A layered coating CCM for a hydrogen fuel cell and a preparation method thereof
By using layered coating CCM structure in hydrogen fuel cells, combining the gradient distribution of low-load and high-load Pt/C catalysts and the use of CNTs, the adsorption force of perfluorosulfonic acid ionomers to platinum catalysts is solved. , improves the electrochemical reaction efficiency and durability of hydrogen fuel cells, while reducing costs.
Patent Information
- Application Number
- CN202411116976.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The adsorption force between perfluorosulfonic acid ionomer and platinum catalyst in existing hydrogen fuel cells is strong, resulting in an increase in the transmission resistance of the reaction gas, a decrease in battery performance, and insufficient distribution of the porosity gradient of the catalytic layer, which affects the electrochemical reaction efficiency.
The layered CCM structure is adopted. The cathode side is composed of a bottom layer with a low load Pt/C, a high I/C ratio, an intermediate layer and an outer layer with a high load Pt/C and a low I/C ratio. The anode side is composed of a low The loading Pt/C and high loading Pt/C are composed of which improves conductivity and hydrophobicity through CNTs, and optimizes the catalyst distribution to improve proton conduction and reaction rate.
It improves the H proton conduction capacity and reaction rate, reduces the toxic effect of perfluorosulfonic acid groups on Pt, improves power generation efficiency and durability, and reduces costs.
Smart Images

Figure CN118645638B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a layered coating CCM of a hydrogen fuel cell and a preparation method thereof. Background Art
[0002] As fossil energy is becoming increasingly depleted, it is urgent to find alternative new energy sources. Hydrogen energy, as an efficient, clean, safe and sustainable secondary energy source, has attracted much attention in recent years. Hydrogen energy can penetrate into all aspects of traditional energy, including transportation, long-term energy storage, industrial fuel, portable equipment and other fields. Hydrogen fuel cells are considered to have broad development prospects due to their excellent performance in hydrogen energy utilization efficiency, power density, emissions and other aspects.
[0003] Proton exchange membrane fuel cells are power generation devices that convert the chemical energy in hydrogen directly into electrical energy through electrochemical reactions. They have the advantages of high energy conversion efficiency, zero emissions, and no noise. The membrane electrode is the core component of the fuel cell, and from the inside to the outside it consists of three parts: a proton exchange membrane, a catalyst layer, and a diffusion layer. The proton exchange membrane currently used is mainly perfluorosulfonic acid proton exchange membrane, and the catalyst layer is the site of the electrochemical reaction in the fuel cell. It is mainly prepared by mixing Pt catalyst with perfluorosulfonic acid ionomer and / or covalent organic framework material by a certain method and transferring it to the proton exchange membrane or diffusion layer. Among them, the surface of Pt nanoparticles plays a catalytic role in H 2 , O 2 The role of perfluorosulfonic acid ionomer is to transfer protons.
[0004] Perfluorosulfonic acid ionomers are composed of a hydrophobic carbon fluoride main chain and a hydrophilic side chain sulfonic acid end group, and have strong hydration, especially short side chain perfluorosulfonic acid ionomers have better water retention and wetting ability, and can better conduct protons. However, the adsorption force between the sulfonic acid groups in the perfluorosulfonic acid ionomer and the platinum in the platinum catalyst is strong. A large number of sulfonic acid groups cover the surface of platinum, forming a dense ionomer coating layer, which will increase the transmission resistance of the reaction gas at the catalytic active interface, and then lead to severe concentration polarization of the battery, and greatly reduce the battery performance.
[0005] The Chinese patent application publication number CN 106684395 A provides a manufacturing process for a cathode catalyst layer with gradient porosity for a fuel cell. In the overall manufacturing process of the catalyst layer, a completely consistent catalyst slurry is used. By controlling the spray volume of the catalyst slurry sprayed each time and the temperature of the proton exchange membrane surface, the surface temperature of the catalyst layer during the spraying process is effectively controlled, and then the volatilization rate of the total solvent in the slurry is controlled to control the porosity of the catalyst layer, and finally a gradient distribution of the porosity of the catalyst layer is achieved. However, due to the consistent composition of the slurry, even if the coating is carried out in steps, the I / C ratio and the precious metal loading in the final coating remain unchanged, and there will be no gradient changes.
[0006] Therefore, a new cathode catalyst layer, membrane electrode and anode catalyst layer were developed to make them highly active and low-cost. At the same time, CCM has higher proton transfer capacity, gas diffusion capacity and strong hydrophobicity. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a layered coated CCM for a hydrogen fuel cell and a preparation method thereof. The cathode side of the CCM of the present invention is composed of three catalytic layers, namely, a first bottom layer, an intermediate layer and a first outer layer, and the anode side is composed of two catalytic layers, namely, a second bottom layer and a second outer layer. The first bottom layer and the second bottom layer are coated with a low Pt / C loading and a high I / C ratio to improve H proton conduction. The intermediate coating is a transition coating, and CNTs with better hydrophobicity and conductivity are added as a matrix to improve the conductivity and hydrophobicity of the catalyst. The first outer layer and the second outer layer are coated with a high Pt / C loading and a low I / C ratio to increase active sites and improve the reaction rate.
