the volume ratio of EMC to PC is 1:1. FEC (fluoroethylene carbonate) is an additive, accounting for 2% of the volume of the electrolyte; the negative electrode pole piece is a metal sodium sheet.
[0023] Advantages of the present invention:
[0024] 1. The present invention dopes copper and titanium elements into the transition metal layer, and then reconstructs it in situ on the surface through high-temperature secondary calcination to generate a composite structure of a surface rock salt phase and an internal O3 phase. The composite structure improves the interface stability of the material during high-voltage cycling.
[0025] 2. The present invention provides a type of high-voltage stable sodium oxide positive electrode material, which has the characteristics of good air stability, high specific capacity and long cycle life under high voltage. The raw materials used in the material are widely distributed in nature and have low cost. The material is synthesized by solid phase method, the process is simple and controllable, and can be prepared on a large scale, which is suitable for industrial application of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1The XRD patterns of high voltage stable sodium oxide positive electrode materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3;
[0027] Figure 2 This is a structural STEM image of the high voltage stable sodium oxide positive electrode material prepared in Example 1;
[0028] Figure 3 The first cycle charge-discharge curves of the high voltage stable sodium oxide positive electrode materials prepared in Example 1 and Comparative Examples 1 to 3 (active material loading: 2 to 4 mg cm -2 , current density: 20 mA g -1 );
[0029] Figure 4 The first cycle charge-discharge curve of the high voltage stable sodium oxide positive electrode material prepared in Example 2 (active material loading: 2-4 mg cm -2 , current density: 20 mA g -1 );
[0030] Figure 5 The first cycle charge-discharge curve of the high voltage stable sodium oxide positive electrode material prepared in Example 3 (active material loading: 2-4 mg cm -2 , current density: 20 mA g -1 );
[0031] Figure 6 The capacity cycle comparison diagram of the high voltage stable sodium oxide positive electrode materials prepared in Example 1 and Comparative Examples 1 to 3 (active material loading: 2 to 4 mg cm -2 , current density: 200 mA·g -1 );
[0032] Figure 7 The capacity cycle comparison diagram of the high voltage stable sodium oxide positive electrode materials prepared in Examples 1 to 3 (active material loading: 2 to 4 mg cm -2 , current density: 200 mA·g -1 ); DETAILED DESCRIPTION
[0033] In order to more clearly understand the present invention, the technical scheme of the present invention is further described below through specific examples. The purity of the sodium carbonate, nickel oxide, copper oxide, ferric oxide, manganese dioxide, titanium dioxide and organic solvent used in the examples is not less than 99%.
[0034] Example 1
[0035] A high voltage stable sodium oxide positive electrode material Na 0.9Ni 0.32 Cu 0.08 Fe 0.1 Mn 0.3 Ti 0.2 The preparation method of O2, the specific steps are as follows:
[0036] (1) Weigh 1.00 g of sodium carbonate, 0.48 g of nickel oxide, 0.13 g of copper oxide, 0.16 g of ferric oxide, 0.53 g of manganese dioxide and 0.32 g of titanium dioxide, mix them well and place them in a ball mill. Use anhydrous ethanol as a solvent for wet ball milling for 4 h to obtain a precursor slurry.
[0037] (2) drying the precursor slurry obtained in step (1) in a forced air drying oven at 80° C. for 30 min to obtain a precursor powder;
[0038] (3) The precursor powder obtained in step (2) is placed in an Al2O3 crucible, calcined for the first time at 900°C for 15 h in an air atmosphere, and then naturally cooled to obtain the initial material powder.
[0039] (4) The initial material powder obtained in step (3) is calcined for a second time at 1000°C for 1 h, and quenched and cooled to obtain a high voltage stable sodium oxide positive electrode material Na 0.9 Ni 0.32 Cu 0.08 Fe 0.1 Mn 0.3 Ti 0.2 O2, XRD spectrum as Figure 1 As shown. Figure 1 It can be seen that the material structure is an O3 phase structure. The structural STEM image of the high voltage stable sodium oxide positive electrode material prepared in Example 1 is as follows Figure 2 shown.
[0040] Example 2
[0041] A high voltage stable sodium oxide positive electrode material Na 0.9 Ni 0.3 Cu 0.1 Fe 0.1 Mn 0.3 Ti 0.2 The preparation method of O2, the specific steps are as follows:
[0042] (1) Weigh 1.00 g of sodium carbonate, 0.45 g of nickel oxide, 0.16 g of copper oxide, 0.16 g of ferric oxide, 0.53 g of manganese dioxide, and 0.32 g of titanium dioxide, mix them well, and place them in a ball mill. Use anhydrous ethanol as a solvent for wet ball milling for 4 h to obtain a precursor slurry.