[0008] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is:
[0009] In the first aspect, an embodiment of the present invention provides a layered coated CCM for a hydrogen fuel cell, wherein the cathode side of the CCM comprises a first bottom layer, an intermediate layer, and a first outer layer; the coating amount of the catalyst in the first bottom layer is 0.01-0.1 mg / cm 2 The middle layer is a transition coating, which is doped into the CNTs matrix. The coating amount of the catalyst is 0.05-0.1 mg / cm 2 The coating amount of the catalyst in the first outer layer is 0.1-0.15 mg / cm 2 ; The mass loading of precious metals of the catalyst in the first bottom layer, the middle layer and the first outer layer increases successively, and the I / C ratio decreases successively;
[0010] The precious metal mass loading of the catalyst in the first bottom layer is 2-10%, and the I / C ratio is 1.2-1.5; the precious metal mass loading of the catalyst in the middle layer is 10-20%, and the I / C ratio is 0.5-0.8; the precious metal mass loading of the catalyst in the first outer layer is 50-70%, and the I / C ratio is 0.1-0.3;
[0011] The anode side of the CCM includes a second bottom layer and a second outer layer, and the coating amount of the catalyst in the second bottom layer is 0.01-0.05 mg / cm 2 The coating amount of the catalyst in the second outer layer is 0.02-0.1 mg / cm 2 ; The precious metal mass loading of the catalyst in the second bottom layer is less than the precious metal mass loading of the catalyst in the second outer layer, and the I / C ratio in the second bottom layer is greater than the I / C ratio in the second outer layer;
[0012] The precious metal mass loading of the catalyst in the second bottom layer is 2-10%, and the I / C ratio is 1.2-1.5; the precious metal mass loading of the catalyst in the second outer layer is 50-70%, and the I / C ratio is 0.1-0.3;
[0013] In the I / C ratio, I represents the mass of solids in the Nafion solution, and C represents the mass of the carbon support in the platinum-containing catalyst;
[0014] The catalyst is a Pt / C catalyst.
[0015] In a second aspect, an embodiment of the present invention provides a method for preparing a layered coated CCM for a hydrogen fuel cell, comprising the following steps:
[0016] Cathode side CCM bottom layer preparation
[0017] (1) Weighing of materials: First weigh a platinum-containing catalyst with a platinum mass loading of 2-10%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 1.2-1.5, wherein the solid content is controlled at 2.5-10%;
[0018] (2) Preparation of oil film: The materials weighed in step (1) are mixed with a platinum-containing catalyst and H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the platinum-containing catalyst needs to be fully dispersed after adding water, then the Nafion solution is added, and finally the ethanol is added;
[0019] (3) Oil film treatment: The slurry obtained in step (2) is treated by ultrasonic or ball milling. 90 Controlled below 1μm;
[0020] (4) Coating: The oil film obtained in step (3) is coated on the proton exchange membrane. The coating amount of the catalyst is 0.01-0.1 mg / cm 2 ;
[0021] Preparation of CCM transition layer on cathode side
[0022] (5) Weighing of materials: First weigh CNTs and a platinum-containing catalyst with a platinum mass loading of 10-20%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 0.5-0.8, wherein the solid content is controlled at 2.5-10%;
[0023] (6) Preparation of oil film: The materials weighed in step (5) were mixed according to the conditions of CNTs, platinum-containing catalyst, and H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the platinum-containing catalyst needs to be fully dispersed after adding water, then the Nafion solution is added, and finally the ethanol is added;
[0024] (7) Oil film treatment: D of the slurry in step (6) is treated by ultrasonic or ball milling. 90 Controlled below 1μm;
[0025] (8) Coating: The oil film obtained in step (7) is coated on the proton exchange membrane in step (4), and the coating amount of the catalyst is 0.05-0.1 mg / cm 2 ;
[0026] Preparation of CCM outer layer on cathode side
[0027] (9) Weighing of materials: First weigh a platinum-containing catalyst with a platinum mass loading of 50-70%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 0.1-0.3, wherein the solid content is controlled at 2.5-10%;
[0028] (10) Preparation of oil film: The materials weighed in step (9) are mixed with a platinum catalyst, H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the platinum-containing catalyst needs to be fully dispersed after adding water, then the Nafion solution is added, and finally the ethanol is added;
[0029] (11) Oil film treatment: D of the slurry in step (10) is treated by ultrasonic or ball milling. 90 Controlled below 1μm;
[0030] (12) Coating: The oil film obtained in step (11) is coated on the proton exchange membrane in step (8), and the coating amount of the catalyst is 0.1-0.15 mg / cm2 ;
[0031] Anode side CCM bottom layer preparation
[0032] (13) Weighing of materials: First weigh a platinum-containing catalyst with a platinum mass loading of 2-10%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 1.2-1.5, wherein the solid content is controlled at 2.5-10%;
[0033] (14) Preparation of oil film: The materials weighed in step (13) are mixed with a platinum catalyst, H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the platinum-containing catalyst needs to be fully dispersed after adding water, then the Nafion solution is added, and finally the ethanol is added;
[0034] (15) Oil film treatment: D of the slurry in step (14) is treated by ultrasonic or ball milling. 90 Controlled below 1μm;
[0035] (16) Coating: The oil film obtained in step (15) is coated on the other surface of the proton exchange membrane in step (12), and the coating amount of the catalyst is 0.01-0.05 mg / cm 2 ;
[0036] Anode side CCM outer layer preparation
[0037] (17) Weighing of materials: First weigh a platinum-containing catalyst with a platinum mass loading of 50-70%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 0.1-0.3, wherein the solid content is controlled at 2.5-10%;
[0038] (18) Preparation of oil film: The materials weighed in step (17) are mixed with a platinum catalyst, H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the platinum-containing catalyst needs to be fully dispersed after adding water, then the Nafion solution is added, and finally the ethanol is added;
[0039] (19) Oil film treatment: D of the slurry in step (18) is treated by ultrasonic or ball milling. 90 Controlled below 1μm;
[0040] (20) Coating: The oil film obtained in step (19) is coated on the proton exchange membrane in step (16), and the coating amount of the catalyst is 0.02-0.1 mg / cm 2 , a layered coated CCM was obtained.
[0041] Furthermore, the solid content of the Nafion solution is 10-30%.
[0042] Furthermore, the proton exchange membrane in step (4) is a Gore or DuPont proton exchange membrane with a thickness of 8-15 μm.
[0043] Furthermore, the platinum-containing catalyst is a Pt / C catalyst or a PtCo / C catalyst.
[0044] Furthermore, the amount of CNTs added in step (5) is 5-20% of the weight of the platinum-containing catalyst.
[0045] The technical solution provided by the embodiment of the present invention has the following beneficial effects:
[0046] (1) The CCM of the present invention improves the existing coating process by adopting layered coating, with the bottom layer adopting low-loaded Pt / C and high I / C ratio, which effectively improves the conduction of H protons and reduces the damage of perfluorosulfonic acid groups to Pt groups, where I represents the solid mass in the Nafion solution and C represents the mass of the carbon carrier in the platinum-containing catalyst. The outer layer of the CCM adopts high-loaded Pt / C and low I / C ratio, which, on the one hand, increases active sites, improves reaction rate, and improves power generation efficiency; on the other hand, the lower I / C ratio can effectively avoid the poisoning effect of perfluorosulfonic acid groups on Pt, which is conducive to the improvement of performance and durability.
[0047] (2) The incorporation of CNTs (carbon nanotubes) into the Pt / C catalyst improves the conductivity and hydrophobicity of CCM and improves the durability of CCM.
[0048] (3) Since only the outer layer uses a high-load Pt, and the bottom layer and transition layer use a lower-load Pt, the overall cost is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 It is a polarization curve diagram of the single cell made of CCM in Examples 1-3 of the present invention and Comparative Example 1.
[0050] Figure 2 It is a polarization curve diagram of the single cell made of CCM in Example 3 of the present invention and Comparative Example 2.
[0051] Figure 3 It is a polarization curve diagram of a single cell made of CCM in Comparative Examples 3 and 4 of the present invention. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0053] The material information in the embodiments and comparative examples is as follows:
[0054] Nafion solutions are all DuPont solutions, product model D2020.
[0055] CNTs were purchased from Jiangsu Tiannai Technology Co., Ltd., material name FT7010, product batch number ZP211122.
[0056] The diffusion layer is Toray carbon paper, model number is TGL-R-055.