[0043] (2) Dry the precursor slurry obtained in step (1) in a forced air drying oven at 80°C for 30 min to obtain a precursor powder.
[0044] (3) The precursor powder obtained in step (2) is placed in an Al2O3 crucible, calcined for the first time at 900°C for 15 h in an air atmosphere, and then naturally cooled to obtain the initial material powder.
[0045] (4) The initial material powder obtained in step (3) is calcined for a second time at 1000°C for 1 h, and quenched and cooled to obtain a high voltage stable sodium oxide positive electrode material Na 0.9 Ni 0.3 Cu 0.1 Fe 0.1 Mn 0.3 Ti 0.2 O2, XRD spectrum as Figure 1 As shown. Figure 1 It can be seen that the material structure is an O3 phase structure.
[0046] Example 3
[0047] A high voltage stable sodium oxide positive electrode material Na 0.9 Ni 0.3 Cu 0.1 Fe 0.1 Mn 0.2 Ti 0.3 The preparation method of O2, the specific steps are as follows:
[0048] (1) Weigh 1.00 g of sodium carbonate, 0.45 g of nickel oxide, 0.16 g of copper oxide, 0.16 g of ferric oxide, 0.35 g of manganese dioxide, and 0.45 g of titanium dioxide, mix them well, and place them in a ball mill. Use anhydrous ethanol as a solvent for wet ball milling for 4 h to obtain a precursor slurry.
[0049] (2) Dry the precursor slurry obtained in step (1) in a forced air drying oven at 80°C for 30 min to obtain a precursor powder.
[0050] (3) The precursor powder obtained in step (2) is placed in an Al2O3 crucible, calcined for the first time at 900°C for 15 h in an air atmosphere, and then naturally cooled to obtain the initial material powder.
[0051] (4) The initial material powder obtained in step (3) is calcined for a second time at 1000°C for 1 h, and quenched and cooled to obtain a high voltage stable sodium oxide positive electrode material Na 0.9 Ni 0.3 Cu 0.1 Fe 0.1 Mn 0.2 Ti 0.3O2, XRD spectrum as Figure 1 As shown. Figure 1 It can be seen that the material structure is an O3 phase structure.
[0052] Comparative Example 1
[0053] A high voltage stable sodium oxide positive electrode material Na 0.9 Ni 0.4 Fe 0.1 Mn 0.5 The preparation method of O2, the specific steps are as follows:
[0054] (1) Weigh 1.00 g of sodium carbonate, 0.59 g of nickel oxide, 0.87 g of ferric oxide, and 0.88 g of manganese dioxide, mix them well, and place them in a ball mill. Use anhydrous ethanol as a solvent and wet-mill them for 4 h to obtain a precursor slurry.
[0055] (2) Dry the precursor slurry obtained in step (1) in a forced air drying oven at 80°C for 30 min to obtain a precursor powder.
[0056] (3) The precursor powder obtained in step (2) was placed in an Al2O3 crucible, calcined for the first time at 900°C for 15 h in an air atmosphere, and then cooled naturally to obtain Na 0.9 Ni 0.4 Fe 0.1 Mn 0.5 O2. XRD Figure 1 As shown. Figure 1 It can be seen that the structure of the high voltage stable sodium oxide positive electrode material is an O3 phase structure.
[0057] Comparative Example 2
[0058] The difference from Comparative Example 1 is that step (4) is added, wherein the Na obtained in step (3) is 0.9 Ni 0.4 Fe 0.1 Mn 0.5 O2 was calcined at 1000℃ for 1 h, quenched and cooled, and XRD results were as follows: Figure 1 As shown. Figure 1 It can be seen that the structure of the high voltage stable sodium oxide positive electrode material is an O3 phase structure.
[0059] Comparative Example 3
[0060] The difference from Example 1 is that the secondary high-temperature calcination in step (4) is not performed. Figure 1 shown.
[0061] The electrochemical performance test results of the high voltage stable sodium oxide positive electrode materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Tables 1 and Figure 3~Figure 7 shown.
[0062] Test Method
[0063] Preparation of sodium ion battery electrodes: High voltage stable sodium oxide positive electrode material, conductive agent Super P and binder PVDF are mixed evenly in a mass ratio of 8:1:1, and an appropriate amount of NMP is added to make a slurry. The slurry is evenly coated on aluminum foil and placed in a vacuum oven at 80°C for drying to make sodium ion battery electrode sheets.