[0057] Example 1
[0058] A method for preparing a layered coated CCM for a hydrogen fuel cell comprises the following steps:
[0059] Cathode side CCM bottom layer preparation
[0060] (1) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 2%, and weigh deionized water and ethanol at a volume ratio of 5:5, respectively. The amount of Nafion solution (mass concentration of 25%) added is weighed at an I / C ratio of 1.5, wherein the solid content is controlled at 10%;
[0061] (2) Preparation of oil film: The materials weighed in step (1) are mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 25%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 25% is added, and finally the ethanol is added;
[0062] (3) Oil film treatment: The oil film obtained in step (2) is treated by ultrasonic, ball milling and other processes to obtain slurry D 90 Controlled below 1μm;
[0063] (4) Coating: The oil film obtained in step (3) is coated on a Gore proton exchange membrane with a thickness of 8 μm and a size of 5*5 cm by spraying or slit coating. The coating amount of the catalyst is 0.05 mg / cm 2 , dry at 80°C until the weight does not change;
[0064] Preparation of CCM transition layer on cathode side
[0065] (5) Weighing of materials: CNTs and Pt / C catalyst with a platinum mass loading of 20% were weighed at a weight ratio of 0.05:0.95, deionized water and ethanol were weighed at a volume ratio of 4:6, and the amount of Nafion solution with a mass concentration of 25% was weighed at an I / C ratio of 0.8, wherein the solid content was controlled in the range of 5%;
[0066] (6) Preparation of oil film: The materials weighed in step (5) were mixed according to the ratio of CNTs, Pt / C, H 2 O, Nafion solution with a mass concentration of 25%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 25% is added, and finally the ethanol is added;
[0067] (7) Oil film treatment: The oil film obtained in step (6) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0068] (8) Coating: The oil film obtained in step (7) is coated on the proton exchange membrane of step (4) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.1 mg / cm 2 , dry at 80°C until the weight does not change;
[0069] Preparation of CCM outer layer on cathode side
[0070] (9) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 60%, weigh deionized water and ethanol at a volume ratio of 3:7, and weigh a 25% Nafion solution at an I / C ratio of 0.2, wherein the solid content is controlled at 5%;
[0071] (10) Preparation of oil film: The materials weighed in step (9) were mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 25%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 25% is added, and finally the ethanol is added;
[0072] (11) Oil film treatment: The oil film obtained in step (10) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0073] (12) Coating: The oil film obtained in step (11) is coated on the proton exchange membrane of step (8) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.15 mg / cm 2 , dry at 80°C until the weight does not change;
[0074] Anode side CCM bottom layer preparation
[0075] (13) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 2%, weigh deionized water and ethanol at a volume ratio of 5:5, and weigh a 25% Nafion solution at an I / C ratio of 1.5, wherein the solid content is controlled at 5%;
[0076] (14) Preparation of oil film: The materials weighed in step (13) are mixed according to the ratio of Pt / C and H 2 O, Nafion solution with a mass concentration of 25%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 25% is added, and finally the ethanol is added;
[0077] (15) Oil film treatment: The oil film obtained in step (14) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0078] (16) Coating: The oil film obtained in step (15) is coated on the other surface of the proton exchange membrane in step (12) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.05 mg / cm 2 , dry at 80°C until the weight does not change;
[0079] Anode side CCM outer layer preparation
[0080] (17) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 60%, weigh deionized water and ethanol at a volume ratio of 3:7, and weigh a 25% Nafion solution at an I / C ratio of 0.2, wherein the solid content is controlled at 5%;
[0081] (18) Preparation of oil film: The materials weighed in step (17) were mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 25%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 25% is added, and finally the ethanol is added;
[0082] (19) Oil film treatment: The oil film obtained in step (18) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0083] (20) Coating: The oil film obtained in step (19) is coated on the proton exchange membrane of step (16) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.05 mg / cm 2 , and dried at 80°C until the weight does not change to obtain a layered coated CCM.
[0084] Diffusion layers were cut into square pieces with a length and width of 5 cm*5 cm, and the cut diffusion layers were placed on both sides of the layered coated CCM to obtain membrane electrodes.
[0085] Example 2
[0086] A method for preparing a layered coated CCM for a hydrogen fuel cell comprises the following steps:
[0087] Cathode side CCM bottom layer preparation
[0088] (1) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 5%, weigh deionized water and ethanol at a volume ratio of 4:6, and weigh a 20% Nafion solution at an I / C ratio of 1.3, wherein the solid content is controlled at 10%;
[0089] (2) Preparation of oil film: The materials weighed in step (1) are mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 20%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 20% is added, and finally the ethanol is added;
[0090] (3) Oil film treatment: The oil film obtained in step (2) is treated by ultrasonic, ball milling and other processes to obtain slurry D 90 Controlled below 1μm;
[0091] (4) Coating: The oil film obtained in step (3) is coated on a Gore proton exchange membrane with a thickness of 8 μm and a size of 5*5 cm by spraying or slit coating. The coating amount of the catalyst is 0.05 mg / cm 2 , dry at 80°C until the weight does not change;
[0092] Preparation of CCM transition layer on cathode side
[0093] (5) Weighing of materials: CNTs and Pt / C catalyst with a platinum mass loading of 10% were weighed at a weight ratio of 0.1:0.9, deionized water and ethanol were weighed at a volume ratio of 4:6, and the amount of Nafion solution with a mass concentration of 20% was weighed at an I / C ratio of 0.6, wherein the solid content was controlled in the range of 10%;
[0094] (6) Preparation of oil film: The materials weighed in step (5) were mixed according to the ratio of CNTs, Pt / C, H 2 O, Nafion solution with a mass concentration of 20%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 20% is added, and finally the ethanol is added;
[0095] (7) Oil film treatment: The oil film obtained in step (6) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0096] (8) Coating: The oil film obtained in step (7) is coated on the proton exchange membrane of step (4) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.1 mg / cm 2 ;
[0097] Preparation of CCM outer layer on cathode side
[0098] (9) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 70%, weigh deionized water and ethanol at a volume ratio of 2:8, and weigh a 20% Nafion solution at an I / C ratio of 0.15, wherein the solid content is controlled at 10%;
[0099] (10) Preparation of oil film: The materials weighed in step (9) were mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 20%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 20% is added, and finally the ethanol is added;
[0100] (11) Oil film treatment: The oil film obtained in step (10) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0101] (12) Coating: The oil film obtained in step (11) is coated on the proton exchange membrane of step (8) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.15 mg / cm 2 , dry at 80°C until the weight does not change;
[0102] Anode side CCM bottom layer preparation
[0103] (13) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 10%, weigh deionized water and ethanol at a volume ratio of 4:6, and weigh a 20% Nafion solution at an I / C ratio of 1.2, wherein the solid content is controlled in the range of 10%;
[0104] (14) Preparation of oil film: The materials weighed in step (13) are mixed according to the ratio of Pt / C and H 2 O, Nafion solution with a mass concentration of 20%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 20% is added, and finally the ethanol is added;
[0105] (15) Oil film treatment: The oil film obtained in step (14) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0106] (16) Coating: The oil film obtained in step (15) is coated on the other surface of the proton exchange membrane in step (12) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.05 mg / cm 2 , dry at 80°C until the weight does not change;
[0107] Anode side CCM outer layer preparation
[0108] (17) Material weighing: First weigh a Pt / C catalyst with a platinum mass loading of 70%, weigh deionized water and ethanol at a volume ratio of 2:8, and weigh a 20% Nafion solution at an I / C ratio of 0.15, wherein the solid content is controlled at 10%;
[0109] (18) Preparation of oil film: The materials weighed in step (17) were mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 20%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 20% is added, and finally the ethanol is added;
[0110] (19) Oil film treatment: The oil film obtained in step (18) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0111] (20) Coating: The oil film obtained in step (19) is coated on the proton exchange membrane of step (16) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.05 mg / cm 2 , and dried at 80°C until the weight does not change to obtain a layered coated CCM.
[0112] Diffusion layers were cut into square pieces with a length and width of 5 cm*5 cm, and the cut diffusion layers were placed on both sides of the CCM to obtain membrane electrodes.
[0113] Example 3
[0114] A method for preparing a layered coated CCM for a hydrogen fuel cell comprises the following steps:
[0115] Cathode side CCM bottom layer preparation
[0116] (1) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 10%, weigh deionized water and ethanol at a volume ratio of 3:7, and weigh a Nafion solution with a mass concentration of 15% at an I / C ratio of 1.3, wherein the solid content is controlled at 3%;
[0117] (2) Preparation of oil film: The materials weighed in step (1) are mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 15%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 15% is added, and finally the ethanol is added;
[0118] (3) Oil film treatment: The oil film obtained in step (2) is treated by ultrasonic, ball milling and other processes to obtain slurry D 90 Controlled below 1μm;
[0119] (4) Coating: The oil film obtained in step (3) is coated on a Gore proton exchange membrane with a thickness of 8 μm and a size of 5*5 cm by spraying or slit coating. The coating amount of the catalyst is 0.05 mg / cm 2 , dry at 80°C until the weight does not change;
[0120] Preparation of CCM transition layer on cathode side
[0121] (5) Weighing of materials: CNTs and Pt / C catalyst with a platinum mass loading of 15% were weighed at a weight ratio of 0.2:0.8, deionized water and ethanol were weighed at a volume ratio of 4:6, and the amount of Nafion solution with a mass concentration of 20% was weighed at an I / C ratio of 0.5, wherein the solid content was controlled in the range of 3%;
[0122] (6) Preparation of oil film: The materials weighed in step (5) were mixed according to the ratio of CNTs, Pt / C, H 2 O, Nafion solution with a mass concentration of 15%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 15% is added, and finally the ethanol is added;
[0123] (7) Oil film treatment: The oil film obtained in step (6) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0124] (8) Coating: The oil film obtained in step (7) is coated on the proton exchange membrane of step (4) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.1 mg / cm 2 , dry at 80°C until the weight does not change;
[0125] Preparation of CCM outer layer on cathode side
[0126] (9) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 55%, weigh deionized water and ethanol at a volume ratio of 2:8, and weigh a Nafion solution with a mass concentration of 15% at an I / C ratio of 0.1, wherein the solid content is controlled at 3%;
[0127] (10) Preparation of oil film: The materials weighed in step (9) were mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 15%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 15% is added, and finally the ethanol is added;
[0128] (11) Oil film treatment: The oil film obtained in step (10) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0129] (12) Coating: The oil film obtained in step (11) is coated on the proton exchange membrane of step (8) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.15 mg / cm 2 , dry at 80°C until the weight does not change;
[0130] Anode side CCM bottom layer preparation
[0131] (13) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 10%, weigh deionized water and ethanol at a volume ratio of 3:7, and weigh a Nafion solution with a mass concentration of 15% at an I / C ratio of 1.3, wherein the solid content is controlled at 10%;
[0132] (14) Preparation of oil film: The materials in step (13) are mixed according to Pt / C, H 2 O, Nafion solution with a mass concentration of 15%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 15% is added, and finally the ethanol is added;
[0133] (15) Oil film treatment: The oil film obtained in step (14) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0134] (16) Coating: The oil film obtained in step (15) is coated on the other surface of the proton exchange membrane in step (12) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.05 mg / cm 2 , dry at 80°C until the weight does not change;
[0135] Anode side CCM outer layer preparation
[0136] (17) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 55%, weigh deionized water and ethanol at a volume ratio of 2:8, and weigh a Nafion solution with a mass concentration of 15% at an I / C ratio of 0.1, wherein the solid content is controlled at 3%;
[0137] (18) Preparation of oil film: The materials weighed in step (17) were mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 15%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 15% is added, and finally the ethanol is added;
[0138] (19) Oil film treatment: The oil film obtained in step (18) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0139] (20) Coating: The oil film obtained in step (19) is coated on the proton exchange membrane of step (16) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.05 mg / cm 2 , and dried at 80°C until the weight does not change to obtain a layered coated CCM.