[0064] Preparation of sodium ion battery: The sodium ion battery electrode sheet, diaphragm, electrolyte and negative electrode sheet are assembled in sequence in an argon atmosphere to finally obtain a sodium ion battery; the diaphragm is glass fiber; the solute in the electrolyte is 1M NaPF6, the solvent is EMC and PC, and the volume ratio of EMC and PC is 1:1. FEC is an additive, accounting for 2% of the volume of the electrolyte; the negative electrode sheet is a metal sodium sheet.
[0065] Test conditions
[0066] The high voltage stable sodium oxide positive electrode materials prepared in the examples and comparative examples were prepared into sodium ion battery pole pieces and sodium ion batteries. The prepared sodium ion batteries were tested. The electrochemical performance test results are shown in Table 1. The test temperature was 25°C, the voltage range was 2-4.2 V, and the voltage at 20 mA·g -1 The first cycle charge and discharge curve (such as Figure 3~Figure 5 ). at 200 mA·g -1 The capacity retention rate after 100 and 200 cycles was obtained (e.g. Figure 6~Figure 7 ).
[0067] The capacity retention rate of Comparative Example 1 after 200 cycles is only 60.7%. In Comparative Example 2, without copper and titanium doping, after high-temperature secondary calcination, the capacity retention rate of 200 cycles is increased to 67.2%. Comparative Example 3, which is doped with copper and titanium but not subjected to high-temperature secondary calcination, has improved cycle stability compared to Comparative Examples 1 and 2, and the capacity retention rate after 200 cycles is 77.7%. After secondary calcination, the cycle stability of Examples 1 to 3 is further improved, and the capacity retention rate after 200 cycles is 92% to 93%.
[0068] Table 1 Electrochemical performance test results of examples and comparative examples
[0069] Example / Comparative Example <![CDATA[Initial cycle discharge specific capacity (mAh·g -1 ).]]> 100-cycle capacity retention rate (%) 200-cycle capacity retention rate (%) Example 1 146.1 97.0 92.9 Example 2 147.9 95.5 92.4 Example 3 140.2 95.1 92.0 Comparative Example 1 210.9 66.1 60.7 Comparative Example 2 191.4 74.6 67.2 Comparative Example 3 146.0 84.5 77.7
[0070] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept, which all belong to the protection scope of the present invention.
Claims
1. A type of high voltage stable sodium oxide positive electrode material, characterized by: The chemical formula is Na a Ni b Cu c Fe d Mn e Ti f O2, where 0.7≤a≤1, 0.2≤b≤0.45, 0≤c≤0.1, 0≤d≤0.2, 0.2≤e≤0.5, 0≤f≤0.3, b+ c + d + e + f = 1, the bulk phase of the material is an O3 phase structure, the surface is a rock salt phase structure, between the O3 phase structure and the rock salt phase structure is a spinel phase structure, and the thickness of the rock salt phase structure is 2-3 nm; The preparation method comprises the following steps: (1) Weighing and mixing the sodium source and each transition metal source in proportion, and grinding them by wet grinding to obtain a uniformly mixed precursor slurry; (2) placing the precursor slurry obtained in step (1) into a forced air drying oven for drying to obtain a precursor powder; (3) calcining the precursor powder obtained in step (2) for the first time at a temperature of 800-1000° C. for 10-15 hours, and slowly cooling to obtain an initial material powder; (4) The initial material powder obtained in step (3) is subjected to a second calcination at a temperature of 900-1200° C. for 1-3 hours, and quenched to obtain a high-voltage stable sodium oxide positive electrode material.
2. The high voltage stable sodium oxide positive electrode material according to claim 1, characterized in that: The sodium source in step (1) is one of sodium carbonate, sodium bicarbonate or sodium acetate; the transition metal source includes a nickel source, a copper source, an iron source, a manganese source, a titanium source, and is one of an oxide, a carbonate or an acetate.
3. A sodium ion battery pole piece comprising the high voltage stable sodium oxide positive electrode material according to claim 1.
4. A method for preparing a sodium ion battery pole piece according to claim 3, characterized in that: The high-voltage stable sodium oxide positive electrode material, the conductive agent Super P and the binder PVDF are evenly mixed in a mass ratio of 8:1:1, and an appropriate amount of NMP is added to make a slurry. The slurry is evenly coated on an aluminum foil and placed in a vacuum oven at 80°C for drying to make a sodium ion battery electrode.
5. A sodium ion battery comprising the sodium ion battery pole piece according to claim 3.
6. The method for preparing a sodium ion battery according to claim 5, characterized in that: The sodium ion battery pole piece, the separator, the electrolyte and the negative electrode piece are assembled in sequence in an argon atmosphere to finally produce a sodium ion battery.