[0140] Diffusion layers were cut into square pieces with a length and width of 5 cm*5 cm, and the cut diffusion layers were placed on both sides of the CCM to obtain membrane electrodes.
[0141] Comparative Example 1
[0142] A method for preparing a CCM membrane electrode for a hydrogen fuel cell comprises the following steps:
[0143] (1) Weighing of cathode materials: First weigh a Pt / C catalyst with a platinum mass loading of 60%, weigh deionized water and ethanol at a volume ratio of 3:7, and weigh a 15% Nafion solution at an I / C ratio of 0.9, wherein the solid content is controlled at 10%;
[0144] (2) Preparation of oil film: Mix the above materials according to Pt / C, H 2 O, Nafion solution with a mass concentration of 15%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 15% is added, and finally the ethanol is added;
[0145] (3) Oil film treatment: The oil film is treated by ultrasonic, ball milling and other processes to remove the slurry D 90 Controlled below 1μm;
[0146] (4) Cathode coating: The above oil film is coated on a Gore proton exchange membrane with a thickness of 8 μm and a size of 5*5 cm by spraying or slit coating. The coating amount of the catalyst is 0.3 mg / cm 2 , dry at 80°C until the weight does not change;
[0147] (5) Weighing of anode materials: First weigh a Pt / C catalyst with a platinum mass loading of 40%, weigh deionized water and ethanol at a volume ratio of 4:6, and weigh a 15% Nafion solution at an I / C ratio of 0.9, wherein the solid content is controlled at 10%;
[0148] (6) Preparation of oil film: Mix the above materials according to Pt / C, H 2 O, Nafion solution with a mass concentration of 15%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 15% is added, and finally the ethanol is added;
[0149] (7) Oil film treatment: The oil film is treated by ultrasonic, ball milling and other processes to remove the slurry D 90 Controlled below 1μm;
[0150] (8) Coating: The above-mentioned oil film is coated on the other surface of the proton exchange membrane in step (4) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.1 mg / cm 2 , dry at 80°C until the weight does not change;
[0151] (9) Cut the diffusion layers into square pieces with a length and width of 5 cm*5 cm respectively, and place the cut diffusion layers on both sides of the CCM to obtain membrane electrodes.
[0152] Comparative Example 2
[0153] A method for preparing a layered coated CCM for a hydrogen fuel cell is different from Example 3 in that CNTs are not added when preparing the CCM transition layer on the cathode side, and the other conditions are exactly the same as Example 3.
[0154] In order to further verify the experimental effect that the precious metal loading increases and the I / C ratio decreases from the inside to the outside of the CCM of the present invention, comparative examples 3 and 4 are provided.
[0155] Comparative Example 3
[0156] A method for preparing a layered coated CCM for a hydrogen fuel cell comprises the following steps:
[0157] Cathode side CCM bottom layer preparation
[0158] (1) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 60%, and weigh deionized water and ethanol at a volume ratio of 5:5 respectively. The amount of Nafion solution (mass concentration of 25%) added is weighed at an I / C ratio of 0.3, wherein the solid content is controlled at 10%;
[0159] (2) Preparation of oil film: The materials weighed in step (1) are mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 25%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 25% is added, and finally the ethanol is added;
[0160] (3) Oil film treatment: The oil film obtained in step (2) is treated by ultrasonic, ball milling and other processes to obtain slurry D 90 Controlled below 1μm;
[0161] (4) Coating: The oil film obtained in step (3) is coated on a Gore proton exchange membrane with a thickness of 8 μm and a size of 5*5 cm by spraying or slit coating. The coating amount of the catalyst is 0.1 mg / cm 2 , dry at 80°C until the weight does not change;
[0162] Preparation of CCM outer layer on cathode side
[0163] (5) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 40%, weigh deionized water and ethanol at a volume ratio of 3:7, and weigh a Nafion solution with a mass concentration of 25% at an I / C ratio of 1.0, wherein the solid content is controlled at 5%;
[0164] (6) Preparation of oil film: The materials weighed in step (5) are mixed according to Pt / C, H2 O, Nafion solution with a mass concentration of 25%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 25% is added, and finally the ethanol is added;
[0165] (7) Oil film treatment: The oil film obtained in step (6) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0166] (8) Coating: The oil film obtained in step (7) is coated on the proton exchange membrane of step (4) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.3 mg / cm 2 , dry at 80°C until the weight does not change;
[0167] Anode side preparation
[0168] (9) Weighing of materials: First weigh a Pt / C catalyst with a platinum mass loading of 60%, weigh deionized water and ethanol at a volume ratio of 5:5, and weigh a 25% Nafion solution at an I / C ratio of 0.3, wherein the solid content is controlled at 5%;
[0169] (10) Preparation of oil film: The materials weighed in step (9) were mixed according to the ratio of Pt / C, H 2 O, Nafion solution with a mass concentration of 25%, and ethanol are added to the stirred beaker in this order, wherein the Pt / C needs to be fully dispersed after adding water, then the Nafion solution with a mass concentration of 25% is added, and finally the ethanol is added;
[0170] (11) Oil film treatment: The oil film obtained in step (10) is treated by ultrasonic, ball milling or other processes to obtain slurry D 90 Controlled below 1μm;
[0171] (12) Coating: The oil film obtained in step (11) is coated on the other surface of the proton exchange membrane in step (8) by spraying or slit coating, with a size of 5*5 cm and a catalyst coating amount of 0.1 mg / cm 2 , and dried at 80°C until the weight does not change to obtain a CCM with layered coating on the cathode side.
[0172] Diffusion layers were cut into square pieces with a length and width of 5 cm*5 cm, and the cut diffusion layers were placed on both sides of the layered coated CCM to obtain membrane electrodes.
[0173] Comparative Example 4
[0174] A method for preparing a layered coated CCM for a hydrogen fuel cell, wherein the composition and preparation method of the anode side in Comparative Examples 3 and 4 are the same, and the difference in the cathode side composition is shown in Table 1, the preparation and coating of the cathode side bottom layer slurry in Comparative Example 4 are the same as the cathode side outer layer in Comparative Example 3, and the preparation and coating of the cathode side outer layer slurry in Comparative Example 4 are the same as the cathode side bottom layer in Comparative Example 3.
[0175] Table 1 Composition of the anode side and cathode side in Comparative Examples 3 and 4
[0176]
[0177] The CCMs prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to single cell tests. The test cell temperature was 80°C, the dew point temperature of the cathode and anode was 65°C, air was introduced into the cathode side, hydrogen was introduced into the anode side, the back pressure of the cathode and anode was 150 kPa, and the H 2 / Air stoichiometric ratio = 1.5:2.5.
[0178] Endurance test: Set the voltage to 0.6-0.95V square wave cycle, number of cycles: 30,000, to examine the durability performance of CCM.
[0179] Figure 1 The test results show that Examples 1-3 exhibit high membrane electrode activity, 1A / cm 2 The operating voltage is greater than 0.75V, 2A / cm 2 The operating voltage is greater than 0.66 V. Example 1 After 30,000 potential scans, the membrane electrode activity did not show a significant decrease, 1 A / cm 2 The operating voltage is greater than 0.73V, 2A / cm 2 The lower operating voltage is greater than 0.63V.
[0180] Figure 2 The test results show that the membrane electrode activity obtained in Comparative Example 2 without CNTs is lower than that of the membrane electrode doped with CNTs in Example 3.
[0181] Figure 3 The test results show that compared with comparative example 3, comparative example 4 exhibits higher membrane electrode activity, which indicates that the cathode configuration of the present invention, in which the precious metal content increases from the inside to the outside and the I / C ratio decreases, is beneficial to the improvement of membrane electrode performance.
[0182] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A layered coated CCM for a hydrogen fuel cell, It is characterized in that The cathode side of the CCM includes a first bottom layer, an intermediate layer and a first outer layer; the coating amount of the catalyst in the first bottom layer is 0.01-0.1 mg / cm 2 The middle layer is a transition coating, which is doped into the CNTs matrix. The coating amount of the catalyst is 0.05-0.1 mg / cm 2 The coating amount of the catalyst in the first outer layer is 0.1-0.15 mg / cm 2 ; The mass loading of precious metals of the catalyst in the first bottom layer, the middle layer and the first outer layer increases successively, and the I / C ratio decreases successively; The precious metal mass loading of the catalyst in the first bottom layer is 2-10%, and the I / C ratio is 1.2-1.5; the precious metal mass loading of the catalyst in the middle layer is 10-20%, and the I / C ratio is 0.5-0.8; the precious metal mass loading of the catalyst in the first outer layer is 50-70%, and the I / C ratio is 0.1-0.3; The anode side of the CCM includes a second bottom layer and a second outer layer, and the coating amount of the catalyst in the second bottom layer is 0.01-0.05 mg / cm 2 The coating amount of the catalyst in the second outer layer is 0.02-0.1 mg / cm 2 ; The precious metal mass loading of the catalyst in the second bottom layer is less than the precious metal mass loading of the catalyst in the second outer layer, and the I / C ratio in the second bottom layer is greater than the I / C ratio in the second outer layer; The precious metal mass loading of the catalyst in the second bottom layer is 2-10%, and the I / C ratio is 1.2-1.5; the precious metal mass loading of the catalyst in the second outer layer is 50-70%, and the I / C ratio is 0.1-0.3; The catalyst is a Pt / C catalyst; in the I / C ratio, I represents the solid mass in the Nafion solution when preparing the cathode side of the CCM and the anode side of the CCM, and C represents the mass of the carbon carrier in the Pt / C catalyst.
2. A method for preparing a layered coated CCM for a hydrogen fuel cell, It is characterized in that The following steps are involved: Preparation of CCM cathode bottom layer (1) Weighing of materials: First weigh a platinum-containing catalyst with a platinum mass loading of 2-10%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 1.2-1.5, wherein the solid content is controlled at 2.5-10%; (2) Preparation of oil film: The materials weighed in step (1) are mixed with a platinum-containing catalyst and H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the Nafion solution is added after the platinum-containing catalyst is fully dispersed in water, and finally ethanol is added; (3) Oil film treatment: The slurry obtained in step (2) is treated by ultrasonic or ball milling. 90 Controlled below 1μm; (4) Coating: The oil film obtained in step (3) is coated on the proton exchange membrane. The coating amount of the catalyst is 0.01-0.1 mg / cm 2 ; Preparation of transition layer on cathode side of CCM (5) Weighing of materials: First weigh CNTs and a platinum-containing catalyst with a platinum mass loading of 10-20%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 0.5-0.8, wherein the solid content is controlled at 2.5-10%; (6) Preparation of oil film: The materials weighed in step (5) were mixed according to the conditions of CNTs, platinum-containing catalyst, and H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the Nafion solution is added after the platinum-containing catalyst is fully dispersed in water, and finally ethanol is added; (7) Oil film treatment: D of the slurry in step (6) is treated by ultrasonic or ball milling. 90 Controlled below 1μm; (8) Coating: The oil film obtained in step (7) is coated on the proton exchange membrane in step (4), and the coating amount of the catalyst is 0.05-0.1 mg / cm 2 ; Preparation of the outer layer of the cathode side of CCM (9) Weighing of materials: First weigh a platinum-containing catalyst with a platinum mass loading of 50-70%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 0.1-0.3, wherein the solid content is controlled at 2.5-10%; (10) Preparation of oil film: The materials weighed in step (9) are mixed with a platinum-containing catalyst and H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the Nafion solution is added after the platinum-containing catalyst is fully dispersed in water, and finally ethanol is added; (11) Oil film treatment: D of the slurry in step (10) is treated by ultrasonic or ball milling. 90 Controlled below 1μm; (12) Coating: The oil film obtained in step (11) is coated on the proton exchange membrane in step (8), and the coating amount of the catalyst is 0.1-0.15 mg / cm 2 ; Preparation of CCM anode side bottom layer (13) Weighing of materials: First weigh a platinum-containing catalyst with a platinum mass loading of 2-10%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 1.2-1.5, wherein the solid content is controlled at 2.5-10%; (14) Preparation of oil film: The materials weighed in step (13) are mixed with a platinum catalyst, H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the Nafion solution is added after the platinum-containing catalyst is fully dispersed in water, and finally ethanol is added; (15) Oil film treatment: D of the slurry in step (14) is treated by ultrasonic or ball milling. 90 Controlled below 1μm; (16) Coating: The oil film obtained in step (15) is coated on the other surface of the proton exchange membrane in step (12), and the coating amount of the catalyst is 0.01-0.05 mg / cm 2 ; Preparation of the outer layer of the anode side of CCM (17) Weighing of materials: First weigh a platinum-containing catalyst with a platinum mass loading of 50-70%, weigh deionized water and ethanol at a volume ratio of 2-5:5-8 respectively, and weigh the amount of Nafion solution added at an I / C ratio of 0.1-0.3, wherein the solid content is controlled at 2.5-10%; (18) Preparation of oil film: The materials weighed in step (17) are mixed with a platinum catalyst, H 2 O, Nafion solution, and ethanol are added to a stirred beaker in this order, wherein the Nafion solution is added after the platinum-containing catalyst is fully dispersed in water, and finally ethanol is added; (19) Oil film treatment: D of the slurry in step (18) is treated by ultrasonic or ball milling. 90 Controlled below 1μm; (20) Coating: The oil film obtained in step (19) is coated on the proton exchange membrane in step (16), and the coating amount of the catalyst is 0.02-0.1 mg / cm 2 , a layered coated CCM is obtained; In the I / C ratio, I represents the solid mass in the Nafion solution when preparing each layer of the cathode side of the CCM and the anode side of the CCM, and C represents the mass of the carbon support in the platinum-containing catalyst.
3. The method for preparing the layered coated CCM of the hydrogen fuel cell according to claim 2, It is characterized in that The solid content of the Nafion solution is 10-30%.
4. The method for preparing a layered coated CCM for a hydrogen fuel cell according to claim 2, It is characterized in that The platinum-containing catalyst is a Pt / C catalyst or a PtCo / C catalyst.
5. The method for preparing the layered coated CCM of the hydrogen fuel cell according to claim 2, It is characterized in that The amount of CNTs added in step (5) is 5-20% of the weight of the platinum-containing catalyst.